Two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid, their preparation methods, and their application in the degradation of mustard gas.

By preparing two-dimensional sub-nanomaterials of titanium dioxide and phosphomolybdic acid, the problems of slow CEES degradation rate and poor catalyst stability were solved, achieving efficient CEES oxidative degradation under extreme conditions, which is suitable for personal protective equipment.

CN118527160BActive Publication Date: 2026-11-10SOUTHWEST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410595396.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-14
Publication Date
2026-11-10
Estimated Expiration
2044-05-14

AI Technical Summary

Technical Problem

Existing CEES degradation methods suffer from problems such as slow rate, numerous byproducts, and poor catalyst stability, making them difficult to apply effectively, especially under extreme conditions.

Method used

Two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid were used. Titanium dioxide was assembled on the surface of oriented phosphomolybdic acid clusters to form core-shell structured two-dimensional sub-nanobelts. These were then combined with PHP microspheres loaded onto cotton fabric and water-activated reactions were used to catalytically degrade CEES.

Benefits of technology

It achieves rapid and efficient oxidative degradation of CEES under extreme conditions, producing non-toxic products. The catalyst has high activity and stability, making it suitable for personal protective equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118527160B_ABST
    Figure CN118527160B_ABST
Patent Text Reader

Abstract

This invention relates to two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid, their preparation methods, and their application in the degradation of mustard gas, belonging to the field of nanomaterial preparation technology. The material disclosed in this invention has a two-dimensional ribbon structure. With the assistance of long-chain ligands (oleylamine and octadecene), polyoxometalate clusters of phosphomolybdic acid are oriented, and titanium dioxide is distributed on the surface of the phosphomolybdic acid clusters, collectively assembling into two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid. Given that the thickness of the two-dimensional sub-nanomaterial is only at the sub-nanometer level, the active sites can be fully exposed, thus exhibiting extremely high catalytic activity. Furthermore, the preparation method of the two-dimensional sub-nanomaterials of this invention mainly involves adding phosphomolybdic acid, titanium sulfate, octadecene, and oleylamine separately to water, reacting them in a high-pressure reactor, and then repeatedly washing with cyclohexane and ethanol before centrifugation. The preparation method of this invention has the advantages of simple reaction operation, wide availability of raw materials, and the ability to produce in batches.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nanomaterial preparation technology, and relates to two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid, their preparation methods, and their application in the degradation of mustard gas. Background Technology

[0002] Currently, various degradation methods for CEES have been developed, including hydrolysis, photodegradation, sulfide reduction, and oxidative degradation. Hydrolysis generally suffers from slow rates and numerous byproducts. Photodegradation primarily utilizes visible light to generate electron-hole pairs in semiconductor materials, thus producing oxidation capabilities; however, it requires a light source such as visible light and may fail under extreme conditions. Sulfide reduction readily produces hydrogen sulfide gas, which is highly toxic. Therefore, oxidative degradation offers the advantage of producing a single, non-toxic product, potentially making it more advantageous in some extreme situations. Furthermore, the selection and performance of the catalyst are crucial factors. Given the need for rapid and efficient detoxification under extreme conditions, researchers have developed various types of catalysts, including metal-organic frameworks, inorganic oxides, polymers, and alkali metals. While these catalysts have made progress in some areas, many problems remain, including poor stability, demanding catalytic conditions, and slow catalytic rates.

[0003] Subnanomaterials are materials smaller than 1 nm in at least one dimension; "subnano" is a concept relative to the nanoscale. Typically, the properties of nanomaterials depend on their size; when their size is smaller than 1 nm, they exhibit unique physical, chemical, or biological properties. Similar to nanomaterials, subnanomaterials can be classified into zero-dimensional, one-dimensional, two-dimensional, and three-dimensional subnanomaterials. Because two-dimensional subnanomaterials are less than 1 nm thick, they possess unique structures and properties, potentially exhibiting superior performance in catalysis. These materials can provide larger surface areas, higher active site densities, and better electrical or optical properties, thereby improving catalytic effects. Research on subnanomaterials not only contributes to the development of catalysis science but may also bring innovations in fields such as energy, environment, and medicine.

[0004] Therefore, using two-dimensional sub-nanomaterials to catalyze the oxidative degradation of CEES is a research direction with great practical significance. Summary of the Invention

[0005] In view of this, one objective of the present invention is to provide two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid; another objective of the present invention is to provide a method for preparing two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid; and a third objective of the present invention is to provide the application of two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid in the degradation of mustard gas.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] 1. A two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid, wherein the two-dimensional sub-nanomaterial is a two-dimensional sub-nanobelt material assembled by distributing titanium dioxide on the surface of oriented phosphomolybdic acid clusters.

[0008] Preferably, the mass ratio of titanium dioxide to phosphomolybdic acid in the two-dimensional sub-nanomaterial is 1:5.

[0009] 2. The preparation method of the above-mentioned two-dimensional sub-nanomaterials, wherein the preparation method includes the following steps:

[0010] (1) Add titanium sulfate to the aqueous solution of phosphomolybdic acid, stir and mix evenly, then add octadecene, continue stirring and mixing evenly, add oleylamine, and react in a high-pressure reactor.

[0011] (2) After the reaction is complete, wash with cyclohexane and ethanol respectively and centrifuge. Repeat the operation to obtain two-dimensional sub-nano materials based on titanium dioxide and phosphomolybdic acid.

[0012] Preferably, in step (1), the concentration of phosphomolybdic acid in the aqueous solution of phosphomolybdic acid is 0.01 g / mL.

[0013] Preferably, in step (1), the mass-volume ratio of phosphomolybdic acid, titanium sulfate, octadecene and oleylamine in the aqueous solution of phosphomolybdic acid is 0.2:0.04:12.5:7.5, g:g:mL:mL.

[0014] Preferably, in step (1), the stirring time is 5 to 20 minutes.

[0015] Preferably, in step (1), the reaction temperature is 180°C and the time is 6 hours, and the pressure in the high-pressure reactor is 50-200 MPa.

[0016] 3. Application of the above-mentioned two-dimensional sub-nano materials in the catalytic degradation of mustard gas.

[0017] 4. A method for catalytic degradation of mustard gas, the method comprising: preparing a solution of PHP microspheres and the above-mentioned two-dimensional sub-nano materials, immersing the substrate in the solution for loading and drying, adding mustard gas, and catalytically degrading mustard gas by activating the reaction with water;

[0018] The PHP microspheres were prepared by the following method: H2O2 and polyvinylpyrrolidone (PVP) were mixed and stirred to obtain a gel-like product, which was then freeze-dried and ground to obtain powdered PHP microspheres.

[0019] Preferably, the mass ratio of the PHP microspheres to the two-dimensional sub-nanomaterial is not less than 1:1, and the volume ratio of the two-dimensional sub-nanomaterial to mustard gas is not less than 10:1.

[0020] The substrate is cotton fabric or synthetic fiber;

[0021] The mass ratio of H2O2 to polyvinylpyrrolidone (PVP) is 1.5:1.

[0022] The beneficial effects of this invention are as follows:

[0023] 1. This invention discloses a two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid. The material has a core-shell structure, in which titanium dioxide is the core and phosphomolybdic acid is the shell. With the assistance of long-chain ligands (oleylamine and octadecene), polyoxometalate clusters (phosphomolybdic acid clusters) are oriented and arranged, and titanium dioxide is distributed on the surface. Together they assemble into metal oxide / polyoxometalate cluster sub-nanobelts, which is the two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid. Since the thickness of the two-dimensional sub-nanomaterial is only at the sub-nanometer level, it can completely expose the active sites, thus exhibiting great catalytic activity.

[0024] 2. This invention discloses a method for preparing two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid. The method mainly involves adding phosphomolybdic acid, titanium sulfate, octadecene, and oleylamine to water, reacting them in a high-pressure reactor, and then repeatedly washing with cyclohexane and ethanol before centrifugation. The preparation method of this invention has the advantages of simple reaction operation, wide availability of raw materials, and the ability to produce in batches.

[0025] 3. This invention also discloses a method for catalytic degradation of mustard gas, which mainly involves loading PHP microspheres and two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid onto cotton fabric, adding mustard gas (taking 2-chloroethyl ethyl sulfoxide (CEESO) as an example), and then oxidizing the mustard gas (taking 2-chloroethyl ethyl sulfoxide (CEESO) as an example) into a non-toxic product through an activation reaction with water, thereby achieving the purpose of catalytic degradation of mustard gas.

[0026] Other advantages, objectives, and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination, or may be learned from practice of the invention. The objectives and other advantages of the invention can be realized and obtained through the following description. Attached Figure Description

[0027] To make the objectives, technical solutions, and advantages of the present invention clearer, the preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings, wherein:

[0028] Figure 1 The flowchart (a) shows the preparation process of two-dimensional sub-nanomaterials (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid, and the schematic diagram (b) shows the catalytic degradation of CEES.

[0029] Figure 2 The transmission electron microscope (TEM) (a) and atomic force microscope (AFM) (b) characterization results of the materials prepared in Example 1;

[0030] Figure 3 The image shows a transmission electron microscope (TEM) image of the material prepared in Example 1.

[0031] Figure 4 The image shows the X-ray photoelectron spectroscopy (XPS) spectrum of the material prepared in Example 1;

[0032] Figure 5 The UV-Vis absorption spectra of the materials (TiO2 / PMASNBs) and PMA prepared in Example 1 are shown.

[0033] Figure 6 The results of infrared vibrational spectral analysis of the materials (TiO2 / PMASNBs), PMA, and TiO2 prepared in Example 1 are shown.

[0034] Figure 7 XPS analysis results of the two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid prepared in Example 1 (a), XPS analysis results of the products after the catalytic degradation reaction in Example 2 (b), Electron paramagnetic resonance (ESR) analysis results of the two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid prepared in Example 1 (c), Fluorescence decay of DMA molecules in the presence of H2O2 only (inset plot shows the change of DMA molecule fluorescence over time in the presence of H2O2 only) (d), Fluorescence decay of DMA molecules in the presence of H2O2 and TiO2 / PMA sub-nanobelts (inset plot shows DMA fluorescence decay over time). The fluorescence of molecule A changes over time in the presence of H2O2 and TiO2 / PMA subnanobelts (e), the electron paramagnetic resonance (ESR) analysis results of the products after the catalytic degradation reaction in Example 2 (f), the change in UV absorption of nitrotetrazole blue chloride (NBT) in the presence of only H2O2 (g), the change in UV absorption of nitrotetrazole blue chloride (NBT) in the presence of both H2O2 and TiO2 / PMA subnanobelts (h), and the electron paramagnetic resonance (ESR) analysis results of the catalytic material (TiO2 / PMA subnanobelts) in the catalytic degradation reaction process in Example 2 (i).

[0035] Figure 8In the figure, a represents the proposed oxidation pathway of CEES using TiO2 / PMA subnanobelts; b represents the conversion of CEES within 5 minutes under room temperature and natural light; c represents the effect of the concentrations of TiO2, PMA clusters, and TiO2 / PMA subnanobelts on the reaction progress of CEES catalytic oxidation; d represents the conversion rate of TiO2 / PMA subnanobelts under xenon lamp, natural light, and darkness; e represents the conversion rate of CEES after 8 cycles of continuous addition under the action of catalysts (two-dimensional subnanomaterials based on titanium dioxide and phosphomolybdic acid (TiO2 / PMA subnanobelts) and PHP microspheres); and f represents the infrared spectra of two-dimensional subnanomaterials based on titanium dioxide and phosphomolybdic acid (TiO2 / PMA subnanobelts) after 1 and 8 cycles of catalytic degradation of CEES.

[0036] Figure 9 Image a shows the formation of PHP microspheres using polyvinylpyrrolidone (PVP) crosslinking oxidant H2O2, the reverse reaction of PHP microspheres in the presence of water, and the application of PHP microspheres and the two-dimensional sub-nanomaterial (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid prepared in Example 1 in a gas mask. Image b shows the UV-Vis absorption spectra of PHP, PVP, and the mixed material (PHP and TiO2 / PMA sub-nanobelt mixture, i.e., PHP-SNBs). Image c shows the infrared absorption spectra of PHP, PVP, and the mixed material (PHP and TiO2 / PMA sub-nanobelt mixture, i.e., TiO2 / PMA / PHP SNBs). Image d shows photos of the filter cotton in the gas mask before and after catalyst loading. Images e and f are SEM images (scale 200 μm) of smooth cotton fabric (without catalyst loading) and cotton fabric loaded with catalyst, respectively. Image g shows the conversion rate of CEES of cotton fabric loaded with TiO2 / PMA sub-nanobelts after storage at room temperature for 0, 7, 14, and 21 days. Detailed Implementation

[0037] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments are only schematic representations of the basic concept of the present invention. Unless otherwise specified, the following embodiments and features can be combined with each other.

[0038] Example 1

[0039] The preparation process of two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid is as follows: Figure 1As shown in Figure a, the specific preparation method is as follows:

[0040] (1) Weigh 0.2g of phosphomolybdic acid and add it to 20mL of deionized water. After dissolving it completely, add 0.04g of titanium sulfate and stir for 10min to mix thoroughly. Then add 12.5mL of octadecene and continue stirring for 10min to mix it evenly. Finally, add 7.5mL of oleylamine and react in a high-pressure reactor at 180℃ and 100MPa for 6h.

[0041] (2) After the reaction was completed, the materials were washed with cyclohexane and ethanol, centrifuged and filtered. The process was repeated three times to obtain two-dimensional sub-nano materials (TiO2 / PMA sub-nano belts) based on titanium dioxide and phosphomolybdic acid.

[0042] Example 2

[0043] A method for catalytic degradation of 2-chloroethyl ethyl sulfide (CEES) specifically includes the following steps:

[0044] (1) Preparation of powdered PHP microspheres: H2O2 and polyvinylpyrrolidone (PVP) were mixed at a mass ratio of 1.5:1 and stirred for 24 h to obtain a gel-like product. After freeze-drying for 24 h, a solid was obtained and then ground to obtain powdered PHP microspheres.

[0045] (2) Catalytic degradation of 2-chloroethyl ethyl sulfide (CEES): 0.500g of the powdered PHP microspheres prepared above and 0.500g of the two-dimensional sub-nanomaterials (TiO2 / PMA sub-nanobelts, TiO2 / PMASNBs) based on titanium dioxide and phosphomolybdic acid prepared in Example 1 were mixed and loaded onto cotton fabric (the cotton fabric was immersed in the mixture of PHP microspheres and TiO2 / PMA sub-nanobelts). 10μL of mustard gas simulant (2-chloroethyl ethyl sulfide (CEES)) was dropped onto the cotton fabric loaded with the catalyst, and the reaction was activated by 100μL of water, which oxidized 2-chloroethyl ethyl sulfide (CEES) to 2-chloroethyl ethyl sulfoxide (CEESO).

[0046] Performance testing

[0047] 1. Preparation process and degradation principle of two-dimensional sub-nanomaterials (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid

[0048] The above schematic diagrams of the two-dimensional sub-nanomaterials (TiO2 / PMA sub-nanobelts, TiO2 / PMASNBs) based on titanium dioxide and phosphomolybdic acid and the PHP microspheres catalytic degradation of 2-chloroethyl ethyl sulfide (CEES) are shown in the figure. Figure 1As shown in Figure b, PHP functions similarly to hydrogen peroxide. To facilitate storage, PVP is used as a cross-linking agent to first form PHP microspheres, which can then undergo a reverse reaction under the influence of water to regenerate hydrogen peroxide. From Figure 1 As can be seen from Figure b, TiO2 / PMA sub-nanobelts catalyze the generation of ROS from hydrogen peroxide, thereby catalyzing the oxidation of CEES to CEESO, achieving a conversion rate of 99% within 5 minutes, and no toxic CEESO2 generation was detected.

[0049] 2. Morphology, elemental composition, and spectroscopic characterization of two-dimensional sub-nanomaterials (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid.

[0050] To verify the successful synthesis of TiO2 / PMA subnanobelts, the material prepared in Example 1 was characterized by transmission electron microscopy (TEM) and atomic force microscopy (AFM), and the results are as follows: Figure 2 As shown in Figures a and b, the product prepared in Example 1 exhibits an irregular banded morphology. Figure 2 (a) and shows a thickness of approximately 0.7 nm. Figure 2 (b) This demonstrates that the product prepared in Example 1 is a sub-nanometer material.

[0051] Elemental energy dispersive spectroscopy (EDS) analysis was performed on the transmission electron microscope (TEM) images of the materials prepared in Example 1, and the results are as follows: Figure 3 As shown in the figure, the elemental energy dispersive spectroscopy (EDS) diagram shows the appearance of all elements in the material prepared in Example 1, with each element designated by a separate color. The results show that P (green), Ti (pink), and Mo (cyan) have an almost uniform distribution in the material.

[0052] The surface of the material prepared in Example 1 was further characterized by X-ray photoelectron spectroscopy (XPS), and the results are as follows: Figure 4 As shown. From Figure 4 As can be seen from the data, the surface elemental characterization results of the material prepared in Example 1 are consistent with the results shown in the energy spectrum, proving that the preparation method in Example 1 did indeed prepare two-dimensional sub-nano materials based on titanium dioxide and phosphomolybdic acid.

[0053] In addition, the materials prepared in Example 1 and PMA (phosphomolybdic acid) were characterized by UV-Vis absorption spectroscopy, and the results are as follows: Figure 5 As shown. From Figure 5 It was observed that the blue-black TiO2 / PMA subnanobelts absorbed across the entire UV-Vis region, while the yellow-brown PMA clusters absorbed only at 260 nm.

[0054] Infrared vibrational spectroscopy analysis was also performed on the materials prepared in Example 1, PMA, and TiO2, and the results are as follows: Figure 6 As shown. From Figure 6 It can be seen that, compared with the Fourier transform infrared (FTIR) spectrum of PMA, ν (Mo-O-Mo) (890cm -1 ≈760cm -1 ), ν (Mo-O) (≈964cm -1 ), ν (P-O) (≈1064cm –1 The same three peaks also appeared in the FTIR spectrum of the two-dimensional sub-nanomaterial (TiO2 / PMA sub-nanobelt) based on titanium dioxide and phosphomolybdic acid prepared in Example 1.

[0055] All the above test results demonstrate the successful synthesis of two-dimensional sub-nanomaterials (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid.

[0056] 3. Oxygen vacancies and catalytic generation of reactive oxygen species in two-dimensional sub-nanomaterials (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid.

[0057] Because large irregular regions appeared in the transmission electron microscope images of the two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid prepared in Example 1, it was suspected that oxygen vacancies might have been generated. Therefore, XPS analysis was performed on the two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid prepared in Example 1, and the results are as follows. Figure 7 As shown in Figure a. From Figure 7 As can be seen in Figure a, a signal of 531.8 eV was found in the O1s spectrum of the two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid prepared in Example 1, indicating the presence of oxygen vacancies. This explains the presence of large amorphous regions in the morphology characterization image of the two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid prepared in Example 1. Meanwhile, electron paramagnetic resonance (ESR) analysis was performed on the two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid prepared in Example 1, and the results are as follows... Figure 7 As shown in c. Figure 7 Electron paramagnetic resonance (ESR) analysis of c also confirmed the presence of oxygen vacancies. XPS analysis of the products after the catalytic degradation reaction in Example 2 yielded the following results: Figure 7 As shown in Figure b, the O 1s spectrum signal disappears at 531.8 eV after the catalytic degradation reaction of the two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid, indicating that oxygen vacancies do indeed participate in the reaction throughout the catalytic degradation process. Furthermore, the catalytic degradation reaction in Example 2 mainly involves species that catalytically generate reactive oxygen species.1 O2 and ·O2 - Experiments were conducted using 9,10-dimethylanthracene (DMA) as a singlet oxygen indicator. The fluorescence of DMA molecules decayed in the presence of H2O2 alone, as shown in the following figures. Figure 7 As shown in Figure d (the inset plot shows the fluorescence change of DMA molecules over time in the presence of H2O2 alone), the fluorescence decay of DMA molecules is observed in the presence of both H2O2 and TiO2 / PMA subnanobelts. Figure 7 As shown in figure e (the inset plot shows the fluorescence of DMA molecules over time in the presence of H2O2 and TiO2 / PMA subnanobelts),... Figure 7 d and Figure 7 By comparing the fluorescence decay changes and inlay plots of 9,10-dimethylanthracene, the following phenomena can be observed: With the addition of TiO2 / PMA subnanobelts as a catalyst, more singlet oxygen was generated, leading to a rapid decrease in the fluorescence intensity of 9,10-dimethylanthracene. This demonstrates that TiO2 / PMA subnanobelts have the ability to catalyze the production of singlet oxygen from H2O2. In addition, ESR testing was performed on the products after the catalytic degradation reaction in Example 2, and the results are as follows... Figure 7 As shown in Figure f, a 1:1:1 triplet singlet signal was generated in the ESR spectrum, further confirming the ability of TiO2 / PMA subnanobelts to catalyze the generation of singlet oxygen. Secondly, NBT was used as an indicator of superoxide anions. It is known that nitrotetrazole blue chloride (NBT) has UV absorption at 263 nm. However, in the presence of only H2O2, the UV absorption of nitrotetrazole blue chloride (NBT) did not change significantly (e.g., ...). Figure 7 As shown in Figure g, the inset plot shows the change in UV absorption of nitrotetrazole blue (NBT) over time. However, in the presence of both H₂O₂ and TiO₂ / PMA subnanobelts, the UV absorption of nitrotetrazole blue (NBT) decreased within 5 minutes (e.g., ...). Figure 7 As shown in Figure h, the inset plot shows the change of UV absorption of nitrotetrazole blue (NBT) over time, proving that TiO2 / PMA subnanobelts can catalyze the generation of superoxide anions.

[0058] ESR tests were performed on the catalytic material (TiO2 / PMA subnanobelts) used in the catalytic degradation reaction in Example 2, and the results are as follows: Figure 7 As shown in Figure i, the presence of a 1:2:2:1 signal peak in the ESR spectrum further confirms the generation of superoxide anions during the catalytic oxidation process in Example 2.

[0059] 4. CEES Catalytic Oxidation Kinetics

[0060] Based on the above experimental results, the oxidation reaction pathway of CEES using TiO2 / PMA subnanobelts can be deduced, specifically as follows: Figure 8 As shown in Figure a. The generation of H2O2 via TiO2 / PMA subnanobelt catalysis. 1 O2 and ·O2 - The reaction with CEES forms a sulfonamide intermediate; subsequently, the electrophilic oxygen of the electrophilic intermediate is transferred to a second CEES molecule; finally, the intermediate can decompose into two CEESO molecules, thereby achieving the oxidation of CEES. The TiO2 present in the two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid prepared in this invention is frequently used as a photosensitive material in oxidation reactions. Therefore, the conversion rate of the TiO2 / PMA sub-nanobelt reaction under xenon lamp, natural light, and darkness was investigated (e.g., Figure 8 (As shown in d). Studies have shown that xenon lamp irradiation can activate the photosensitivity of TiO2 and improve the oxidation conversion rate. However, the conversion rate is still as high as 95% under natural light, and even under dark conditions, the conversion rate is as high as 92.81%. This means that the reaction pathway under dark conditions is different from that under light conditions. This result depends on the inherent oxidation characteristics of PMA in the material. Therefore, in the study of catalytic degradation of CEES in this invention, the PMA on the two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid prepared in this invention also plays a major oxidation role, but it does not cause CEES to be peroxidized to CEESO2. Instead, the reaction stops at CEESO.

[0061] Therefore, the study can be conducted primarily under natural light conditions, and the reaction products are mainly produced using... 1 HNMR was used for monitoring. Under room temperature and natural light conditions, the conversion of CEES within 5 minutes was as follows: Figure 8 As shown in Figure b, the CEES reaction was completed within 5 minutes, indicating that the two-dimensional sub-nanomaterial (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid prepared in this invention exhibits excellent catalytic performance as a catalyst. Furthermore, the catalytic oxidation reaction kinetics of CEES were also investigated. Figure 8 Figure c shows the effects of the concentrations of TiO2, PMA clusters, and TiO2 / PMA subnanobelts on the reaction progress of CEES catalytic oxidation. From... Figure 8 As can be seen from c, the reaction time is related to ln(c) t / c0)(c t The linear relationship between the reactant concentration at time t and the initial reactant concentration (c0) indicates that the oxidation of CEES follows a pseudo-first-order kinetic process. The pseudo-first-order kinetic constant (k) of TiO2 / PMA subnanobelts is 2.9 min. -1 The obtained half-life (t) 1 / 2The reaction time was 12 s, indicating that TiO2 / PMA subnanobelts exhibit excellent CEES degradation performance, and the reaction is consistent with pseudo-first-order kinetics. These results demonstrate that the two-dimensional subnanomaterials (TiO2 / PMA subnanobelts) based on titanium dioxide and phosphomolybdic acid prepared in this invention possess superior catalytic performance in the CEES degradation process.

[0062] 5. Stability of two-dimensional sub-nanomaterials (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid

[0063] In catalytic reactions, the reusability and stability of the catalyst are crucial for its practical application. The fact that the reaction almost completely stopped after the catalyst was removed by filtration demonstrates the heterogeneous nature of the catalyst. Figure 8 In the figure, 'e' represents the conversion rate after 8 cycles of continuous addition of CEES under the action of a catalyst (two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid (TiO2 / PMA sub-nanobelts) and PHP microspheres). Figure 8 The catalyst stability test of Zhonge showed that the conversion rate of CEES remained close to 100% for 8 consecutive cycles of CEES addition, and no obvious performance degradation was observed. Figure 8 Image f shows the infrared spectra of two-dimensional sub-nanomaterials (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid after 1 and 8 cycles of catalytic degradation of CEES. Figure 8 As can be seen from f, the infrared spectra of TiO2 / PMA subnanobelts showed no significant changes after one cycle of catalytic degradation of CEES and after eight cycles of continuous catalytic degradation, confirming the true heterogeneous nature and structural stability of TiO2 / PMA subnanobelts. This demonstrates that TiO2 / PMA subnanobelts exhibit excellent structural stability during the selective oxidation of sulfides to the corresponding sulfoxides.

[0064] 6. Practical Applications of Catalysts Based on Two-Dimensional Sub-Nano Materials (TiO2 / PMA Sub-Nanobels) of Titanium Dioxide and Phosphomolybdic Acid

[0065] To further explore the practical applications of the two-dimensional sub-nanomaterial (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid of this invention, it is considered to load the two-dimensional sub-nanomaterial (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid of this invention onto the filter layer of a gas mask. To immobilize H2O2 on a solid carrier, polyvinylpyrrolidone (PVP) is used as the crosslinking agent for H2O2, forming PHP microspheres. These PHP microspheres can undergo a reverse reaction in the presence of water to produce H2O2. Therefore, the PHP microspheres and the two-dimensional sub-nanomaterial (TiO2 / PMA sub-nanobelts) based on titanium dioxide and phosphomolybdic acid prepared in Example 1 can be used as a source of reactive oxygen species for detoxifying CEES in the presence of natural light (as shown in the schematic diagram). Figure 9 (as shown in a). Figure 9 Figures b and c show the UV and IR absorption spectra of PVP, PHP microspheres, and a hybrid material (TiO2 / PMA / PHP SNBs (PHP-SNBs) formed by mixing TiO2 / PMA subnanobelts (TiO2 / PMA SNBs) with PHP microspheres, respectively. It can be seen that mixing PHP microspheres with TiO2 / PMA subnanobelts does not affect their respective UV and IR absorption, indicating that PHP microspheres (the synthesized crosslinked product of PVP and H2O2) have almost no impact on the material properties after mixing with TiO2 / PMA subnanobelts. Meanwhile, circularly cut cotton fabric was immersed in the TiO2 / PMA subnanobelt dispersion for one hour and dried at 60℃ for 1 hour. Photos of the cotton fabric before and after loading are shown below. Figure 9 As shown in d. Figure 9 Image f shows a SEM image of a cotton fabric loaded with TiO2 / PMA subnanobelts. It reveals that the surface of the cotton fibers in the filter layer of the TiO2 / PMA-loaded cotton fabric exhibits a rough fiber surface, contrasting with smooth cotton fibers (as shown in the SEM image below). Figure 9 This contrasts sharply with (as shown in e), demonstrating the successful loading of the catalyst material.

[0066] With water as the solvent, cotton fabric loaded with catalyst (TiO2 / PMA sub-nanobelts) can achieve 90% catalytic oxidative degradation of CEES within 5 minutes. Figure 9In the figure, g represents the CEES conversion rate of cotton fabric loaded with TiO2 / PMA subnanobelts after storage at room temperature for 0, 7, 14, and 21 days, respectively. It can be seen that after 21 days of storage at room temperature, the cotton fabric of the gas mask loaded with TiO2 / PMA subnanobelts and PHP microspheres can still efficiently degrade CEES, with a conversion rate remaining above 60%. This indicates that the high catalytic activity and stability of TiO2 / PMA subnanobelts and PHP microspheres in coated textiles for chemical warfare agent detoxification show promising applications in the development of real-time personal protective equipment.

[0067] Furthermore, regarding the method for preparing two-dimensional sub-nanomaterials in Example 1, varying the stirring time within the range of 5–20 min and the pressure in the high-pressure reactor within the range of 0–200 MPa also yields two-dimensional sub-nanomaterials assembled from titanium dioxide distributed on the surface of oriented phosphomolybdic acid clusters. The mass ratio of titanium dioxide to phosphomolybdic acid in these two-dimensional sub-nanomaterials is 1:5. Relevant tests show that their performance is similar to that of the two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid in Example 1, and both can be used for the catalytic degradation of mustard gas.

[0068] In summary, this invention discloses a two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid. This material has a core-shell structure, with titanium dioxide as the core and phosphomolybdic acid as the shell. With the assistance of long-chain ligands (oleylamine and octadecene), polyoxometalate clusters (phosphomolybdic acid clusters) are oriented and assembled into metal oxide / polyoxometalate cluster sub-nanobelts, which is the two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid. Given that the thickness of the two-dimensional sub-nanomaterial is only at the sub-nanometer level, the active sites can be fully exposed, thus exhibiting extremely high catalytic activity. This invention also discloses a method for preparing the two-dimensional sub-nanomaterial based on titanium dioxide and phosphomolybdic acid. The method mainly involves adding phosphomolybdic acid, titanium sulfate, octadecene, and oleylamine to water, reacting them in a high-pressure reactor, and then repeatedly washing with cyclohexane and ethanol before centrifugation. The preparation method of this invention has the advantages of simple reaction operation, wide availability of raw materials, and the ability to produce in batches. In addition, this invention also discloses a method for catalytic degradation of mustard gas. The method mainly involves loading PHP microspheres and two-dimensional sub-nanomaterials based on titanium dioxide and phosphomolybdic acid onto cotton fabric, adding mustard gas (taking 2-chloroethyl ethyl sulfoxide (CEESO) as an example), and then oxidizing the mustard gas (taking 2-chloroethyl ethyl sulfoxide (CEESO) as an example) into a non-toxic product through an activation reaction with water, thereby achieving the purpose of catalytic degradation of mustard gas.

[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A method for catalytically degrading mustard gas, characterized in that, The method is as follows: PHP microspheres and two-dimensional sub-nano materials are prepared into a solution, the substrate is immersed in the solution for loading and then dried, mustard gas is added, and the mustard gas is catalytically degraded by activating the reaction with water. The PHP microspheres were prepared by the following method: H2O2 and polyvinylpyrrolidone were mixed and stirred to obtain a gel-like product, which was then freeze-dried and ground to obtain powdered PHP microspheres. The two-dimensional sub-nanomaterial is a two-dimensional sub-nano ribbon material assembled by distributing titanium dioxide on the surface of oriented phosphomolybdic acid clusters.

2. The method according to claim 1, characterized in that, The mass ratio of the PHP microspheres to the two-dimensional sub-nano materials is not less than 1:1, and the volume ratio of the two-dimensional sub-nano materials to mustard gas is not less than 10:

1. The substrate is cotton fabric or synthetic fiber; The mass ratio of H2O2 to polyvinylpyrrolidone is 1.5:

1.

3. The method for catalytic degradation of mustard gas according to claim 1 or 2, characterized in that, The mass ratio of titanium dioxide to phosphomolybdic acid in the two-dimensional sub-nanomaterial is 1:

5.

4. The method for catalytic degradation of mustard gas according to claim 1 or 2, characterized in that, The preparation method of the two-dimensional sub-nanomaterial includes the following steps: (1) Add titanium sulfate to the aqueous solution of phosphomolybdic acid, stir and mix evenly, then add octadecene, continue stirring and mixing evenly, add oleylamine, and react in a high-pressure reactor; (2) After the reaction is complete, wash with cyclohexane and ethanol respectively and centrifuge. Repeat the operation to obtain two-dimensional sub-nano materials based on titanium dioxide and phosphomolybdic acid.

5. The preparation method according to claim 4, characterized in that, In step (1), the concentration of phosphomolybdic acid in the aqueous solution of phosphomolybdic acid is 0.01 g / mL.

6. The preparation method according to claim 4, characterized in that, In step (1), the mass-volume ratio of phosphomolybdic acid, titanium sulfate, octadecene and oleylamine in the aqueous solution of phosphomolybdic acid is 0.2:0.04:12.5:7.5, g:g:mL:mL.

7. The preparation method according to claim 4, characterized in that, In step (1), the stirring time is 5 to 20 minutes.

8. The preparation method according to claim 4, characterized in that, In step (1), the reaction temperature is 180℃ and the time is 6h, and the pressure in the high-pressure reactor is 50~200MPa.