A kind of preparation method of modified sodium polyacrylate dispersant
Through the preparation method of modified sodium polyacrylate dispersant, copolymerization is used to form a charged diffusion layer, which solves the problem of insufficient dispersion performance of sodium polyacrylate dispersant in certain applications and achieves better dispersion performance and suspension stability. .
Patent Information
- Application Number
- CN202410985585.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-23
AI Technical Summary
Existing sodium polyacrylate dispersants have insufficient dispersion properties in some applications and are difficult to effectively stabilize suspensions. In particular, they have problems such as high agglomeration, high viscosity, and poor dispersion in calcium carbonate grinding and slurry processing.
A preparation method of modified sodium polyacrylate dispersant is adopted, and a series of raw materials such as p-aldehyde benzoic acid, tris(2-aminoethyl)amine, 1,3-propanesulfonolactone, allyl bromide and other raw materials are used. Reaction to form intermediate 3, and through copolymerization, a modified sodium polyacrylate dispersant is obtained. The alkenyl group and methacrylic acid contained in it are used to copolymerize to form a diffusion layer of charged ions, which enhances electrostatic repulsion, prevents flocculation, and improves dispersion performance. .
The prepared modified sodium polyacrylate dispersant has good dispersion properties and can be effectively adsorbed on the particle surface to form a complete covering layer to prevent flocculation, improve the stability and dispersion properties of the suspension, and is suitable for calcium carbonate grinding and slurry treatment. .
Smart Images

Figure CN118515808B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dispersants, in particular to a method for preparing a modified sodium polyacrylate dispersant. Background Art
[0002] Dispersants are widely used in coal, ore, paint, ceramics, pesticides and other products to obtain uniform and stable suspensions. Dispersants affect the stability of suspensions by increasing steric hindrance or providing electrostatic barriers to prevent flocculation. Among the many dispersants, polymer dispersants improve the stability of suspensions by adsorbing particles. Therefore, designing and synthesizing new polymer dispersants and studying their dispersing properties are of certain significance to improving the dispersing properties of various products.
[0003] Sodium polyacrylate is a new functional polymer material and an important chemical product. It is made from acrylic acid and its esters through aqueous solution polymerization. It is widely used in water treatment agents, thickeners, flocculants, dispersants and other fields. It belongs to a type of polymer electrolyte and is a new type of polymer material with a wide range of uses.
[0004] For example, the patent application with publication number CN102775546A discloses a branched polyacrylic acid dispersant and its preparation method and application. The invention introduces polyene monomers into sodium polyacrylate dispersant to obtain a branched dispersed structure, which is applied to calcium carbonate to reduce the agglomeration degree between calcium carbonate particles, so that the grinding of calcium carbonate has the characteristics of high grinding efficiency, low slurry viscosity, good dispersibility and relatively stable. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the deficiencies of the prior art, the present invention provides a method for preparing a modified sodium polyacrylate dispersant. The prepared modified sodium polyacrylate dispersant has good dispersing performance.
[0007] (II) Technical solution
[0008] A preparation method of a modified sodium polyacrylate dispersant, the preparation method is as follows:
[0009] (1) Add p-formylbenzoic acid to methanol solvent, stir and disperse, add tri(2-aminoethyl)amine at 5-10°C, stir evenly, raise the temperature to 20-35°C, react for 6-12h, add sodium borohydride, continue to react for 2-5h, remove formaldehyde after the reaction, extract with chloroform, wash, dry, and rotary evaporate to obtain intermediate 1.
[0010] (2) Add intermediate 1 to methanol solvent, stir and disperse, then add 1,3-propanesulfonic acid lactone, stir evenly, heat to 60-70°C, react for 24-48 hours, then add sodium carbonate, continue stirring and react for 2-4 hours. After the reaction is completed, filter, distill under reduced pressure, wash, and dry to obtain intermediate 2.
[0011] (3) Add intermediate 2 to acetone solvent, stir and disperse, add allyl bromide at 5-10°C, continue stirring and reacting for 5-10 hours, and after the reaction is completed, filter, wash and dry to obtain intermediate 3.
[0012] (4) Add intermediate 3, acrylic acid, methacrylic acid, sodium sulfite and potassium persulfate into deionized water, stir and disperse, heat to 60-80°C, react for 5-10 hours, and after the reaction is completed, cool to 40-50°C, add sodium hydroxide solution to adjust the pH to 7-9, and obtain a modified sodium polyacrylate dispersant.
[0013] Preferably, in step (1), the molar ratio of p-formylbenzoic acid, tris(2-aminoethyl)amine, and sodium borohydride is 3-4:1:3.5-4.5.
[0014] Preferably, in step (2), the molar ratio of the intermediate 1, 1,3-propanesulfonate, and sodium carbonate is 1:3-6:4-6.
[0015] Preferably, in step (3), the molar ratio of the intermediate 2 to allyl bromide is 1:1-1.5.
[0016] Preferably, in step (4), the molar ratio of the intermediate 3, acrylic acid and methacrylic acid is 0.5-1:1:1-1.3.
[0017] Preferably, in step (4), the molar ratio of sodium sulfite to potassium persulfate is 1.5:1; and the amount of potassium persulfate used is 15% of the mass of acrylic acid.
[0018] Preferably, in step (4), the mass concentration of the sodium hydroxide solution is 30%.
[0019] 3. Beneficial technical effects
[0020] The present invention uses p-formylbenzoic acid, tris(2-aminoethyl)amine, 1,3-propanesulfonic acid lactone, allyl bromide and the like as raw materials, and undergoes a series of reactions to obtain an intermediate 3, and copolymerizes the alkenyl contained in the intermediate 3 with acrylic acid and methacrylic acid to obtain a modified sodium polyacrylate dispersant. The intermediate 3 prepared by the present invention is simple in preparation method and novel in structure through Schiff base reaction, reduction reaction, ring-opening alkylation reaction and quaternization reaction.
[0021] The modified sodium polyacrylate dispersant prepared by the present invention contains hydrophilic groups such as carboxyl and sulfonic acid groups, which can be adsorbed on the surface of slurry particles so that the particles have the same charge, while the remaining particles with opposite charges freely diffuse into the surrounding liquid medium to form a diffusion layer of charged ions, and then form a double electric layer, so that the particles are stably present in the medium through electrostatic repulsion, and because the adsorption layer formed by the dispersant on the particle surface can completely cover the particle surface, flocculation is further prevented and the dispersion performance is improved. The modified sodium polyacrylate dispersant prepared by the present invention has good dispersion performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the preparation route of intermediate 3. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further described below with reference to specific embodiments, but the protection content of the present invention is not limited thereto. Embodiment 1
[0024] (1) Add 35 mmol of p-formylbenzoic acid to 100 mL of methanol solvent and stir to disperse. Then add 10 mmol of tris(2-aminoethyl)amine at 10°C and stir evenly. Heat to 20°C and react for 12 h. Then add 40 mmol of sodium borohydride and continue to react for 4 h. After the reaction is completed, remove formaldehyde, extract with chloroform, wash, dry and evaporate to obtain intermediate 1.
[0025] (2) Add 8 mmol of intermediate 1 to 150 mL of methanol solvent, stir and disperse, then add 30 mmol of 1,3-propanesulfonic acid lactone, stir evenly, heat to 70°C, react for 42 hours, then add 48 mmol of sodium carbonate, continue stirring and react for 3 hours. After the reaction is completed, filter, evaporate under reduced pressure, wash, and dry to obtain intermediate 2.
[0026] (3) Add 20 mmol of intermediate 2 into 150 mL of acetone solvent and stir to disperse. Then add 25 mmol of allyl bromide at 10°C and continue stirring to react for 5 h. After the reaction is completed, filter, wash and dry to obtain intermediate 3.
[0027] (4) 10 mmol of intermediate 3, 20 mmol of acrylic acid, 20 mmol of methacrylic acid, 1.2 mmol of sodium sulfite and 0.8 mmol of potassium persulfate were added to deionized water, stirred and dispersed, heated to 60°C, and reacted for 5 h. After the reaction was completed, cooled to 40°C, and a sodium hydroxide solution with a mass concentration of 30% was added thereto to adjust the pH to 9, thereby obtaining a modified sodium polyacrylate dispersant. Embodiment 2
[0028] (1) Add 40 mmol of p-formylbenzoic acid to 100 mL of methanol solvent and stir to disperse. Then add 10 mmol of tris(2-aminoethyl)amine at 5°C and stir evenly. Heat to 35°C and react for 10 h. Then add 45 mmol of sodium borohydride and continue to react for 5 h. After the reaction is completed, remove formaldehyde, extract with chloroform, wash, dry and evaporate to obtain intermediate 1.
[0029] (2) Add 8 mmol of intermediate 1 to 150 mL of methanol solvent, stir and disperse, then add 30 mmol of 1,3-propanesulfonic acid lactone, stir evenly, heat to 70°C, react for 48 hours, then add 48 mmol of sodium carbonate, continue stirring and react for 2 hours. After the reaction is completed, filter, evaporate under reduced pressure, wash, and dry to obtain intermediate 2.
[0030] (3) Add 20 mmol of intermediate 2 into 150 mL of acetone solvent and stir to disperse. Then add 25 mmol of allyl bromide at 5°C and continue stirring to react for 6 h. After the reaction is completed, filter, wash and dry to obtain intermediate 3.
[0031] (4) 12 mmol of intermediate 3, 20 mmol of acrylic acid, 25 mmol of methacrylic acid, 1.2 mmol of sodium sulfite and 0.8 mmol of potassium persulfate were added to deionized water, stirred and dispersed, heated to 80°C, and reacted for 6 hours. After the reaction was completed, the mixture was cooled to 50°C, and a sodium hydroxide solution with a mass concentration of 30% was added to adjust the pH to 7 to obtain a modified sodium polyacrylate dispersant. Embodiment 3
[0032] (1) Add 40 mmol of p-formylbenzoic acid to 100 mL of methanol solvent and stir to disperse. Then add 10 mmol of tris(2-aminoethyl)amine at 5°C and stir evenly. Heat to 25°C and react for 6 h. Then add 35 mmol of sodium borohydride and continue to react for 2 h. After the reaction is completed, remove formaldehyde, extract with chloroform, wash, dry and evaporate to obtain intermediate 1.
[0033] (2) Add 8 mmol of intermediate 1 to 150 mL of methanol solvent, stir and disperse, then add 48 mmol of 1,3-propanesulfonic acid lactone, stir evenly, heat to 65°C, react for 24 h, then add 32 mmol of sodium carbonate, continue stirring and react for 4 h. After the reaction is completed, filter, evaporate under reduced pressure, wash, and dry to obtain intermediate 2.
[0034] (3) Add 20 mmol of intermediate 2 into 150 mL of acetone solvent and stir to disperse. Then add 20 mmol of allyl bromide at 5°C and continue stirring to react for 5 h. After the reaction is completed, filter, wash and dry to obtain intermediate 3.
[0035] (4) 15 mmol of intermediate 3, 20 mmol of acrylic acid, 26 mmol of methacrylic acid, 1.2 mmol of sodium sulfite and 0.8 mmol of potassium persulfate were added to deionized water, stirred and dispersed, heated to 70°C, reacted for 10 h, and after the reaction was completed, cooled to 45°C, and a sodium hydroxide solution with a mass concentration of 30% was added thereto to adjust the pH to 9, thereby obtaining a modified sodium polyacrylate dispersant. Embodiment 4
[0036] (1) Add 35 mmol of p-formylbenzoic acid to 100 mL of methanol solvent and stir to disperse. Then add 10 mmol of tris(2-aminoethyl)amine at 5°C and stir evenly. Heat to 35°C and react for 10 h. Then add 45 mmol of sodium borohydride and continue to react for 4 h. After the reaction is completed, remove formaldehyde, extract with chloroform, wash, dry and evaporate to obtain intermediate 1.
[0037] (2) Add 8 mmol of intermediate 1 to 150 mL of methanol solvent, stir and disperse, then add 30 mmol of 1,3-propanesulfonic acid lactone, stir evenly, heat to 70°C, react for 48 hours, then add 48 mmol of sodium carbonate, continue stirring and react for 3 hours. After the reaction is completed, filter, evaporate under reduced pressure, wash, and dry to obtain intermediate 2.
[0038] (3) Add 20 mmol of intermediate 2 into 150 mL of acetone solvent and stir to disperse. Then add 30 mmol of allyl bromide at 5°C and continue stirring to react for 6 h. After the reaction is completed, filter, wash and dry to obtain intermediate 3.
[0039] (4) 18 mmol of intermediate 3, 20 mmol of acrylic acid, 26 mmol of methacrylic acid, 1.2 mmol of sodium sulfite and 0.8 mmol of potassium persulfate were added to deionized water, stirred and dispersed, heated to 70°C, and reacted for 8 h. After the reaction was completed, the mixture was cooled to 50°C, and a sodium hydroxide solution with a mass concentration of 30% was added to adjust the pH to 7 to obtain a modified sodium polyacrylate dispersant. Embodiment 5
[0040] (1) Add 35 mmol of p-formylbenzoic acid to 100 mL of methanol solvent and stir to disperse. Then add 10 mmol of tris(2-aminoethyl)amine at 10°C and stir evenly. Heat to 25°C and react for 10 h. Then add 40 mmol of sodium borohydride and continue to react for 4 h. After the reaction is completed, remove formaldehyde, extract with chloroform, wash, dry and evaporate to obtain intermediate 1.
[0041] (2) Add 8 mmol of intermediate 1 to 150 mL of methanol solvent, stir and disperse, then add 24 mmol of 1,3-propanesulfonic acid lactone, stir evenly, heat to 60°C, react for 36 hours, then add 32 mmol of sodium carbonate, continue stirring and react for 2 hours. After the reaction is completed, filter, evaporate under reduced pressure, wash, and dry to obtain intermediate 2.
[0042] (3) Add 20 mmol of intermediate 2 into 150 mL of acetone solvent and stir to disperse. Then add 25 mmol of allyl bromide at 10°C and continue stirring to react for 10 h. After the reaction is completed, filter, wash and dry to obtain intermediate 3.
[0043] (4) 20 mmol of intermediate 3, 20 mmol of acrylic acid, 22 mmol of methacrylic acid, 1.2 mmol of sodium sulfite and 0.8 mmol of potassium persulfate were added to deionized water, stirred and dispersed, heated to 75°C, and reacted for 8 hours. After the reaction was completed, the mixture was cooled to 50°C, and a sodium hydroxide solution with a mass concentration of 30% was added to adjust the pH to 8 to obtain a modified sodium polyacrylate dispersant.
[0044] Comparative Example 1
[0045] (1) Add 35 mmol of p-formylbenzoic acid to 100 mL of methanol solvent and stir to disperse. Then add 10 mmol of tris(2-aminoethyl)amine at 10°C and stir evenly. Heat to 20°C and react for 12 h. Then add 40 mmol of sodium borohydride and continue to react for 4 h. After the reaction is completed, remove formaldehyde, extract with chloroform, wash, dry and evaporate to obtain intermediate 1.
[0046] (2) Add 20 mmol of intermediate 1 to 150 mL of acetone solvent, stir and disperse, then add 25 mmol of allyl bromide at 10°C, continue stirring and reacting for 5 h. After the reaction is completed, filter, wash and dry to obtain a tricarboxy quaternary ammonium salt intermediate, whose structural formula is: .
[0047] (3) 10 mmol of tricarboxyl quaternary ammonium salt intermediate, 20 mmol of acrylic acid, 20 mmol of methacrylic acid, 1.2 mmol of sodium sulfite and 0.8 mmol of potassium persulfate were added to deionized water, stirred and dispersed, heated to 60°C, reacted for 5 hours, and after the reaction was completed, cooled to 40°C, and a sodium hydroxide solution with a mass concentration of 30% was added thereto to adjust the pH to 9, thereby obtaining a modified sodium polyacrylate dispersant.
[0048] Comparative Example 2
[0049] The difference between this comparative example and Example 1 is that in step (4), intermediate 3 is not contained.
[0050] Take 0.5g of dispersant and add it to 50g of deionized water, stir and disperse, then add 100g of ceramic iron powder and stir evenly, use a viscometer to measure the viscosity of the slurry, and use the slurry viscosity to characterize the dispersing effect of the dispersant.
[0051] Table 1: Viscosity performance test results of various embodiments and comparative examples
[0052]
[0053] The smaller the viscosity, the better the dispersibility. As can be seen from the table, the viscosity of Examples 1-5 and Comparative Example 1 is smaller than that of Comparative Example 2, so the dispersibility is better. This is because Examples 1-5 and Comparative Example 1 contain more hydrophilic groups than Comparative Example 2, which can improve the dispersibility of the slurry. Therefore, the dispersant prepared by the present invention has better dispersibility.
[0054] 0.4 g of dispersant was added to 50 mL of deionized water, stirred and dispersed, and then 1 g of solid barium sulfate was added thereto. High shear dispersing emulsifier was used to emulsify at a speed of 10000 r / min for 10 min. The mixture was then transferred to a 100 mL measuring cylinder, deionized water was added thereto to make up to 100 mL, the mixture was inverted 5 times, and allowed to stand at 25 °C for 30 min. 90 mL of the upper suspension was removed with a pipette, and the remaining 10 mL of the suspension was placed in a 100 mL measuring cylinder with a mass of m 1 The measuring cylinder was rinsed with deionized water until all the sediment in the measuring cylinder was transferred to the culture dish, dried, and weighed m 2 , insoluble matter mass = m 2 -m 1 , suspension rate (%) = 10×(1.4-mass of insoluble matter) / (9×1.4).
[0055] Table 2: Suspension rate test results of various embodiments and comparative examples
[0056]
[0057] It can be seen from the table that the suspension rate of Examples 1-5 is higher than that of Comparative Examples 1-2. Therefore, the dispersant prepared by the present invention has a better dispersing effect.
[0058] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a modified sodium polyacrylate dispersant, characterized in that: The preparation method is as follows: (1) Add p-formylbenzoic acid to methanol solvent, stir and disperse, add tri(2-aminoethyl)amine at 5-10°C, stir evenly, heat to 20-35°C, react for 6-12h, add sodium borohydride, continue to react for 2-5h, remove formaldehyde after the reaction, extract with chloroform, wash, dry, and rotary evaporate to obtain intermediate 1, wherein the molar ratio of p-formylbenzoic acid, tri(2-aminoethyl)amine, and sodium borohydride is 3-4:1:3.5-4.5; (2) Add intermediate 1 to methanol solvent, stir and disperse, then add 1,3-propane sultone, stir evenly, heat to 60-70°C, react for 24-48h, then add sodium carbonate, wherein the molar ratio of intermediate 1, 1,3-propane sultone and sodium carbonate is 1:3-6:4-6, continue stirring and react for 2-4h, filter, distill under reduced pressure, wash and dry to obtain intermediate 2; (3) Add intermediate 2 to acetone solvent, stir and disperse, add allyl bromide at 5-10°C, wherein the molar ratio of intermediate 2 to allyl bromide is 1:1-1.5, continue stirring and reacting for 5-10 hours, and after the reaction is completed, filter, wash and dry to obtain intermediate 3; (4) Add intermediate 3, acrylic acid, methacrylic acid, sodium sulfite and potassium persulfate into deionized water, wherein the molar ratio of intermediate 3, acrylic acid and methacrylic acid is 0.5-1:1:1-1.3, stir and disperse, heat to 60-80°C, react for 5-10 hours, and after the reaction is completed, cool to 40-50°C, add sodium hydroxide solution to adjust the pH to 7-9, and obtain a modified sodium polyacrylate dispersant.
2. The method for preparing a modified sodium polyacrylate dispersant according to claim 1, wherein In the step (4), the molar ratio of sodium sulfite to potassium persulfate is 1.5:1; and the amount of potassium persulfate used is 15% of the mass of acrylic acid.
3. The preparation method of modified sodium polyacrylate dispersant according to claim 1, characterized in that, In the step (4), the mass concentration of the sodium hydroxide solution is 30%.