A hydrogen storage material and its preparation process and hydrogen nickel battery
By treating carbon nanotubes with specific chemicals and coating them with a composite alloy, the hydrogen storage material achieves improved hydrogen absorption and desorption kinetics, enhancing nickel-hydrogen battery performance.
Patent Information
- Application Number
- CN202410940386.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Current magnesium-based hydrogen storage materials have poor hydrogen absorption and desorption kinetics and high stability, leading to inadequate performance in nickel-hydrogen batteries, while existing combinations of hydrogen storage alloys and carbon nanotubes do not meet current usage needs.
A hydrogen storage material is prepared by treating carbon nanotubes with mixed acid, hydrogen peroxide, radio frequency glow discharge low-temperature plasma, and Ni(NO3)2 solution, and coating them with a composite alloy material containing Mg 1.8 Ag 0.2 Ni and amorphous FeTi 1.2, which enhances hydrogen storage capacity and kinetics.
The modified carbon nanotubes and composite alloy material improve hydrogen storage capacity, reduce desorption temperatures, and enhance the charge and discharge capacity and cycle stability of nickel-hydrogen batteries.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of hydrogen storage materials and nickel-hydrogen batteries, and in particular to a hydrogen storage material and a preparation process thereof, and a nickel-hydrogen battery. Background Art
[0002] Mg is abundant in nature, easy to prepare, low in cost, and can react with hydrogen to form MgH2, a hydride between ionic bonds and covalent bonds. Studies have found that the hydrogen absorption and desorption performance of pure Mg is not as good as that of magnesium-based alloys. Although magnesium-based alloys have large hydrogen storage capacity and low prices, compared with other materials, the hydrides of magnesium-based hydrogen storage materials are too stable, with poor hydrogen absorption and desorption kinetics and high hydrogen absorption and desorption temperatures. The current methods for improving the hydrogen absorption and desorption kinetics of magnesium-based alloys usually come at the expense of a decrease in hydrogen storage capacity per unit weight. The development of hydrogen storage alloys that have little or no effect on hydrogen storage capacity and can improve hydrogen absorption and desorption kinetics is still the current key research direction.
[0003] At present, environmentally friendly nickel-hydrogen batteries have gradually replaced nickel-cadmium batteries that seriously pollute the environment. However, the development of battery negative electrode materials with high capacity and high cycle stability, namely hydrogen storage materials, is still the key to restricting the application of nickel-hydrogen batteries. Metal hydrogen storage materials such as hydrogen storage alloys and non-metallic hydrogen storage materials such as carbon nanotubes have their own characteristics in hydrogen storage performance and have complementary advantages. Previously, researchers have used hydrogen storage alloys and carbon nanotubes together as hydrogen storage materials, and achieved improvements in hydrogen storage pressure and hydrogen absorption and desorption platforms, but they still cannot meet current usage needs. Improving the performance of carbon nanotubes is expected to improve the performance indicators of nickel-hydrogen batteries. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a hydrogen storage material and a preparation process thereof, and a nickel-hydrogen battery.
[0005] The object of the present invention can be achieved by the following technical scheme: a hydrogen storage material includes raw materials such as carbon nanotubes, mixed acid, hydrogen peroxide solution, deionized water, Ni(NO3)2 aqueous solution, composite alloy material and polyethyleneimine;
[0006] The mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1, the volume fraction of the hydrogen peroxide solution is 30%, and the molar concentration of the Ni(NO3)2 aqueous solution is 1 mol / L;
[0007] The hydrogen storage material is prepared by the following steps:
[0008] Step S1: putting carbon nanotubes into a high-temperature box-type resistance furnace, calcining at 650°C for 3h in an air atmosphere to obtain pretreated carbon nanotubes, then adding the pretreated carbon nanotubes to a mixed acid and soaking them for 36-40h, then filtering, washing the filter residue with deionized water until it is neutral, obtaining filter residue a, then soaking the filter residue a in a hydrogen peroxide solution at 55-65°C for 40min, filtering, washing the filter residue with deionized water until it is neutral, obtaining filter residue b, and then using radio frequency glow discharge low-temperature plasma to activate the filter residue b for 4 0min, to obtain the treated carbon nanotubes, then immerse the treated carbon nanotubes in an aqueous solution of Ni(NO3)2 for 12-14h, dry at 110°C for 24h, calcine at 450°C for 3h, and reduce at 550°C in a hydrogen atmosphere for 3h to obtain modified carbon nanotubes, the amount ratio of carbon nanotubes, mixed acid, hydrogen peroxide solution and Ni(NO3)2 aqueous solution is 0.01-0.015g: 200-250mL: 200-250mL: 200-250mL;
[0009] During the reaction of step S1, the carbon nanotubes are treated with mixed acid, hydrogen peroxide solution, radio frequency glow discharge low-temperature plasma and Ni(NO3)2 aqueous solution to obtain modified carbon nanotubes, and the hydrogen storage capacity of the modified carbon nanotubes is significantly increased.
[0010] Step S2: firstly adding polyethyleneimine to deionized water to obtain a polyethyleneimine aqueous solution, then placing the composite alloy material in the polyethyleneimine aqueous solution and stirring and ultrasonicating for 3-3.5 hours to obtain a mixture, filtering the mixture, washing with deionized water, and then adding the mixture to deionized water to obtain a polyethyleneimine-coated composite alloy material, wherein the amount ratio of the composite alloy material, polyethyleneimine and deionized water is 1g:1-1.5g:350-400mL;
[0011] During the reaction of step S2, polyethyleneimine is coated on the surface of the composite alloy material by stirring and ultrasonic action, so as to facilitate the coating of the modified carbon nanotubes on the surface in the next step.
[0012] Step S3: adding the modified carbon nanotubes to deionized water, stirring for 30-35 minutes to obtain a modified carbon nanotube aqueous solution, then adding the above-mentioned polyethyleneimine-coated composite alloy material to the modified carbon nanotube aqueous solution, stirring for 22-24 hours to mix, filtering, and then vacuum drying at 55-65° C. for 15-16 hours to obtain a hydrogen storage material, wherein the length of the modified carbon nanotubes is 3-5 μm, and the amount ratio of the modified carbon nanotubes, deionized water and the polyethyleneimine-coated composite alloy material is 0.004-0.01 g: 200 mL: 1-1.2 g;
[0013] During the reaction process of step S3, the modified carbon nanotubes are coated on the surface of the composite alloy material coated with polyethyleneimine to obtain a hydrogen storage material, which has the advantages of hydrogen storage performance of both the modified carbon nanotubes and the composite alloy material.
[0014] The composite alloy material is prepared by the following steps:
[0015] Step A1: Mg powder, Ag powder and Ni powder are added to an induction furnace which has been evacuated and filled with argon, and smelted at 1380-1420°C under the protection of argon atmosphere to obtain a molten liquid, and then the molten liquid is poured into a water-cooled ingot mold under the protection of argon atmosphere for casting to form an ingot; then the ingot is subjected to a homogenization treatment at 950-1000°C for 12-15 hours under the protection of argon, and then cooled to room temperature with the furnace to obtain Mg 1.8 Ag 0.2 Ni alloy; Fe powder and Ti powder are mixed, and ball milled for 10-12h under the conditions of argon atmosphere protection and ball-to-material ratio of 20:1 to obtain amorphous FeTi 1.2 ; The dosage ratio of Mg powder, Ag powder and Ni powder is 1.8g:0.2g:1g, the dosage ratio of Fe powder and Ti powder is 1g:1.2g, and the mass fraction of Mg powder, Ag powder, Ni powder, Fe powder and Ti powder is 99.9%;
[0016] During the reaction of step A1, metal Ag is introduced into the magnesium-nickel alloy to prevent evaporation and oxidation of Mg and reduce the stability of the hydride, so that the hydrogenation and dehydrogenation processes can occur at a lower temperature.
[0017] Step A2: Mg 1.8 Ag 0.2 Ni alloy and amorphous FeTi 1.2 Add it to a high-energy ball mill and carry out strong mechanical ball milling for 24-30 hours under the conditions of high-purity hydrogen atmosphere protection, ball-to-material ratio of 30-40:1, and rotation speed of 500-600r / min, then slowly add graphite and polyvinyl alcohol aqueous solution, stir for 1-1.5 hours under the condition of rotation speed of 300-400r / min, and dry to obtain a composite alloy material, Mg 1.8 Ag 0.2 Ni alloy, amorphous FeTi 1.2 , the dosage ratio of polyvinyl alcohol aqueous solution and graphite is 1g: 0.3-0.4g: 25-35mL: 0.03-0.04g, the graphite is coarse structure graphite, and the mass fraction of polyvinyl alcohol aqueous solution is 5%;
[0018] During the reaction of step A2, the amorphous FeTi 1.2 With Mg 1.8 Ag 0.2After mixing with Ni alloy, it is mixed with graphite and bonded with polyvinyl alcohol aqueous solution to obtain a composite alloy material. 1.2 Mg 1.8 Ag 0.2 The Ni alloy plays a catalytic role in the hydrogenation and dehydrogenation process. The coarse-structured graphite not only has a high hydrogen adsorption capacity and hydrogen storage density, but also has good electrical conductivity and thermal conductivity, which can quickly realize the hydrogen adsorption and release process, which is similar to the amorphous FeTi 1.2 Synergistically accelerate Mg 1.8 Ag 0.2 Hydrogenation and dehydrogenation processes of Ni alloys.
[0019] Beneficial effects of the present invention: The hydrogen storage material prepared by the present invention comprises raw materials such as carbon nanotubes, mixed acid, hydrogen peroxide solution, deionized water, aqueous solution of Ni(NO3)2, composite alloy material and polyethyleneimine. The composite alloy material introduces metal Ag, amorphous FeTi 1.2 The introduction of metal Ag into the magnesium-nickel alloy can prevent the evaporation and oxidation of Mg in the hydrogen storage material, while reducing the stability of the hydride, so that the hydrogenation and dehydrogenation processes can occur at a lower temperature; the amorphous FeTi 1.2 The catalytic effect improves the hydrogen absorption and desorption kinetics of hydrogen storage materials, increases hydrogen storage capacity and reduces the temperature of hydrogen absorption and desorption process. It also has excellent antioxidant effect. Coarse structure graphite not only has high hydrogen adsorption capacity and hydrogen storage density, but also has good electrical conductivity and thermal conductivity, which can quickly realize the hydrogen adsorption and release process. 1.2 Synergistically accelerate Mg 1.8 Ag 0.2 The hydride and dehydrogenation process of Ni alloy can improve the charge and discharge capacity and cycle performance of hydrogen nickel battery.
[0020] Modified carbon nanotubes are prepared by treating carbon nanotubes with mixed acid, hydrogen peroxide solution, radio frequency glow discharge low-temperature plasma and Ni(NO3)2 aqueous solution. The hydrogen storage capacity of the modified carbon nanotubes is significantly increased, thereby increasing the hydrogen storage capacity of the hydrogen storage material. After the modified carbon nanotubes are coated with the composite alloy material, the oxidation resistance and corrosion resistance of the alloy surface can be improved, and the life of the hydrogen storage material can be extended. The charge and discharge cycle stability and high-rate discharge performance of the hydrogen storage material are significantly improved, thereby improving the charge and discharge capacity and cycle stability of hydrogen nickel batteries and extending the battery life. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0022] A composite alloy material is prepared by the following steps:
[0023] Step A1: Mg powder, Ag powder and Ni powder are added to an induction furnace which has been evacuated and filled with argon gas, and smelted at 1380°C under the protection of argon atmosphere to obtain a molten liquid, and then the molten liquid is poured into a water-cooled ingot mold under the protection of argon atmosphere for casting to form an ingot; then the ingot is subjected to a homogenization treatment at 950°C for 12 hours under the protection of argon gas, and is cooled to room temperature with the furnace to obtain Mg 1.8 Ag 0.2 Ni alloy; Fe powder and Ti powder were mixed, and ball milled for 10 hours under argon atmosphere protection and a ball-to-material ratio of 20:1 to obtain amorphous FeTi 1.2 ; The dosage ratio of Mg powder, Ag powder and Ni powder is 1.8g:0.2g:1g, the dosage ratio of Fe powder and Ti powder is 1g:1.2g, and the mass fraction of Mg powder, Ag powder, Ni powder, Fe powder and Ti powder is 99.9%;
[0024] Step A2: Mg 1.8 Ag 0.2 Ni alloy and amorphous FeTi 1.2 The mixture was added to a high-energy ball mill and subjected to strong mechanical ball milling for 24 h under the conditions of high-purity hydrogen atmosphere protection, ball-to-material ratio of 30:1, and rotation speed of 500 r / min. Then, graphite and polyvinyl alcohol aqueous solution were added, stirred for 1 h and dried at a rotation speed of 300 r / min to obtain a composite alloy material, Mg 1.8 Ag 0.2 Ni alloy, amorphous FeTi 1.2 The dosage ratio of polyvinyl alcohol aqueous solution and graphite is 1g:0.3g:25mL:0.03g, the graphite is coarse structure graphite, and the mass fraction of polyvinyl alcohol aqueous solution is 5%. Example 2
[0025] A composite alloy material is prepared by the following steps:
[0026] Step A1: Mg powder, Ag powder and Ni powder are added to an induction furnace which has been evacuated and filled with argon, and smelted at 1400°C under the protection of argon atmosphere to obtain a molten liquid, and then the molten liquid is poured into a water-cooled ingot mold under the protection of argon atmosphere for casting to form an ingot; then the ingot is subjected to a homogenization treatment at 950°C for 14 hours under the protection of argon, and is cooled to room temperature with the furnace to obtain Mg 1.8 Ag 0.2 Ni alloy; Fe powder and Ti powder were mixed, and ball milled for 11 hours under argon atmosphere protection and a ball-to-material ratio of 20:1 to obtain amorphous FeTi 1.2 ; The dosage ratio of Mg powder, Ag powder and Ni powder is 1.8g:0.2g:1g, the dosage ratio of Fe powder and Ti powder is 1g:1.2g, and the mass fraction of Mg powder, Ag powder, Ni powder, Fe powder and Ti powder is 99.9%;
[0027] Step A2: Mg 1.8 Ag 0.2 Ni alloy and amorphous FeTi 1.2 The mixture was added to a high-energy ball mill and subjected to strong mechanical ball milling for 27 h under the conditions of high-purity hydrogen atmosphere protection, ball-to-material ratio of 35:1, and rotation speed of 550 r / min. Then, graphite and polyvinyl alcohol aqueous solution were added, and the mixture was stirred for 1.3 h and dried at a rotation speed of 300 r / min to obtain a composite alloy material, Mg 1.8 Ag 0.2 Ni alloy, amorphous FeTi 1.2 The dosage ratio of polyvinyl alcohol aqueous solution and graphite is 1g:0.35g:30mL:0.035g, the graphite is coarse structure graphite, and the mass fraction of polyvinyl alcohol aqueous solution is 5%. Example 3
[0028] A composite alloy material is prepared by the following steps:
[0029] Step A1: Mg powder, Ag powder and Ni powder are added to an induction furnace which has been evacuated and filled with argon, and smelted at 1420°C under the protection of argon atmosphere to obtain a molten liquid, and then the molten liquid is poured into a water-cooled ingot mold under the protection of argon atmosphere for casting to form an ingot; then the ingot is subjected to a homogenization treatment at 1000°C for 15 hours under the protection of argon, and is cooled to room temperature with the furnace to obtain Mg 1.8 Ag 0.2 Ni alloy; Fe powder and Ti powder were mixed, and ball milled for 12 hours under argon atmosphere protection and a ball-to-material ratio of 20:1 to obtain amorphous FeTi 1.2; The dosage ratio of Mg powder, Ag powder and Ni powder is 1.8g:0.2g:1g, the dosage ratio of Fe powder and Ti powder is 1g:1.2g, and the mass fraction of Mg powder, Ag powder, Ni powder, Fe powder and Ti powder is 99.9%;
[0030] Step A2: Mg 1.8 Ag 0.2 Ni alloy and amorphous FeTi 1.2 Add it to a high-energy ball mill and carry out strong mechanical ball milling for 30 hours under the conditions of high-purity hydrogen atmosphere protection, ball-to-material ratio of 40:1, and rotation speed of 500-600r / min. Then add graphite and polyvinyl alcohol aqueous solution, stir for 1.5 hours and dry at a rotation speed of 400r / min to obtain a composite alloy material, Mg 1.8 Ag 0.2 Ni alloy, amorphous FeTi 1.2 The dosage ratio of polyvinyl alcohol aqueous solution and graphite is 1g:0.4g:35mL:0.04g, the graphite is coarse structure graphite, and the mass fraction of polyvinyl alcohol aqueous solution is 5%. Example 4
[0031] A hydrogen storage material, comprising raw materials of carbon nanotubes, mixed acid, hydrogen peroxide solution, deionized water, Ni(NO3)2 aqueous solution, composite alloy material and polyethyleneimine; the mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1, the volume fraction of the hydrogen peroxide solution is 30%, and the molar concentration of the Ni(NO3)2 aqueous solution is 1 mol / L;
[0032] The hydrogen storage material is prepared by the following steps:
[0033] Step S1: putting carbon nanotubes into a high-temperature box-type resistance furnace, calcining at 650°C for 3h in an air atmosphere to obtain pretreated carbon nanotubes, then adding the pretreated carbon nanotubes to a mixed acid and soaking them for 36h, then filtering, washing the filter residue with deionized water until neutral, obtaining filter residue a, then soaking the filter residue a in a hydrogen peroxide solution at 55°C for 40min, filtering, washing the filter residue with deionized water until neutral, obtaining filter residue b, and then activating the filter residue b with radio frequency glow discharge low-temperature plasma for 40min to obtain treated carbon nanotubes, then immersing the treated carbon nanotubes in a Ni(NO3)2 aqueous solution for 12h, drying at 110°C for 24h, calcining at 450°C for 3h, and reducing at 550°C in a hydrogen atmosphere for 3h to obtain modified carbon nanotubes, the amount ratio of carbon nanotubes, mixed acid, hydrogen peroxide solution and Ni(NO3)2 aqueous solution is 0.01g:200mL:200mL:200mL;
[0034] Step S2: firstly adding polyethyleneimine to deionized water to obtain a polyethyleneimine aqueous solution, then placing the composite alloy material obtained in Example 1 in the polyethyleneimine aqueous solution and stirring and ultrasonically stirring for 3 hours to obtain a mixture, filtering the mixture, washing with deionized water, and then adding the mixture to deionized water to obtain a polyethyleneimine-coated composite alloy material, wherein the amount ratio of the composite alloy material, polyethyleneimine and deionized water is 1g:1g:350mL;
[0035] Step S3: Add the modified carbon nanotubes to deionized water and stir for 30 minutes to obtain a modified carbon nanotube aqueous solution, then add the above-mentioned polyethyleneimine-coated composite alloy material to the modified carbon nanotube aqueous solution, stir for 22 hours to mix, filter, and then vacuum dry at 55°C for 15 hours to obtain a hydrogen storage material. The length of the modified carbon nanotubes is 3 μm, and the amount ratio of the modified carbon nanotubes, deionized water and polyethyleneimine-coated composite alloy material is 0.004g:200mL:1g. Example 5
[0036] A hydrogen storage material, comprising raw materials of carbon nanotubes, mixed acid, hydrogen peroxide solution, deionized water, Ni(NO3)2 aqueous solution, composite alloy material and polyethyleneimine; the mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1, the volume fraction of the hydrogen peroxide solution is 30%, and the molar concentration of the Ni(NO3)2 aqueous solution is 1 mol / L;
[0037] The hydrogen storage material is prepared by the following steps:
[0038] Step S1: putting the carbon nanotubes into a high-temperature box-type resistance furnace, calcining them at 650°C for 3h in an air atmosphere to obtain pretreated carbon nanotubes, then adding the pretreated carbon nanotubes to a mixed acid and soaking them for 38h, then filtering, washing the filter residue with deionized water until it is neutral, obtaining filter residue a, then soaking the filter residue a in a hydrogen peroxide solution at 60°C for 40min, filtering, washing the filter residue with deionized water until it is neutral, obtaining filter residue b, and then using radio frequency glow discharge low-temperature plasma to treat the filter residue. The slag b was activated for 40 minutes to obtain the treated carbon nanotubes, and then the treated carbon nanotubes were immersed in an aqueous solution of Ni(NO3)2 for 13 hours, dried at 110°C for 24 hours, calcined at 450°C for 3 hours, and reduced at 550°C in a hydrogen atmosphere for 3 hours to obtain modified carbon nanotubes. The amount ratio of carbon nanotubes, mixed acid, hydrogen peroxide solution and Ni(NO3)2 aqueous solution was 0.012 g: 225 mL: 225 mL: 225 mL;
[0039] Step S2: firstly adding polyethyleneimine to deionized water to obtain a polyethyleneimine aqueous solution, then placing the composite alloy material obtained in Example 2 in the polyethyleneimine aqueous solution and stirring and ultrasonicating for 3.5 hours to obtain a mixture, filtering the mixture, washing with deionized water, and then adding the mixture to deionized water to obtain a polyethyleneimine-coated composite alloy material, wherein the amount ratio of the composite alloy material, polyethyleneimine and deionized water is 1 g:1.2 g:370 mL;
[0040] Step S3: Add the modified carbon nanotubes to deionized water and stir for 32 minutes to obtain a modified carbon nanotube aqueous solution, then add the above-mentioned polyethyleneimine-coated composite alloy material to the modified carbon nanotube aqueous solution, stir for 23 hours to mix, filter, and then vacuum dry at 60°C for 15 hours to obtain a hydrogen storage material. The length of the modified carbon nanotubes is 4 μm, and the amount ratio of the modified carbon nanotubes, deionized water and polyethyleneimine-coated composite alloy material is 0.007g:200mL:1.1g. Example 6
[0041] A hydrogen storage material, comprising raw materials of carbon nanotubes, mixed acid, hydrogen peroxide solution, deionized water, Ni(NO3)2 aqueous solution, composite alloy material and polyethyleneimine; the mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1, the volume fraction of the hydrogen peroxide solution is 30%, and the molar concentration of the Ni(NO3)2 aqueous solution is 1 mol / L;
[0042] The hydrogen storage material is prepared by the following steps:
[0043] Step S1: putting the carbon nanotubes into a high-temperature box-type resistance furnace, calcining them at 650°C for 3h in an air atmosphere to obtain pretreated carbon nanotubes, then adding the pretreated carbon nanotubes to a mixed acid and soaking them for 40h, then filtering, washing the filter residue with deionized water until it is neutral, obtaining filter residue a, then soaking the filter residue a in a hydrogen peroxide solution at 65°C for 40min, filtering, washing the filter residue with deionized water until it is neutral, obtaining filter residue b, and then using radio frequency glow discharge low-temperature plasma to treat the filter residue. The slag b was activated for 40 minutes to obtain the treated carbon nanotubes, and then the treated carbon nanotubes were immersed in a Ni(NO3)2 aqueous solution for 14 hours, dried at 110°C for 24 hours, calcined at 450°C for 3 hours, and reduced at 550°C in a hydrogen atmosphere for 3 hours to obtain modified carbon nanotubes. The amount ratio of carbon nanotubes, mixed acid, hydrogen peroxide solution and Ni(NO3)2 aqueous solution was 0.015 g: 250 mL: 250 mL: 250 mL;
[0044] Step S2: firstly adding polyethyleneimine to deionized water to obtain a polyethyleneimine aqueous solution, then placing the composite alloy material obtained in Example 3 in the polyethyleneimine aqueous solution and stirring and ultrasonically stirring for 3.5 hours to obtain a mixture, filtering the mixture, washing with deionized water, and then adding the mixture to deionized water to obtain a polyethyleneimine-coated composite alloy material, wherein the amount ratio of the composite alloy material, polyethyleneimine and deionized water is 1g:1.5g:400mL;
[0045] Step S3: Add the modified carbon nanotubes to deionized water and stir for 35 minutes to obtain a modified carbon nanotube aqueous solution, then add the above-mentioned polyethyleneimine-coated composite alloy material to the modified carbon nanotube aqueous solution, stir for 24 hours to mix, filter, and then vacuum dry at 65°C for 16 hours to obtain a hydrogen storage material. The length of the modified carbon nanotubes is 5 μm, and the amount ratio of the modified carbon nanotubes, deionized water and the polyethyleneimine-coated composite alloy material is 0.01g:200mL:1.2g. Example 7
[0046] A nickel-hydrogen battery comprises a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, a diaphragm and an electrolyte layer in contact with the positive electrode and the negative electrode; the positive electrode active material is Ni(OH)2, the negative electrode active material is the hydrogen storage material obtained in Example 4, the diaphragm is an aqueous battery diaphragm, and the electrolyte layer is a 6 mol / L potassium hydroxide solution.
[0047] The nickel-hydrogen battery is prepared by the following steps: directly assembling a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, a separator and an electrolyte layer in contact with the positive electrode and the negative electrode into a full battery, thus obtaining a nickel-hydrogen battery. Example 8
[0048] A nickel-hydrogen battery comprises a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, a diaphragm and an electrolyte layer in contact with the positive electrode and the negative electrode; the positive electrode active material is Ni(OH)2, the negative electrode active material is the hydrogen storage material obtained in Example 5, the diaphragm is an aqueous battery diaphragm, and the electrolyte layer is a 6 mol / L potassium hydroxide solution.
[0049] The nickel-hydrogen battery is prepared by the following steps: directly assembling a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, a separator and an electrolyte layer in contact with the positive electrode and the negative electrode into a full battery, thus obtaining a nickel-hydrogen battery. Example 9
[0050] A nickel-hydrogen battery comprises a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, a diaphragm and an electrolyte layer in contact with the positive electrode and the negative electrode; the positive electrode active material is Ni(OH)2, the negative electrode active material is the hydrogen storage material obtained in Example 6, the diaphragm is an aqueous battery diaphragm, and the electrolyte layer is a 6 mol / L potassium hydroxide solution.
[0051] The nickel-hydrogen battery is prepared by the following steps: directly assembling a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, a separator and an electrolyte layer in contact with the positive electrode and the negative electrode into a full battery, thus obtaining a nickel-hydrogen battery.
[0052] Comparative Example 1:
[0053] This comparative example is a commercially available nickel-hydrogen battery.
[0054] Comparative Example 2:
[0055] Compared with Example 9, the modified carbon nanotubes used in the preparation process of the hydrogen storage material obtained in Example 6 were replaced with carbon nanotubes, and the rest was exactly the same as in Example 9 to prepare a nickel-hydrogen battery.
[0056] Comparative Example 3:
[0057] Compared with Example 9, the composite alloy material used in the preparation process of the hydrogen storage material obtained in Example 6 does not introduce the amorphous phase of FeTi 1.2 , the rest is exactly the same as in Example 9 to obtain a nickel-hydrogen battery.
[0058] The hydrogen storage material and nickel-hydrogen battery prepared by the present invention are further tested for their effects, and the test results are as follows.
[0059] In order to test the performance of the hydrogen storage material and nickel-hydrogen battery prepared by the present invention, measurements were performed according to GB / T22084.2-2008 and related methods. The results are shown in Table 1.
[0060] Table 1:
[0061] ;
[0062] According to the data in Table 1, compared with Example 1, it can be seen that the hydrogen storage material prepared in the present invention is applied to the nickel-hydrogen battery, which makes the nickel-hydrogen battery have the advantages of high charge and discharge capacity, long life and good cycle stability, compared with the commercially available nickel-hydrogen battery; compared with Example 2, it can be seen that without modifying the carbon nanotubes, the hydrogen storage capacity of the hydrogen storage material is significantly reduced, which reduces the charge and discharge capacity of the nickel-hydrogen battery; compared with Example 3, it can be seen that the FeTi composite alloy material without introducing the amorphous phase is not 1.2, the hydrogen absorption and desorption kinetics of the composite alloy material decreases, which in turn affects the hydrogen storage performance of the hydrogen storage material, and is therefore not conducive to the cycle performance and charge and discharge capacity retention rate of hydrogen nickel batteries.
[0063] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A hydrogen storage material, characterized in that: The raw materials include carbon nanotubes, mixed acid, hydrogen peroxide solution, deionized water, Ni(NO3)2 aqueous solution, composite alloy material and polyethyleneimine; the mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1, the volume fraction of the hydrogen peroxide solution is 30%, and the molar concentration of the Ni(NO3)2 aqueous solution is 1 mol / L; The composite alloy material is prepared by the following steps: Step A1: Mg powder, Ag powder and Ni powder are added to an induction furnace which has been evacuated and filled with argon, and smelted at 1380-1420°C under the protection of argon atmosphere to obtain a molten liquid, and then the molten liquid is poured into a water-cooled ingot mold under the protection of argon atmosphere for casting to form an ingot; then the ingot is subjected to a homogenization treatment at 950-1000°C for 12-15 hours under the protection of argon, and then cooled to room temperature with the furnace to obtain Mg 1.8 Ag 0.2 Ni alloy; Fe powder and Ti powder are mixed, and ball milled for 10-12h under the conditions of argon atmosphere protection and ball-to-material ratio of 20:1 to obtain amorphous FeTi 1.2 ; Step A2: Mg 1.8 Ag 0.2 Ni alloy and amorphous FeTi 1.2 Add into high-energy ball mill and carry out strong mechanical ball milling for 24-30 hours under the conditions of high-purity hydrogen atmosphere protection, ball-to-material ratio of 30-40:1, and rotation speed of 500-600r / min, then slowly add graphite and polyvinyl alcohol aqueous solution, stir for 1-1.5 hours at a rotation speed of 300-400r / min, and dry to obtain the composite alloy material.
2. A hydrogen storage material according to claim 1, characterized in that: In step A1, the usage ratio of Mg powder, Ag powder and Ni powder is 1.8g:0.2g:1g, the usage ratio of Fe powder and Ti powder is 1g:1.2g, and the total mass fraction of Mg powder, Ag powder, Ni powder, Fe powder and Ti powder is 99.9%.
3. A hydrogen storage material according to claim 1, characterized in that: In step A2, Mg 1.8 Ag 0.2 Ni alloy, amorphous FeTi 1.2 , the dosage ratio of polyvinyl alcohol aqueous solution and graphite is 1g:0.3-0.4g:25-35mL:0.03-0.04g, the graphite is coarse structure graphite, and the mass fraction of polyvinyl alcohol aqueous solution is 5%.
4. The process for preparing a hydrogen storage material according to claim 1, characterized in that: Prepared by the following steps: Step S1: putting carbon nanotubes into a high-temperature box-type resistance furnace, calcining at 650°C for 3h in an air atmosphere to obtain pretreated carbon nanotubes, then adding the pretreated carbon nanotubes to a mixed acid and soaking them for 36-40h, then filtering, washing the filter residue with deionized water until neutral, obtaining filter residue a, then soaking the filter residue a in a hydrogen peroxide solution at 55-65°C for 40min, filtering, washing the filter residue with deionized water until neutral, obtaining filter residue b, then using radio frequency glow discharge low-temperature plasma to activate the filter residue b for 40min to obtain treated carbon nanotubes, then immersing the treated carbon nanotubes in an aqueous solution of Ni(NO3)2 for 12-14h, drying at 110°C for 24h, calcining at 450°C for 3h, and reducing at 550°C in a hydrogen atmosphere for 3h to obtain modified carbon nanotubes; Step S2: firstly adding polyethyleneimine to deionized water to obtain a polyethyleneimine aqueous solution, then placing the composite alloy material in the polyethyleneimine aqueous solution and stirring and ultrasonically agitating for 3-3.5 hours to obtain a mixture, filtering the mixture, washing with deionized water, and then adding the mixture to deionized water to obtain a polyethyleneimine-coated composite alloy material; Step S3: Add the modified carbon nanotubes to deionized water and stir for 30-35 minutes to obtain a modified carbon nanotube aqueous solution, then add the above-mentioned polyethyleneimine-coated composite alloy material to the modified carbon nanotube aqueous solution, stir for 22-24 hours, filter, and then vacuum dry at 55-65°C for 15-16 hours to obtain a hydrogen storage material.
5. A process for preparing a hydrogen storage material according to claim 4, characterized in that: In step S1, the usage ratio of carbon nanotubes, mixed acid, hydrogen peroxide solution and Ni(NO3)2 aqueous solution is 0.01-0.015 g: 200-250 mL: 200-250 mL: 200-250 mL.
6. A process for preparing a hydrogen storage material according to claim 4, characterized in that: In step S2, the usage ratio of the composite alloy material, polyethyleneimine and deionized water is 1 g: 1-1.5 g: 350-400 mL.
7. A process for preparing a hydrogen storage material according to claim 4, characterized in that: In step S3, the length of the modified carbon nanotubes is 3-5 μm, and the usage ratio of the modified carbon nanotubes, deionized water and the composite alloy material coated with polyethyleneimine is 0.004-0.01 g: 200 mL: 1-1.2 g.
8. A nickel-hydrogen battery, characterized in that: Comprising the hydrogen storage material as described in any one of claims 1 to 3 above.
9. A nickel-hydrogen battery according to claim 8, characterized in that: It comprises a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, a separator and an electrolyte layer in contact with the positive electrode and the negative electrode; the positive electrode active material is Ni(OH)2, the negative electrode active material is a hydrogen storage material, the separator is an aqueous battery separator, and the electrolyte layer is a 6 mol / L potassium hydroxide solution; The preparation process of the nickel-hydrogen battery is as follows: a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, a separator and an electrolyte layer in contact with the positive electrode and the negative electrode are directly assembled into a full battery to obtain a nickel-hydrogen battery.
Citation Information
Patent Citations
Novel organic coated core-shell nano composite hydrogen storage material and preparation method thereof
CN108193107A
Coating method of rare earth hydrogen storage alloy powder for negative electrode for carbon nanotube coated nickel-hydrogen battery