A bamboo-based hard carbon negative electrode material and preparation method thereof and alkali metal battery
Through chemical pretreatment and benzene organic matter impregnation technology, the thermal stability and structural problems of bamboo-based hard carbon anode materials have been solved, its electrochemical performance and carbon yield have been improved, and large capacity and rapid storage have been achieved.
Patent Information
- Application Number
- CN202410986955.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing bamboo-based hard carbon negative electrode material preparation method has problems such as poor thermal stability and structural melting and foaming, resulting in low carbon yield and poor electrical performance, limiting its application in alkali metal batteries.
Chemical pretreatment ensures uniform penetration of the cross-linking agent, introducing heteroatoms and impregnating cross-linked bamboo powder with benzene-based organic matter to improve the disorder and pore structure of the carbonized product, repair open pores and defects, and improve electrochemical performance.
The carbon yield and electrochemical performance of bamboo-based hard carbon are significantly improved, large capacity and rapid storage are achieved, high first Coulombic efficiency and excellent rate performance are obtained, which is suitable for large-scale production.
Smart Images

Figure CN118515260B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and in particular relates to a bamboo-based hard carbon negative electrode material and a preparation method thereof, and an alkali metal battery. Background Art
[0002] As a new type of negative electrode material, hard carbon has the characteristics of high lithium and sodium storage capacity, low temperature, fast charging, excellent cycle performance and high safety. It is a new generation of negative electrode materials with great potential. In the field of lithium-ion batteries, due to the disordered arrangement of the microcrystalline structure of hard carbon and the large interlayer spacing, lithium ions can easily enter and exit, which can improve the output power of the battery. Under harsh low-temperature conditions, the low working potential of graphite and the slow lithium ion insertion kinetics limit the fast charging performance of lithium-ion batteries. In contrast, the disordered carbon layer of hard carbon promotes the rapid transmission of lithium ions and has better low-temperature performance. Therefore, hard carbon can be used as a negative electrode material and mixed with graphite to effectively improve the battery performance under fast charging and low temperature. In the field of sodium-ion batteries, due to the difficulty of graphite to store sodium and the insufficient capacity of soft carbon, hard carbon has become the preferred negative electrode material for the commercialization of sodium-ion batteries, which is suitable for large-scale energy storage, two-wheeled vehicles, low-speed electric vehicles and other application scenarios. The selection of precursors is crucial for the preparation of high-quality hard carbon materials. At present, the precursors for preparing hard carbon mainly include resins, mineral resources and biomass. Among them, biomass precursors are the mainstream, including coconut shells, apricot shells, starch, lignin, bamboo, etc.
[0003] Bamboo is one of the fastest growing and most carbon-fixing plants in the world, and it generally takes 3-4 years to mature. More importantly, bamboo's innate well-developed cross-linked pores and the structural characteristics of the interconnected internal and external pores provide a natural template for the construction of closed pores inside hard carbon, making it an ideal precursor for hard carbon negative electrode materials. In the prior art, patent CN117163939A discloses a bamboo-based hard carbon negative electrode material for sodium ion batteries and its preparation method and application. It uses bamboo powder as raw material, uses fungi to corrode cellulose in bamboo powder to form pores, and combines subsequent carbonization to prepare bamboo-based hard carbon. However, this method is time-consuming and has a low yield, which is not conducive to its large-scale production. Patent CN116692828A discloses the preparation and application of sodium ion batteries and bamboo-based composite hard carbon negative electrode active materials. It is to pre-treat bamboo powder with alkali first and then acid, and then pre-carbonize, and heat-treat with starch alcohol-water solvent and carbonize to prepare bamboo-based composite hard carbon materials. However, in this method, the starch introduced is a polymer composed of glucose molecules. This natural polymer compound is rich in a variety of oxygen-containing functional groups such as α-1,4 glycosidic bonds and α-1,6 glycosidic bonds, hydroxymethyl, hydroxyl, etc. When the starch is heated, the glycosidic bonds will break, and the C1 atom after the break will be in a left-handed state and react with the C6 atom with higher reaction activity to generate a large amount of left-handed glucose, which will eventually be converted into low molecular weight fragments such as tar, thereby greatly reducing the carbon yield. At the same time, the direct pyrolysis of starch will soften and produce a large amount of gas, and the internal crystalline area will melt. The expansion and escape of these gases will cause the precursor to foam, thereby destroying its original micromorphology, and not utilizing the controllable construction of the hard carbon structure. Patent CN117105199A discloses bamboo-based hard carbon materials and their preparation and application in sodium ion batteries, including regulating bamboo raw materials such as bamboo age and peeling, followed by liquid phase modification in the modifier, and then gas phase roasting modification treatment to construct a microstructure and active sites suitable for sodium ion batteries, improve the performance of sodium ion batteries, and improve the performance uniformity of materials. However, the chemical composition of bamboo is mainly cellulose, hemicellulose and lignin, of which cellulose and hemicellulose account for 60-63wt%. Since cellulose and hemicellulose are both hydrocarbons with poor thermal stability, a large amount of volatiles are produced during the preparation of carbon materials, resulting in a generally low final carbon yield. More importantly, the escape of small molecules during pyrolysis leads to the formation of a large number of defects and pores in the carbon structure. Although these defects and pores provide active sites to improve the sodium / lithium storage capacity and rate performance of hard carbon, they also consume a large amount of sodium ions or lithium ions, increase irreversible capacity, and reduce the initial coulombic efficiency.In addition, the microfibrils in the long fibers show a compact macromolecular structure composed of linear glucose units with strong hydrogen bonds and densely arranged in parallel along the fiber axis. This highly ordered crystal structure significantly reduces its free movement ability, which is not conducive to the regulation of the highly disordered structure in bamboo-based hard carbon, further hindering the practical application of bamboo-based hard carbon as a negative electrode material for alkali metal batteries.
[0004] Therefore, there is an urgent need to provide a method for preparing a bamboo-based hard carbon negative electrode material to solve the problems of poor thermal stability of bamboo powder and structural melting and foaming, thereby improving the electrical performance of alkali metal batteries. Summary of the invention
[0005] In view of the deficiencies of the prior art, the object of the present invention is to provide a bamboo-based hard carbon negative electrode material and a preparation method thereof and an alkali metal battery. The present invention first ensures the uniform penetration of the cross-linking agent in the bamboo structure through chemical pretreatment, realizes the homogenization and cross-linking modification of the bamboo powder, solves the problems of poor thermal stability of the bamboo powder, structural melting and foaming, and improves its carbon yield; at the same time, the cross-linking reaction simultaneously introduces heteroatoms, which can effectively improve the disorder of the carbonization product, widen the carbon layer spacing, enhance the adsorption energy of sodium ions or lithium ions, and significantly improve the electrochemical performance of the bamboo-based hard carbon high platform; in addition, the cross-linked bamboo powder is impregnated with benzene organic matter, and sufficient free radicals are generated under thermal drive, which can quickly rebuild the conjugated carbon structure, thereby repairing the open pores and defects in situ, and significantly improving the reversible capacity of the bamboo-based hard carbon platform area. The bamboo-based hard carbon negative electrode material is expected to achieve large capacity and fast storage at the same time, and obtain high first coulomb efficiency and excellent rate performance. The preparation method has simple equipment, easy control of the operation process, stable product performance, and can achieve large-scale production.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a bamboo-based hard carbon negative electrode material, the preparation method comprising the following steps:
[0008] (1) mixing bamboo powder raw material and alkali solution, and performing chemical pretreatment to obtain softened bamboo powder;
[0009] (2) mixing the softened bamboo powder and a cross-linking agent, and performing a carbonization step to obtain cross-linked bamboo powder;
[0010] (3) The cross-linked bamboo powder and benzene-based organic matter are mixed and subjected to secondary carbonization to obtain the bamboo-based hard carbon negative electrode material.
[0011] The present invention firstly ensures the uniform penetration of the crosslinking agent in the bamboo structure through chemical pretreatment, realizes the homogenization and crosslinking modification of the bamboo powder, solves the problems of poor thermal stability of the bamboo powder, structural melting and foaming, and improves its carbon yield; at the same time, the crosslinking reaction simultaneously introduces heteroatoms, which can effectively improve the disorder of the carbonization product, widen the carbon layer spacing, enhance the adsorption energy of sodium ions or lithium ions, and significantly improve the electrochemical performance of the bamboo-based hard carbon high platform; in addition, the crosslinked bamboo powder is impregnated with benzene organic matter, and sufficient free radicals are generated under thermal drive, which can quickly rebuild the conjugated carbon structure, thereby in situ repairing open pores and defects, and significantly improving the reversible capacity of the bamboo-based hard carbon platform area. The bamboo-based hard carbon negative electrode material is expected to achieve large capacity and fast storage at the same time, and obtain high first coulomb efficiency and excellent rate performance.
[0012] The preparation method provided by the invention has simple equipment, easy-to-control operation process, stable product performance, and can realize large-scale production.
[0013] In the present invention, the purpose of chemical pretreatment is to partially remove lignin and hemicellulose in the bamboo powder raw material.
[0014] As a preferred technical solution of the present invention, the bamboo powder raw material in step (1) includes any one of Bambusa laurelii, Bambusa amarus, Indocalamus pubescens, Bambusa pubescens, Bambusa moso, Bambusa elegans, Bambusa praecox, or a combination of at least two of them.
[0015] It should be noted that the bamboo powder raw materials used in the present invention are all natural bamboo powder, and the age is 3-5 years, for example, 3 years, 4 years or 5 years.
[0016] Preferably, the alkaline solution in step (1) comprises potassium hydroxide solution and / or sodium hydroxide solution.
[0017] Preferably, the concentration of the alkali solution in step (1) is 10-30wt%, for example, 10wt%, 15wt%, 20wt%, 25wt% or 30wt%.
[0018] As a preferred technical solution of the present invention, the mixing method in step (1) is an immersion method.
[0019] Preferably, the mixing time in step (1) is 0.5-2 h, for example, 0.5 h, 1 h, 1.5 h or 2 h.
[0020] Preferably, the temperature of the chemical pretreatment in step (1) is 100-200°C, for example, it can be 100°C, 120°C, 140°C, 160°C, 180°C or 200°C.
[0021] As a preferred technical solution of the present invention, the cross-linking agent in step (2) includes any one of diammonium hydrogen phosphate, phosphoric acid, boric acid or phytic acid, or a combination of at least two thereof.
[0022] In the present invention, heteroatoms such as N, P or B are introduced while adding the crosslinking agent.
[0023] Preferably, the mass ratio of the softened bamboo powder to the cross-linking agent in step (2) is 10:(0.5-8), for example, it can be 10:0.5, 10:1, 10:2, 10:3, 10:4, 10:5, 10:6, 10:7 or 10:8, etc.
[0024] In the present invention, if the mass ratio of softened bamboo powder and cross-linking agent is too small, that is, the amount of cross-linking agent is too much, excessive heteroatoms will be introduced. At high temperature, heteroatoms are easy to overflow, resulting in local gasification of the carbon skeleton, thereby generating a large number of structural defects. These defects will consume a large amount of sodium ions, increase irreversible capacity, and reduce the initial coulomb efficiency; if the mass ratio of softened bamboo powder and cross-linking agent is too large, that is, the amount of cross-linking agent is too small, the cross-linking density will be too low, which is not conducive to the formation of a homogeneous and stable cross-linked structure, resulting in significant gasification, volatilization and volume shrinkage during the high-temperature carbonization of bamboo powder, which ultimately leads to low carbon yield and underdeveloped internal pores of the obtained bamboo-based hard carbon material.
[0025] As a preferred technical solution of the present invention, the mixing method in step (2) includes ball milling.
[0026] Preferably, the mixing time in step (2) is 0.5-2 h, for example, 0.5 h, 1 h, 1.5 h or 2 h.
[0027] Preferably, the primary carbonization in step (2) is carried out in a protective atmosphere.
[0028] Preferably, the gas in the protective atmosphere includes argon and / or nitrogen.
[0029] Preferably, the temperature of the primary carbonization in step (2) is 300-700°C, for example, 300°C, 400°C, 500°C, 600°C or 700°C, etc., preferably 400-650°C.
[0030] In the present invention, if the primary carbonization temperature is too low, the carbonaceous raw materials will not be calcined thoroughly, and the volatile matter will not be fully released, which is not conducive to the controllable construction of closed pores inside the hard carbon during the subsequent high-temperature carbonization process; if the primary carbonization temperature is too high, the free radical content of the carbon matrix will be too low, which is not conducive to the self-healing of open pores in the hard carbon matrix at high temperature to form closed pores. The preferred carbonization temperature is 400-650℃, which can achieve a balance between pore formation and self-healing and maximize the closed pore volume.
[0031] Preferably, the time of the primary carbonization in step (2) is 0.5-3 h, for example, it can be 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h or 3 h, etc., preferably 0.5-1 h.
[0032] Preferably, in step (2), after the primary carbonization, post-treatment is also performed, and the post-treatment steps include:
[0033] The primary carbonized product is first cooled, then washed with acid solution, organic solvent and water in sequence, filtered and dried.
[0034] Preferably, the acid solution includes any one of hydrochloric acid, hydrofluoric acid or acetic acid, or a combination of at least two thereof, preferably hydrofluoric acid.
[0035] It should be noted that the present invention does not limit the type of organic solvent, and illustratively, it may be ethanol or acetone.
[0036] Preferably, the concentration of the acid solution is 1-10wt%, for example, it can be 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%.
[0037] As a preferred technical solution of the present invention, the benzene-based organic matter in step (3) includes any one of toluene, benzaldehyde, methyl benzoate, phenol, nitrobenzene, aniline, benzoic acid, diphenylmethane, triphenylmethane or naphthol, or a combination of at least two thereof.
[0038] Preferably, before the cross-linked bamboo powder and the benzene-based organic matter are mixed in step (3), the benzene-based organic matter is pre-treated, and the pre-treatment step includes:
[0039] The benzene-based organic matter is dissolved in a solvent to obtain a solution containing the benzene-based organic matter.
[0040] Preferably, the concentration of the solution containing benzene-based organic matter is 1-200 mg / mL, for example, it can be 1 mg / mL, 5 mg / mL, 10 mg / mL, 50 mg / mL, 100 mg / mL, 150 mg / mL or 200 mg / mL.
[0041] Preferably, the mixing time in step (3) is 0.5-3 h, for example, 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h or 3 h.
[0042] As a preferred technical solution of the present invention, the secondary carbonization in step (3) is carried out in an inert atmosphere.
[0043] It should be noted that the present invention does not limit the gas in the inert atmosphere, and illustratively, it may be argon or nitrogen.
[0044] Preferably, the temperature of the secondary carbonization in step (3) is 1000-1600°C, for example, it can be 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C or 1600°C, and is preferably 1300-1500°C.
[0045] In the present invention, if the temperature of the secondary carbonization is too low, the open pores cannot be effectively closed, and sufficient closed pores cannot be formed, which is not conducive to the improvement of the platform capacity; if the temperature of the secondary carbonization is too high, although it is conducive to the formation of new closed pores, the migration, accumulation and growth of the graphite layer will cause the closed pores to shrink and the spacing to decrease, hindering the diffusion of sodium ions into the closed pores, thereby reducing the platform capacity.
[0046] Preferably, the insulation time of the secondary carbonization in step (3) is 0.5-5 h, for example, it can be 0.5 h, 1 h, 2 h, 3 h, 4 h or 5 h, and is preferably 1-3 h.
[0047] Preferably, the heating rate of the secondary carbonization in step (3) is 1-3°C / min, for example, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min or 3°C / min.
[0048] Preferably, after the secondary carbonization in step (3), post-treatment is also performed, and the post-treatment steps include:
[0049] The product after secondary carbonization is washed with an acid solution (such as hydrochloric acid, hydrofluoric acid or acetic acid), an organic solvent (such as anhydrous ethanol) and water in sequence, and then dried and crushed.
[0050] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0051] (1) soaking the bamboo powder raw material in an alkali solution with a concentration of 10-30wt% for 0.5-2h, and then performing chemical pretreatment at 100-200°C to obtain softened bamboo powder;
[0052] (2) ball milling the softened bamboo powder and the cross-linking agent in a mass ratio of 10:(0.5-8) in a ball mill for 0.5-2h, then placing the obtained ball milled material in a protective atmosphere for primary carbonization, then cooling to room temperature, and washing with acid, organic solvent and water in sequence, filtering and drying to obtain cross-linked bamboo powder;
[0053] The temperature of the first carbonization is 300-700°C, and the time of the first carbonization is 0.5-3h;
[0054] (3) dissolving the benzene organic matter in a solvent to obtain a solution containing the benzene organic matter with a concentration of 1-200 mg / mL, and then immersing the cross-linked bamboo powder in the solution containing the benzene organic matter under stirring conditions for a period of 0.5-3 hours, and obtaining a cross-linked bamboo powder-coated benzene organic matter intermediate after filtering and drying;
[0055] Wherein, the stirring speed is 200-1000 rpm (for example, it can be 200 rpm, 400 rpm, 600 rpm, 800 rpm or 1000 rpm, etc.);
[0056] (4) in an inert atmosphere, subjecting the cross-linked bamboo powder-coated benzene organic intermediate to secondary carbonization, cooling it to room temperature after completion, and washing it with an acid solution, an organic solvent, and water in sequence, drying it, and crushing it to obtain the bamboo-based hard carbon negative electrode material;
[0057] The temperature of the secondary carbonization is 1000-1600°C, the insulation time of the secondary carbonization is 0.5-5h, and the heating rate of the secondary carbonization is 1-3°C / min.
[0058] In a second aspect, the present invention provides a bamboo-based hard carbon negative electrode material prepared by the preparation method described in the first aspect, wherein the surface pH of the bamboo-based hard carbon negative electrode material is 7-8, for example, it can be 7, 7.2, 7.4, 7.6, 7.8 or 8.
[0059] In the present invention, if the surface pH of the bamboo-based hard carbon negative electrode material is too low, the carboxylmethyl group in the binder such as carboxymethyl cellulose (CMC) molecules will lose negative charge, and the slurry stability will deteriorate; if the pH is too high, the binder such as styrene-butadiene rubber (SBR) glue may demulsify, causing the slurry to settle, thereby reducing the processing performance of the electrode. In order to ensure the stability of the electrode slurry and the excellent processing performance of the electrode, the surface pH of the hard carbon material in the present invention is preferably 7-8.
[0060] Preferably, the specific surface area of the bamboo-based hard carbon negative electrode material is 3-30 m 2 / g, for example, 3m 2 / g, 5m 2 / g, 10m 2 / g, 15m 2 / g, 20m 2 / g, 25m 2 / g or 30m 2 / g, etc.
[0061] Preferably, the interlayer spacing of the bamboo-based hard carbon negative electrode material is 0.38-0.4 nm, for example, 0.38 nm, 0.39 nm or 0.4 nm.
[0062] Preferably, the carbon yield of the bamboo-based hard carbon negative electrode material is 25-45wt%, for example, it can be 25wt%, 30wt%, 35wt%, 40wt% or 45wt%.
[0063] Preferably, the particle size D50 of the bamboo-based hard carbon negative electrode material is ≤15 μm, for example, it may be 15 μm, 10 μm or 5 μm.
[0064] Preferably, the bamboo-based hard carbon negative electrode material has closed pores, and the average pore size of the closed pores is 0.7-1.5 nm, for example, 0.7 nm, 0.9 nm, 1.1 nm, 1.3 nm or 1.5 nm.
[0065] Preferably, the pore connectivity of the bamboo-based hard carbon negative electrode material is ≥0.7, for example, it may be 0.8, 0.9 or 1.
[0066] It should be noted that the pore connectivity of bamboo-based hard carbon anode materials was measured by small-angle X-ray scattering.
[0067] In a third aspect, the present invention provides an alkali metal battery, wherein the alkali metal battery comprises the bamboo-based hard carbon negative electrode material as described in the second aspect.
[0068] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0069] Compared with the prior art, the present invention has the following beneficial effects:
[0070] (1) The present invention firstly ensures the uniform penetration of the crosslinking agent in the bamboo structure through chemical pretreatment, realizes the homogenization and crosslinking modification of the bamboo powder, solves the problems of poor thermal stability of bamboo powder and structural melting and foaming, and improves its carbon yield; at the same time, the crosslinking reaction simultaneously introduces heteroatoms, which can effectively improve the disorder of the carbonization product, widen the carbon layer spacing, enhance the adsorption energy of sodium ions or lithium ions, significantly improve the discharge voltage of bamboo-based hard carbon, and improve its reversible capacity; in addition, the crosslinked bamboo powder is impregnated with benzene organic matter, and sufficient free radicals are generated under thermal drive, which can quickly rebuild the conjugated carbon structure, thereby in situ repairing open pores and defects, and further improve the reversible capacity of the bamboo-based hard carbon platform area. The bamboo-based hard carbon negative electrode material is expected to achieve large capacity and fast storage at the same time, and obtain high first coulomb efficiency and excellent rate performance.
[0071] (2) The preparation method provided by the present invention has simple equipment, easy-to-control operation process, stable product performance, and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] Figure 1 This is the thermogravimetric curve of the bamboo-based hard carbon negative electrode material prepared in Example 1 of the present invention.
[0073] Figure 2 This is the charge and discharge curve of the bamboo-based hard carbon negative electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0074] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0075] It should be noted that the room temperature below refers to 25°C.
[0076] Example 1
[0077] This embodiment provides a method for preparing a bamboo-based hard carbon negative electrode material, the preparation method comprising the following steps:
[0078] (1) 20 g of raw material of moso bamboo powder was vacuum impregnated in a sodium hydroxide solution with a concentration of 20 wt% for 1 h, and then chemically pretreated at 150° C. to obtain softened bamboo powder;
[0079] (2) The softened bamboo powder and the cross-linking agent diammonium hydrogen phosphate are ball-milled in a ball mill at a mass ratio of 10:5 for 1 hour, and then the obtained ball-milled material is placed in a tube furnace under an argon atmosphere for a carbonization. After the carbonization, the ball-milled material is cooled to room temperature, and then washed with 5wt% hydrofluoric acid, anhydrous ethanol and deionized water in sequence, filtered and dried to obtain cross-linked bamboo powder;
[0080] Among them, the temperature of the first carbonization is 650℃, and the time of the first carbonization is 1h;
[0081] (3) dissolving phenol in ethanol to obtain a phenol ethanol solution with a concentration of 30 mg / mL, and then immersing the cross-linked bamboo powder in the phenol ethanol solution under magnetic stirring for 1 hour, and obtaining a cross-linked bamboo powder-coated phenol intermediate after filtering and drying;
[0082] Among them, the speed of magnetic stirring is 600rpm;
[0083] (4) placing the cross-linked bamboo powder-coated phenol intermediate in a carbonization furnace, and subjecting the cross-linked bamboo powder-coated phenol intermediate to secondary carbonization in an argon atmosphere, cooling the intermediate to room temperature after the carbonization, and then washing the intermediate with 5 wt % hydrofluoric acid, anhydrous ethanol and deionized water in sequence, drying and crushing the intermediate to obtain the bamboo-based hard carbon negative electrode material;
[0084] Among them, the temperature of the secondary carbonization is 1300°C, the insulation time of the secondary carbonization is 1h, and the heating rate of the secondary carbonization is 2°C / min.
[0085] This embodiment also provides a bamboo-based hard carbon negative electrode material prepared by the above preparation method, wherein the surface pH of the bamboo-based hard carbon negative electrode material is 7.1 and the specific surface area is 5.6 m 2 / g, the interlayer spacing is 0.39nm, the particle size D50 is 7.2μm, and the pore connectivity of the bamboo-based hard carbon negative electrode material is 0.82;
[0086] The bamboo-based hard carbon negative electrode material has closed pores, and the average pore diameter of the closed pores is 1.1 nm.
[0087] Figure 1 The thermogravimetric curve of the bamboo-based hard carbon negative electrode material prepared in this embodiment is shown. It can be seen from the figure that the carbon yield of the cross-linked bamboo powder is about 30.5wt%, which is significantly improved compared with the carbon yield of pure bamboo powder (21wt%).
[0088] Figure 2 The charge and discharge curve of the bamboo-based hard carbon negative electrode material prepared in this embodiment is shown. It can be seen from the figure that the charge and discharge curve of the bamboo-based hard carbon includes a high potential slope area (0.1-2V) and a low potential platform area (0-0.1V). Among them, the slope area is related to the reversible adsorption of sodium ions in defects and chemical bonds, and the platform area is related to the insertion of sodium ions into the graphite interlayer and the deposition in the closed pores. The introduction of the cross-linked structure in the bamboo powder greatly broadens the interlayer spacing and the number of closed pores of its hard carbon structure, thereby improving the sodium storage capacity of the bamboo-based hard carbon.
[0089] Example 2
[0090] This embodiment provides a method for preparing a bamboo-based hard carbon negative electrode material, the preparation method comprising the following steps:
[0091] (1) 20 g of bamboo powder raw material was vacuum impregnated in a sodium hydroxide solution with a concentration of 10 wt% for 2 h, and then chemically pretreated at 200 °C to obtain softened bamboo powder;
[0092] (2) The softened bamboo powder and the cross-linking agent diammonium hydrogen phosphate are ball-milled in a ball mill at a mass ratio of 10:1 for 0.5 h, and then the obtained ball-milled material is placed in a tube furnace under an argon atmosphere for a carbonization. After the carbonization, the material is cooled to room temperature, and then washed with 5wt% hydrofluoric acid, anhydrous ethanol and deionized water in sequence, filtered and dried to obtain cross-linked bamboo powder;
[0093] Among them, the temperature of the first carbonization is 700℃, and the time of the first carbonization is 1h;
[0094] (3) dissolving benzoic acid in ethanol to obtain a benzoic acid ethanol solution with a concentration of 50 mg / mL, and then immersing the cross-linked bamboo powder in the benzoic acid ethanol solution under magnetic stirring for 3 hours, filtering and drying to obtain a cross-linked bamboo powder-coated benzoic acid intermediate;
[0095] Among them, the speed of magnetic stirring is 200 rpm;
[0096] (4) placing the cross-linked bamboo powder coated benzoic acid intermediate in a carbonization furnace, and subjecting the cross-linked bamboo powder coated benzoic acid intermediate to secondary carbonization in an argon atmosphere, cooling the intermediate to room temperature after the carbonization, and then washing the intermediate with 5 wt% hydrofluoric acid, anhydrous ethanol and deionized water in sequence, drying and crushing the intermediate to obtain the bamboo-based hard carbon negative electrode material;
[0097] Among them, the temperature of the secondary carbonization is 1500°C, the insulation time of the secondary carbonization is 1h, and the heating rate of the secondary carbonization is 3°C / min.
[0098] This embodiment also provides a bamboo-based hard carbon negative electrode material prepared by the above preparation method, wherein the surface pH of the bamboo-based hard carbon negative electrode material is 7.3 and the specific surface area is 4.3 m 2 / g, interlayer spacing of 0.383nm, carbon yield of 28.2wt%, particle size D50 of 7.6μm, and pore connectivity of the bamboo-based hard carbon negative electrode material of 0.73;
[0099] The bamboo-based hard carbon negative electrode material has closed pores, and the average pore diameter of the closed pores is 1.1 nm.
[0100] Example 3
[0101] This embodiment provides a method for preparing a bamboo-based hard carbon negative electrode material, the preparation method comprising the following steps:
[0102] (1) 20 g of raw material of moso bamboo powder was vacuum impregnated in a sodium hydroxide solution with a concentration of 30 wt % for 0.5 h, and then chemically pretreated at 100 ° C to obtain softened bamboo powder;
[0103] (2) The softened bamboo powder and the cross-linking agent boric acid are ball-milled in a ball mill at a mass ratio of 10:0.5 for 0.5 h, and then the obtained ball-milled material is placed in a tube furnace under an argon atmosphere for a carbonization, and then cooled to room temperature, and then washed with 5wt% hydrofluoric acid, anhydrous ethanol and deionized water in sequence, filtered and dried to obtain cross-linked bamboo powder;
[0104] Among them, the temperature of the first carbonization is 500℃, and the time of the first carbonization is 2h;
[0105] (3) dissolving benzoic acid in ethanol to obtain a benzoic acid ethanol solution with a concentration of 50 mg / mL, and then immersing the cross-linked bamboo powder in the benzoic acid ethanol solution under magnetic stirring for 1 hour, filtering and drying to obtain a cross-linked bamboo powder-coated benzoic acid intermediate;
[0106] Among them, the speed of magnetic stirring is 800rpm;
[0107] (4) placing the cross-linked bamboo powder coated benzoic acid intermediate in a carbonization furnace, and subjecting the cross-linked bamboo powder coated benzoic acid intermediate to secondary carbonization in an argon atmosphere, cooling the intermediate to room temperature after the carbonization, and then washing the intermediate with 5 wt% hydrofluoric acid, anhydrous ethanol and deionized water in sequence, drying and crushing the intermediate to obtain the bamboo-based hard carbon negative electrode material;
[0108] The temperature of the secondary carbonization is 1000°C, the holding time of the secondary carbonization is 3h, and the heating rate of the secondary carbonization is 1°C / min.
[0109] This embodiment also provides a bamboo-based hard carbon negative electrode material prepared by the above preparation method, wherein the surface pH of the bamboo-based hard carbon negative electrode material is 7 and the specific surface area is 8.4 m 2 / g, interlayer spacing is 0.384nm, carbon yield is 30.1wt%, particle size D50 is 7.28μm, and the pore connectivity of the bamboo-based hard carbon negative electrode material is 0.7;
[0110] The bamboo-based hard carbon negative electrode material has closed pores, and the average pore diameter of the closed pores is 1.4 nm.
[0111] Example 4
[0112] This embodiment provides a method for preparing a bamboo-based hard carbon negative electrode material, the preparation method comprising the following steps:
[0113] (1) 20 g of raw material of moso bamboo powder was vacuum impregnated in a sodium hydroxide solution with a concentration of 10 wt % for 0.5 h, and then chemically pretreated at 120° C. to obtain softened bamboo powder;
[0114] (2) The softened bamboo powder and the cross-linking agent phytic acid are ball-milled in a ball mill at a mass ratio of 10:5 for 2 h, and then the obtained ball-milled material is placed in a tube furnace under a nitrogen atmosphere for a carbonization. After the carbonization, the ball-milled material is cooled to room temperature, and then washed with 5 wt% hydrofluoric acid, anhydrous ethanol and deionized water in sequence, filtered and dried to obtain cross-linked bamboo powder;
[0115] Among them, the temperature of the first carbonization is 600℃, and the time of the first carbonization is 2h;
[0116] (3) dissolving naphthol in ethanol to obtain a naphthol ethanol solution with a concentration of 20 mg / mL, and then immersing the cross-linked bamboo powder in the naphthol ethanol solution under magnetic stirring for 1.5 h, and obtaining a cross-linked bamboo powder-coated naphthol intermediate after filtering and drying;
[0117] Among them, the speed of magnetic stirring is 500 rpm;
[0118] (4) placing the cross-linked bamboo powder-coated naphthol intermediate in a carbonization furnace, and subjecting the cross-linked bamboo powder-coated benzoic acid intermediate to secondary carbonization in a nitrogen atmosphere, cooling to room temperature after completion, and then washing with 5wt% hydrofluoric acid, anhydrous ethanol and deionized water in sequence, drying and crushing to obtain the bamboo-based hard carbon negative electrode material;
[0119] Among them, the temperature of the secondary carbonization is 1300°C, the insulation time of the secondary carbonization is 2h, and the heating rate of the secondary carbonization is 2°C / min.
[0120] This embodiment also provides a bamboo-based hard carbon negative electrode material prepared by the above preparation method, wherein the surface pH of the bamboo-based hard carbon negative electrode material is 7 and the specific surface area is 6.4 m 2 / g, interlayer spacing of 0.388nm, carbon yield of 25wt%, particle size D50 of 7.28μm, and pore connectivity of the bamboo-based hard carbon negative electrode material of 0.75;
[0121] The bamboo-based hard carbon negative electrode material has closed pores, and the average pore diameter of the closed pores is 1.4 nm.
[0122] Example 5
[0123] This embodiment provides a method for preparing a bamboo-based hard carbon negative electrode material, the preparation method comprising the following steps:
[0124] (1) 20 g of raw material of moso bamboo powder was vacuum impregnated in a sodium hydroxide solution with a concentration of 20 wt % for 0.5 h, and then chemically pretreated at 150° C. to obtain softened bamboo powder;
[0125] (2) The softened bamboo powder and the cross-linking agent diammonium hydrogen phosphate are ball-milled in a ball mill at a mass ratio of 10:4 for 1 hour, and then the obtained ball-milled material is placed in a tube furnace under an argon atmosphere for a carbonization. After the carbonization, the ball-milled material is cooled to room temperature, and then washed with 5wt% hydrofluoric acid, anhydrous ethanol and deionized water in sequence, filtered and dried to obtain cross-linked bamboo powder;
[0126] Among them, the temperature of the first carbonization is 600℃, and the time of the first carbonization is 3h;
[0127] (3) dissolving naphthol in ethanol to obtain a naphthol ethanol solution with a concentration of 20 mg / mL, and then immersing the cross-linked bamboo powder in the naphthol ethanol solution under magnetic stirring for 1 hour, filtering and drying to obtain a cross-linked bamboo powder-coated naphthol intermediate;
[0128] Among them, the speed of magnetic stirring is 800rpm;
[0129] (4) placing the cross-linked bamboo powder-coated naphthol intermediate in a carbonization furnace, and subjecting the cross-linked bamboo powder-coated benzoic acid intermediate to secondary carbonization in an argon atmosphere, cooling to room temperature after completion, and then washing with 5wt% hydrofluoric acid, anhydrous ethanol and deionized water in sequence, drying and crushing to obtain the bamboo-based hard carbon negative electrode material;
[0130] Among them, the temperature of the secondary carbonization is 1300°C, the insulation time of the secondary carbonization is 2h, and the heating rate of the secondary carbonization is 2°C / min.
[0131] This embodiment also provides a bamboo-based hard carbon negative electrode material prepared by the above preparation method, wherein the surface pH of the bamboo-based hard carbon negative electrode material is 7.1 and the specific surface area is 6.27 m 2 / g, interlayer spacing of 0.38nm, carbon yield of 29.6wt%, particle size D50 of 6.76μm, and pore connectivity of the bamboo-based hard carbon negative electrode material of 0.72;
[0132] The bamboo-based hard carbon negative electrode material has closed pores, and the average pore diameter of the closed pores is 1.3 nm.
[0133] Example 6
[0134] The difference between this embodiment and embodiment 1 is that in step (2), the mass ratio of softened bamboo powder to cross-linking agent diammonium hydrogen phosphate is 10:10.
[0135] The rest of the preparation methods and parameters were the same as those in Example 1.
[0136] Example 7
[0137] The difference between this embodiment and embodiment 1 is that in step (2), the mass ratio of softened bamboo powder to cross-linking agent diammonium hydrogen phosphate is 15:0.5.
[0138] The rest of the preparation methods and parameters were the same as those in Example 1.
[0139] Example 8
[0140] The difference between this embodiment and embodiment 1 is that the temperature of the primary carbonization in step (2) is 200°C.
[0141] The rest of the preparation methods and parameters were the same as those in Example 1.
[0142] Example 9
[0143] The difference between this embodiment and embodiment 1 is that the temperature of the primary carbonization in step (2) is 800°C.
[0144] The rest of the preparation methods and parameters were the same as those in Example 1.
[0145] Example 10
[0146] The difference between this embodiment and embodiment 1 is that the temperature of the secondary carbonization in step (4) is 900°C.
[0147] The rest of the preparation methods and parameters were the same as those in Example 1.
[0148] Embodiment 11
[0149] The difference between this embodiment and embodiment 1 is that the temperature of the secondary carbonization in step (4) is 1700°C.
[0150] The rest of the preparation methods and parameters were the same as those in Example 1.
[0151] Comparative Example 1
[0152] The difference between this comparative example and Example 1 is that the cross-linking agent diammonium hydrogen phosphate is not added in step (2).
[0153] The rest of the preparation methods and parameters were the same as those in Example 1.
[0154] Comparative Example 2
[0155] The difference between this comparative example and Example 1 is that step (3) is not performed, but the cross-linked bamboo powder obtained in step (2) is directly subjected to secondary carbonization.
[0156] The rest of the preparation methods and parameters were the same as those in Example 1.
[0157] Performance Testing
[0158] The CR2032 button battery is prepared based on the bamboo-based hard carbon negative electrode material prepared in the above embodiment and comparative example, and the specific steps include:
[0159] The bamboo-based hard carbon negative electrode material, carbon black and polyvinylidene fluoride were mixed in a mass ratio of 80:10:10 to form a slurry, which was then evenly scraped onto the current collector aluminum foil. After drying, the electrode sheets were cut. The battery was assembled in a glove box with Ar atmosphere, using metallic sodium as the counter electrode and 1M NaClO4 (the solvent included ethylene carbonate and diethyl carbonate in a volume ratio of 1:1) solution as the electrolyte to form a CR2032 button battery.
[0160] The above CR2032 button battery was charged and discharged under the following conditions:
[0161] The current density was 30 mA / g and the voltage was 0.001–2 V.
[0162] The test results are shown in Table 1.
[0163] Table 1
[0164]
[0165] analyze:
[0166] It can be seen from the above table that the bamboo-based hard carbon negative electrode material prepared by the preparation method provided by the present invention has excellent reversible capacity, high first coulombic efficiency and excellent rate performance, and is expected to achieve large capacity and fast storage at the same time.
[0167] It can be seen from Example 1 and Example 6-7 that if the mass ratio of softened bamboo powder and cross-linking agent is too small, that is, the amount of cross-linking agent is too much, excessive heteroatoms will be introduced. At high temperatures, heteroatoms are easy to overflow, resulting in local gasification of the carbon skeleton, thereby generating a large number of structural defects. These defects will consume a large amount of sodium ions, increase irreversible capacity, and reduce the initial coulomb efficiency; if the mass ratio of softened bamboo powder and cross-linking agent is too large, that is, the amount of cross-linking agent is too small, the cross-linking density will be too low, which is not conducive to the formation of a homogeneous and stable cross-linked structure, resulting in significant gasification, volatilization and volume shrinkage during the high-temperature carbonization of bamboo powder, which ultimately leads to low carbon yield and underdeveloped internal pores of the obtained bamboo-based hard carbon material, and low capacity.
[0168] It can be seen from Example 1 and Examples 8-9 that if the temperature of the primary carbonization is too low, the carbonaceous raw material will not be calcined thoroughly and the volatile matter cannot be fully released, which is not conducive to the controllable construction of closed pores inside the hard carbon during the subsequent high-temperature carbonization process; if the temperature of the primary carbonization is too high, it will cause the free radical content of the carbon matrix to be too low, which is not conducive to the self-healing of open pores in the hard carbon matrix at high temperature to form closed pores.
[0169] It can be seen from Example 1 and Examples 10-11 that if the temperature of the secondary carbonization is too low, the open pores cannot be effectively closed, and sufficient closed pores cannot be formed, which is not conducive to the improvement of the platform capacity; if the temperature of the secondary carbonization is too high, although it is conducive to the formation of new closed pores, the migration, accumulation and growth of the graphite layer will cause the closed pores to shrink and the spacing to decrease, hindering the diffusion of sodium ions into the closed pores, thereby reducing the platform capacity.
[0170] It can be seen from Example 1 and Comparative Example 1 that if the cross-linking agent diammonium hydrogen phosphate is not added, the starch will be directly pyrolyzed to soften and produce a large amount of gas, and the internal crystalline area will melt. The expansion and escape of these gases will cause the precursor to foam, thereby destroying its original microscopic morphology, and the hard carbon structure will not be controllably constructed, resulting in low capacity and rate.
[0171] It can be seen from Example 1 and Comparative Example 2 that if step (3) is not performed but the cross-linked bamboo powder obtained in step (2) is directly subjected to secondary carbonization, the larger open voids inside the hard carbon cannot be effectively healed to form closed pores, resulting in a lower initial efficiency.
[0172] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a bamboo-based hard carbon negative electrode material, characterized in that: The preparation method comprises the following steps: (1) soaking the bamboo powder raw material in an alkali solution with a concentration of 10-30wt% for 0.5-2h, and then performing chemical pretreatment at 100-200°C to obtain softened bamboo powder; (2) ball milling the softened bamboo powder and the cross-linking agent in a mass ratio of 10:(0.5-8) in a ball mill for 0.5-2h, then placing the obtained ball milled material in a protective atmosphere for primary carbonization, then cooling to room temperature, and washing with acid, organic solvent and water in sequence, filtering and drying to obtain cross-linked bamboo powder; The temperature of the first carbonization is 300-700°C, and the time of the first carbonization is 0.5-3h; the cross-linking agent includes any one of diammonium hydrogen phosphate, phosphoric acid, boric acid or phytic acid, or a combination of at least two thereof; (3) dissolving the benzene organic matter in a solvent to obtain a solution containing the benzene organic matter with a concentration of 1-200 mg / mL, and then immersing the cross-linked bamboo powder in the solution containing the benzene organic matter under stirring conditions for a period of 0.5-3 hours, and obtaining a cross-linked bamboo powder-coated benzene organic matter intermediate after filtering and drying; Wherein, the stirring speed is 200-1000rpm; (4) in an inert atmosphere, the cross-linked bamboo powder-coated benzene organic intermediate is subjected to secondary carbonization, then cooled to room temperature, washed with acid, organic solvent and water in sequence, dried and crushed to obtain the bamboo-based hard carbon negative electrode material; The temperature of the secondary carbonization is 1000-1600°C, the insulation time of the secondary carbonization is 0.5-5h, and the heating rate of the secondary carbonization is 1-3°C / min.
2. The preparation method according to claim 1, characterized in that: The temperature of the secondary carbonization in step (4) is 1300-1500°C.
3. The preparation method according to claim 1, characterized in that: The insulation time of the secondary carbonization in step (4) is 1-3h.
4. A bamboo-based hard carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 3, characterized in that: The surface pH of the bamboo-based hard carbon negative electrode material is 7-8; The specific surface area of the bamboo-based hard carbon negative electrode material is 3-30 m 2 / g; The interlayer spacing of the bamboo-based hard carbon negative electrode material is 0.38-0.4nm; The carbon yield of the bamboo-based hard carbon negative electrode material is 25-45wt%; The particle size D50 of the bamboo-based hard carbon negative electrode material is ≤15 μm; The bamboo-based hard carbon negative electrode material has closed pores, and the average pore size of the closed pores is 0.7-1.5 nm; The pore connectivity of the bamboo-based hard carbon negative electrode material is ≥0.
7.
5. An alkali metal battery, characterized in that: The alkali metal battery comprises the bamboo-based hard carbon negative electrode material as claimed in claim 4.
Citation Information
Patent Citations
Sodium-ion battery and preparation and application of bamboo-based composite hard carbon negative electrode active material of sodium-ion battery
CN116692828A
Bamboo-based hard carbon material, preparation thereof and application of bamboo-based hard carbon material in sodium ion battery
CN117105199A
Hard carbon negative electrode material for bamboo-based sodium ion battery as well as preparation method and application of hard carbon negative electrode material
CN117163939A
Method for making bamboo reed activated carbon
CN110156007A
High-performance biomass-based hard carbon negative electrode material and preparation method thereof
CN118083951A