A kind of compacted calcined petroleum coke and its production method and application

By expanding and modifying petroleum coke, combined with the use of polydopamine modified carbon fiber and asphalt binder, the problem of density and porosity of calcined petroleum coke is solved, the quality and stability of carbon products are improved, and it is suitable for a variety of applications. Production of carbon products.

CN118529718BActive Publication Date: 2024-10-25SHANDONG YUJIA ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411004558.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-25
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing calcined petroleum coke has low bulk density, low true density, and poor electrical conductivity, resulting in poor quality carbon products. The production method is simple but the product indicators fluctuate seriously, making it difficult to meet the demand for high-quality carbon products.

Method used

By mixing and ball milling expanded petroleum coke and CaO, using hydrogen peroxide and mixed acid for low-temperature expansion, combining polydopamine modified carbon fiber and asphalt binder, pressing and calcining, the compacted product has high density, low porosity and small resistivity. Calcined petroleum coke.

Benefits of technology

The density and mechanical properties of petroleum coke are significantly improved, and the porosity and resistivity are reduced. The compacted and calcined petroleum coke produced is suitable for carbon products such as graphitized electrodes and aluminum electrolytic anodes, and has stable and balanced quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention proposes a compacted calcined petroleum coke and a production method and application thereof, belonging to the technical field of petroleum coke. It includes: S1. Preparation of expanded petroleum coke; S2. Preparation of polydopamine modified carbon fiber; S3. Preparation of asphalt binder; S4. Pressing; S5. Calcination. The compacted calcined petroleum coke prepared by the present invention has high density, small porosity, low resistivity, good adhesion, good mechanical properties, simple method, mild conditions, balanced and stable quality, and can be used to produce graphitized electrodes, pre-baked anodes for aluminum electrolysis, self-baked anode paste, cathode tank cold-rammed carbon materials, cathode paste, pure graphitized crucibles, graphite armatures and other carbon products, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of petroleum coke, and in particular to a compacted calcined petroleum coke and a production method and application thereof. Background Art

[0002] The product of the residue, residual oil or petroleum asphalt after high-temperature coking after petroleum distillation is called pre-forged petroleum coke, which becomes calcined petroleum coke after calcination. Calcined petroleum coke can be used to produce carbon products such as graphitized electrodes, pre-baked anodes for aluminum electrolysis, self-baked anode paste, cold-rammed carbon materials for cathode tanks, cathode paste, pure graphitized crucibles, and graphite armatures.

[0003] The bulk density of calcined petroleum coke currently produced is generally 0.9-1.1 g / cm 3 , true density 2.0-2.10g / cm 3 , apparent porosity 40-60%, water absorption 30-50%. Due to its low bulk density, poor compressive strength and electrical conductivity, a large amount of asphalt binder is consumed in the production process of carbon products, and the coking value of asphalt is only 50%, which ultimately affects the quality of carbon products. The performance indicators of petroleum coke are determined by its production and processing methods. The existing method is to directly calcine the pre-forging petroleum coke in a pot calciner to become calcined petroleum coke, and then crush it to the required particle size. Although this method is simple, the product indicators fluctuate severely and fail to meet the requirements, resulting in reduced quality of carbon products. In order to improve the quality of carbon products, a petroleum coke product with high bulk density, true density and good electrical conductivity, and a method for producing the product are needed.

[0004] Chinese patent document CN1227327C discloses compacted calcined petroleum coke and its production method, and mentions that the production method of compacted calcined petroleum coke includes screening and grading-ball pressing-screening-calcination-oil immersion. The compacted calcined petroleum coke product has balanced and stable quality, and the technical indicators of the products produced successively are consistent. However, the compacted calcined petroleum coke still has problems such as poor mechanical properties. Summary of the invention

[0005] The purpose of the present invention is to provide a compacted calcined petroleum coke and its production method and application, which has high density, low porosity, low resistivity, good adhesion, good mechanical properties, simple method, mild conditions, balanced and stable quality, and can be used to produce carbon products such as graphitized electrodes, prebaked anodes for aluminum electrolysis, self-baked anode paste, cathode tank cold-rammed carbon materials, cathode paste, pure graphitized crucibles, graphite armatures, etc., and has broad application prospects.

[0006] The technical solution of the present invention is achieved in this way:

[0007] The present invention provides a method for producing compacted calcined petroleum coke, comprising the following steps:

[0008] S1. Preparation of puffed petroleum coke: crushing petroleum coke, mixing with CaO and ball milling, adding to hydrogen peroxide, heating and stirring to react, filtering, adding to mixed acid, stirring to react, filtering, washing, drying, and low-temperature puffing treatment to obtain puffed petroleum coke, wherein the mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid, and the volume ratio is 1:0.7-1.2, the temperature of the low-temperature puffing treatment is 150-250°C, the time is 1-3h, and the mass ratio of the petroleum coke to CaO is 10:1-2;

[0009] S2. Preparation of polydopamine-modified carbon fiber: adding carbon fiber to water, adding dopamine hydrochloride and a catalyst, heating and stirring the reaction, centrifuging, washing, and drying to obtain polydopamine-modified carbon fiber, wherein the mass ratio of the carbon fiber, dopamine hydrochloride and the catalyst is 10:2-3:0.1-0.2;

[0010] S3. Preparation of asphalt binder: The polydopamine-modified carbon fiber was added to asphalt, stirred and mixed uniformly to obtain an asphalt binder, wherein the mass ratio of the polydopamine-modified carbon fiber and asphalt was 3-5:10;

[0011] S4 pressing: the expanded petroleum coke and asphalt binder are mixed evenly, into a briquette machine, pressed into blocks, to obtain compacted petroleum coke, the mass ratio of the expanded petroleum coke to the asphalt binder is 10: 2-3;

[0012] S5. Calcination: calcining the compacted petroleum coke to obtain compacted calcined petroleum coke.

[0013] As a further improvement of the present invention, the temperature of the heating and stirring reaction in step S1 is 40-50°C, the time is 30-40min, and the time of the stirring reaction is 30-50min.

[0014] As a further improvement of the present invention, in step S1, the solid-liquid ratio of petroleum coke to hydrogen peroxide is 1 g:5-7 mL, the solid-liquid ratio of petroleum coke to mixed acid is 1 g:3-5 mL, and the concentration of hydrogen peroxide is 8-12 wt%.

[0015] As a further improvement of the present invention, the catalyst in step S2 is a Tris-HCl solution with a pH of 8.5-9.5, and the temperature of the heating and stirring reaction is 40-50° C. and the time is 2-3 hours.

[0016] As a further improvement of the present invention, the stirring and mixing time in step S3 is 20-40 minutes.

[0017] As a further improvement of the present invention, the hydraulic thrust of the press roller of the ball press in step S4 is 80-100 tons.

[0018] As a further improvement of the present invention, the calcination temperature in step S5 is 1100-1300° C. and the calcination time is 1-3 h.

[0019] As a further improvement of the present invention, the present invention specifically comprises the following steps:

[0020] S1. Preparation of puffed petroleum coke: 10 parts by weight of petroleum coke is crushed, mixed with 1-2 parts by weight of CaO and ball-milled, added to 8-12wt% hydrogen peroxide, the solid-liquid ratio of the petroleum coke to the hydrogen peroxide is 1g:5-7mL, heated to 40-50°C, stirred for 30-40min, filtered, added to a mixed acid, the solid-liquid ratio of the petroleum coke to the mixed acid is 1g:3-5mL, stirred for 30-50min, filtered, washed, dried, and puffed at 150-250°C for 1-3h to obtain puffed petroleum coke;

[0021] The mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid, with a volume ratio of 1:0.7-1.2;

[0022] S2. Preparation of polydopamine modified carbon fiber: 10 parts by weight of carbon fiber is added to water, 2-3 parts by weight of dopamine hydrochloride and 0.1-0.2 parts by weight of catalyst are added, heated to 40-50°C, stirred for reaction for 2-3h, centrifuged, washed, and dried to obtain polydopamine modified carbon fiber;

[0023] The catalyst is a Tris-HCl solution with a pH of 8.5-9.5;

[0024] S3 Preparation of asphalt binder: 3-5 parts by weight of polydopamine-modified carbon fiber was added to 10 parts by weight of asphalt, stirred and mixed for 20-40min to obtain an asphalt binder;

[0025] S4 pressing: 10 parts by weight of expanded petroleum coke and 2-3 parts by weight of asphalt binder are mixed evenly and fed into a briquette press, the hydraulic thrust of the roller is 80-100 tons, pressed into blocks to obtain compacted petroleum coke;

[0026] S5. Calcination: heat the compacted petroleum coke to 1100-1300°C and calcine for 1-3 hours to obtain compacted calcined petroleum coke.

[0027] The present invention further protects a compacted calcined petroleum coke obtained by the above production method.

[0028] The present invention further protects a use of the above-mentioned compacted calcined petroleum coke in the preparation of carbon products.

[0029] The present invention has the following beneficial effects:

[0030] The price of petroleum coke is low, and its effective use can bring huge profits. However, its high sulfur content limits its application. The sulfur exists in a stable form, distributed in the carbon skeleton and aromatic rings, and is difficult to remove.

[0031] The present invention uses calcium oxide and crushed petroleum coke for mixed ball milling treatment, wherein Ca is intercalated in the petroleum coke, and the structure of the petroleum coke is pre-adjusted, so that the sulfide is fully exposed, the internal graphite microcrystalline structure of the petroleum coke is loosened, the contact efficiency between the sulfide and the oxidant hydrogen peroxide is improved, and the oxidation reaction desulfurization is helpful. The sulfide is oxidized by hydrogen peroxide under mild conditions, and the byproduct is water, which is green and environmentally friendly. After being treated with a mixed acid (concentrated sulfuric acid and concentrated nitric acid) with strong oxidizing ability, on the one hand, the acid can react with the alkaline substance Ca intercalated in the petroleum coke, which can play a rapid expansion role and increase the interlayer spacing of the internal graphite microcrystalline structure. On the other hand, the mixed acid also has good oxidizability and can further oxidize the sulfide, which is convenient for the removal of the sulfide. At the same time, the microstructure of the petroleum coke is made more fluffy, thereby facilitating the penetration and bonding of the asphalt binder, thereby greatly improving the density of the obtained compacted calcined petroleum coke, reducing the porosity, and significantly reducing the resistivity.

[0032] The asphalt binder of the present invention adds carbon fibers modified by coating the surface with polydopamine. On the one hand, the carbon fibers can significantly improve the mechanical properties of the obtained compacted calcined petroleum coke. At the same time, the high viscosity of polydopamine also improves the adhesion of asphalt to petroleum coke and the compatibility of carbon fibers, improves their distribution, reduces agglomeration, increases the density of the compacted calcined petroleum coke, and reduces the porosity.

[0033] The compacted calcined petroleum coke prepared by the invention has high density, low porosity, low resistivity, good adhesion and good mechanical properties. The method is simple, the conditions are mild, and the quality is balanced and stable. The invention can be used to produce carbon products such as graphitized electrodes, prebaked anodes for aluminum electrolysis, self-baked anode paste, cathode tank cold-rammed carbon materials, cathode paste, pure graphitized crucibles, graphite armatures, etc., and has broad application prospects. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Petroleum coke, with a sulfur content of 2.2-2.7 wt%, was purchased from Tianjin Mingxintai Petrochemical Co., Ltd. Example 1

[0036] This embodiment provides a method for producing compacted calcined petroleum coke, which specifically comprises the following steps:

[0037] S1. Preparation of puffed petroleum coke: 10 g of petroleum coke was crushed, mixed with 1 g of CaO and ball-milled, added to 50 mL of 8 wt% hydrogen peroxide, heated to 40 ° C, stirred for 30 min, filtered, added to 30 mL of mixed acid, stirred for 30 min, filtered, washed, dried, and puffed at 150 ° C for 1 h to obtain puffed petroleum coke;

[0038] The mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid, with a volume ratio of 1:0.7;

[0039] S2. Preparation of polydopamine modified carbon fiber: 10 g of carbon fiber was added to 200 mL of water, 2 g of dopamine hydrochloride and 0.1 g of catalyst were added, heated to 40° C., stirred for reaction for 2 h, centrifuged, washed, and dried to obtain polydopamine modified carbon fiber;

[0040] The catalyst is a Tris-HCl solution with a pH of 8.5;

[0041] S3 Preparation of asphalt binder: 3g of polydopamine-modified carbon fiber was added to 10g of asphalt and stirred for 20min to obtain an asphalt binder;

[0042] S4 pressing: 10g of expanded petroleum coke and 2g of asphalt binder were mixed evenly and entered into a briquette press. The hydraulic thrust of the roller was 80 tons and pressed into blocks to obtain compacted petroleum coke.

[0043] S5. Calcination: heat the compacted petroleum coke to 1100°C and calcine for 1 hour to obtain compacted calcined petroleum coke. Example 2

[0044] This embodiment provides a method for producing compacted calcined petroleum coke, which specifically comprises the following steps:

[0045] S1. Preparation of puffed petroleum coke: 10 g of petroleum coke was crushed, mixed with 2 g of CaO and ball-milled, added to 70 mL of 12 wt% hydrogen peroxide, heated to 50 ° C, stirred for 40 min, filtered, added to 50 mL of mixed acid, stirred for 50 min, filtered, washed, dried, and puffed at 250 ° C for 3 h to obtain puffed petroleum coke;

[0046] The mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid, with a volume ratio of 1:1.2;

[0047] S2. Preparation of polydopamine modified carbon fiber: 10 g of carbon fiber was added to 200 mL of water, 3 g of dopamine hydrochloride and 0.2 g of catalyst were added, heated to 50° C., stirred for reaction for 3 h, centrifuged, washed, and dried to obtain polydopamine modified carbon fiber;

[0048] The catalyst is a Tris-HCl solution with a pH of 9.5;

[0049] S3 Preparation of asphalt binder: 5g of polydopamine-modified carbon fiber was added to 10g of asphalt and stirred for 40min to obtain an asphalt binder;

[0050] S4 pressing: 10g of puffed petroleum coke and 3g of asphalt binder were mixed evenly and entered into a briquette press. The hydraulic thrust of the roller was 100 tons and pressed into blocks to obtain compacted petroleum coke.

[0051] S5. Calcination: heat the compacted petroleum coke to 1300°C and calcine for 3 hours to obtain compacted calcined petroleum coke. Example 3

[0052] This embodiment provides a method for producing compacted calcined petroleum coke, which specifically comprises the following steps:

[0053] S1. Preparation of puffed petroleum coke: 10 g of petroleum coke was crushed, mixed with 1.5 g of CaO and ball-milled, added to 60 mL of 10 wt% hydrogen peroxide, heated to 45 ° C, stirred for 35 min, filtered, added to 40 mL of mixed acid, stirred for 40 min, filtered, washed, dried, and puffed at 200 ° C for 2 h to obtain puffed petroleum coke;

[0054] The mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1;

[0055] S2. Preparation of polydopamine modified carbon fiber: 10 g of carbon fiber was added to 200 mL of water, 2.5 g of dopamine hydrochloride and 0.15 g of catalyst were added, heated to 45° C., stirred for reaction for 2.5 h, centrifuged, washed, and dried to obtain polydopamine modified carbon fiber;

[0056] The catalyst is a Tris-HCl solution with a pH of 9;

[0057] S3 Preparation of asphalt binder: 4g of polydopamine-modified carbon fiber was added to 10g of asphalt and stirred for 30min to obtain an asphalt binder;

[0058] S4 pressing: 10g of puffed petroleum coke and 2.5g of asphalt binder were mixed evenly and entered into a briquette press. The hydraulic thrust of the roller was 90 tons and pressed into blocks to obtain compacted petroleum coke.

[0059] S5. Calcination: heat the compacted petroleum coke to 1200°C and calcine for 2 hours to obtain compacted calcined petroleum coke.

[0060] Comparative Example 1

[0061] Compared with Example 3, the difference is that no hydrogen peroxide treatment is performed in step S1.

[0062] The details are as follows:

[0063] S1. Preparation of puffed petroleum coke: 10 g of petroleum coke was crushed, mixed with 1.5 g of CaO and ball-milled, added to 40 mL of mixed acid, stirred for 40 min, filtered, washed, dried, and puffed at 200 ° C for 2 h to obtain puffed petroleum coke;

[0064] The mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1;

[0065] S2. Preparation of polydopamine modified carbon fiber: 10 g of carbon fiber was added to 200 mL of water, 2.5 g of dopamine hydrochloride and 0.15 g of catalyst were added, heated to 45° C., stirred for reaction for 2.5 h, centrifuged, washed, and dried to obtain polydopamine modified carbon fiber;

[0066] The catalyst is a Tris-HCl solution with a pH of 9;

[0067] S3 Preparation of asphalt binder: 4g of polydopamine-modified carbon fiber was added to 10g of asphalt and stirred for 30min to obtain an asphalt binder;

[0068] S4 pressing: 10g of puffed petroleum coke and 2.5g of asphalt binder were mixed evenly and entered into a briquette press. The hydraulic thrust of the roller was 90 tons and pressed into blocks to obtain compacted petroleum coke.

[0069] S5. Calcination: heat the compacted petroleum coke to 1200°C and calcine for 2 hours to obtain compacted calcined petroleum coke.

[0070] Comparative Example 2

[0071] Compared with Example 3, the difference is that no mixed acid treatment is performed in step S1.

[0072] The details are as follows:

[0073] S1. Preparation of puffed petroleum coke: 10 g of petroleum coke was crushed, mixed with 1.5 g of CaO and ball-milled, added to 60 mL of 10 wt% hydrogen peroxide, heated to 45 ° C, stirred for 35 min, filtered, washed, dried, and puffed at 200 ° C for 2 h to obtain puffed petroleum coke;

[0074] S2. Preparation of polydopamine modified carbon fiber: 10 g of carbon fiber was added to 200 mL of water, 2.5 g of dopamine hydrochloride and 0.15 g of catalyst were added, heated to 45° C., stirred for reaction for 2.5 h, centrifuged, washed, and dried to obtain polydopamine modified carbon fiber;

[0075] The catalyst is a Tris-HCl solution with a pH of 9;

[0076] S3 Preparation of asphalt binder: 4g of polydopamine-modified carbon fiber was added to 10g of asphalt and stirred for 30min to obtain an asphalt binder;

[0077] S4 pressing: 10g of puffed petroleum coke and 2.5g of asphalt binder were mixed evenly and entered into a briquette press. The hydraulic thrust of the roller was 90 tons and pressed into blocks to obtain compacted petroleum coke.

[0078] S5. Calcination: heat the compacted petroleum coke to 1200°C and calcine for 2 hours to obtain compacted calcined petroleum coke.

[0079] Comparative Example 3

[0080] Compared with Example 3, the difference is that step S2 is not performed.

[0081] The details are as follows:

[0082] S1. Preparation of puffed petroleum coke: 10 g of petroleum coke was crushed, mixed with 1.5 g of CaO and ball-milled, added to 60 mL of 10 wt% hydrogen peroxide, heated to 45 ° C, stirred for 35 min, filtered, added to 40 mL of mixed acid, stirred for 40 min, filtered, washed, dried, and puffed at 200 ° C for 2 h to obtain puffed petroleum coke;

[0083] The mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1;

[0084] S2 Preparation of asphalt binder: 4g of carbon fiber was added to 10g of asphalt and stirred for 30min to obtain an asphalt binder;

[0085] S3 pressing: 10g of puffed petroleum coke and 2.5g of asphalt binder were mixed evenly and entered into a briquette press. The hydraulic thrust of the roller was 90 tons and pressed into blocks to obtain compacted petroleum coke.

[0086] S4. Calcination: heat the compacted petroleum coke to 1200°C and calcine for 2 hours to obtain compacted calcined petroleum coke.

[0087] Comparative Example 4

[0088] Compared with Example 3, the difference is that step S3 is not performed.

[0089] The details are as follows:

[0090] S1. Preparation of puffed petroleum coke: 10 g of petroleum coke was crushed, mixed with 1.5 g of CaO and ball-milled, added to 60 mL of 10 wt% hydrogen peroxide, heated to 45 ° C, stirred for 35 min, filtered, added to 40 mL of mixed acid, stirred for 40 min, filtered, washed, dried, and puffed at 200 ° C for 2 h to obtain puffed petroleum coke;

[0091] The mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1;

[0092] S2. Preparation of polydopamine modified carbon fiber: 10 g of carbon fiber was added to 200 mL of water, 2.5 g of dopamine hydrochloride and 0.15 g of catalyst were added, heated to 45° C., stirred for reaction for 2.5 h, centrifuged, washed, and dried to obtain polydopamine modified carbon fiber;

[0093] The catalyst is a Tris-HCl solution with a pH of 9;

[0094] S3 pressing: 10g of puffed petroleum coke and 2.5g of asphalt were mixed evenly and entered into a briquette press. The hydraulic thrust of the roller was 90 tons and pressed into blocks to obtain compacted petroleum coke.

[0095] S4. Calcination: heat the compacted petroleum coke to 1200°C and calcine for 2 hours to obtain compacted calcined petroleum coke.

[0096] Test Example 1 Desulfurization Rate

[0097] The residual sulfur mass fraction of the compacted and calcined petroleum cokes obtained in Examples 1-3 and Comparative Examples 1-4 was measured using a microcomputer coulometric sulfur analyzer (CLS-3000), and the final desulfurization rate (%) of the petroleum coke was calculated according to the following formula. The results are shown in Table 1.

[0098] Desulfurization rate (%) = (w0-w1) / w0×100%

[0099] Wherein: w0 and w1 represent the sulfur mass fraction of petroleum coke and the residual sulfur mass fraction of compacted and calcined petroleum coke, respectively, %.

[0100] Table 1 ;

[0101] It can be seen from the above table that the compacted calcined petroleum cokes prepared in Examples 1-3 of the present invention have a good desulfurization rate.

[0102] Test Example 2

[0103] The powder resistivity of the compacted calcined petroleum cokes prepared in Examples 1-3 and Comparative Examples 1-4 was tested according to standard: YS-T 625-2012. The results are shown in Table 2.

[0104] Table 2 ;

[0105] It can be seen from the above table that the compacted calcined petroleum cokes prepared in Examples 1-3 of the present invention have lower powder resistivity.

[0106] Test Example 3

[0107] The performance of the compacted calcined petroleum cokes obtained in Examples 1-3 of the present invention and Comparative Examples 1-4 was tested.

[0108] Apparent porosity: tested according to the method of GB / T 4511.1-2008.

[0109] True specific gravity: tested according to the method of GB / T 4511.4-84.

[0110] Bending performance: The universal testing machine is used to test the bending strength of the material through the three-point bending method. The sample size is 5×10×50 mm 3 The calculation formula is as follows:

[0111] ;

[0112] Where: is the bending strength, MPa; p is the maximum bending force, N; l is the test span, 40 mm; b is the width of the sample, mm; h is the thickness of the sample, mm.

[0113] The results are shown in Table 3.

[0114] Table 3 ;

[0115] It can be seen from the above table that the compacted calcined petroleum cokes prepared in Examples 1-3 of the present invention have a larger density and a higher porosity.

[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for producing compacted calcined petroleum coke, characterized in that: The following steps are involved: S1. Preparation of puffed petroleum coke: crushing petroleum coke, mixing with CaO and ball milling, adding to hydrogen peroxide, heating and stirring to react, filtering, adding to mixed acid, stirring to react, filtering, washing, drying, and low-temperature puffing treatment to obtain puffed petroleum coke, wherein the mixed acid is a mixture of concentrated sulfuric acid and concentrated nitric acid, and the volume ratio is 1:0.7-1.2, the temperature of the low-temperature puffing treatment is 150-250°C, the time is 1-3h, and the mass ratio of the petroleum coke to CaO is 10:1-2; S2. Preparation of polydopamine-modified carbon fiber: adding carbon fiber to water, adding dopamine hydrochloride and a catalyst, heating and stirring the reaction, centrifuging, washing, and drying to obtain polydopamine-modified carbon fiber, wherein the mass ratio of the carbon fiber, dopamine hydrochloride and the catalyst is 10:2-3:0.1-0.2; S3. Preparation of asphalt binder: The polydopamine-modified carbon fiber was added to asphalt, stirred and mixed uniformly to obtain an asphalt binder, wherein the mass ratio of the polydopamine-modified carbon fiber and asphalt was 3-5:10; S4 pressing: the expanded petroleum coke and asphalt binder are mixed evenly, into a briquette machine, pressed into blocks, to obtain compacted petroleum coke, the mass ratio of the expanded petroleum coke to the asphalt binder is 10: 2-3; S5. Calcination: calcining the compacted petroleum coke to obtain compacted calcined petroleum coke.

2. The production method according to claim 1, characterized in that The temperature of the heating and stirring reaction in step S1 is 40-50°C, the time is 30-40min, and the time of the stirring reaction is 30-50min.

3. The production method according to claim 1, characterized in that In step S1, the solid-liquid ratio of petroleum coke to hydrogen peroxide is 1 g:5-7 mL, the solid-liquid ratio of petroleum coke to mixed acid is 1 g:3-5 mL, and the concentration of hydrogen peroxide is 8-12 wt%.

4. The production method according to claim 1, characterized in that In step S2, the catalyst is a Tris-HCl solution with a pH of 8.5-9.5, and the temperature of the heating and stirring reaction is 40-50° C. for 2-3 hours.

5. The production method according to claim 1, characterized in that: The stirring and mixing time in step S3 is 20-40 minutes.

6. The production method according to claim 1, characterized in that: The hydraulic thrust of the press roller of the ball press in step S4 is 80-100 tons.

7. The production method according to claim 1, characterized in that: The calcination temperature in step S5 is 1100-1300° C. and the calcination time is 1-3 hours.

8. A compacted calcined petroleum coke obtained by the production method according to any one of claims 1 to 7.

9. Use of the compacted calcined petroleum coke as claimed in claim 8 in the preparation of carbon products.