A hydrophobic film and preparation method thereof
Through the use of modified nano-zinc oxide and modifiers, the deficiencies in hydrophobicity and antibacterial properties of polypropylene films are solved, and a hydrophobic film with excellent performance and low cost is prepared, which meets the high demand in the field of hydrophobic film technology.
Patent Information
- Application Number
- CN202411000441.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The polypropylene film itself has poor hydrophobicity, resulting in reduced performance during long-term use and cleaning, and lacks antibacterial properties, making it unable to meet the high demand in the field of hydrophobic film technology.
Polypropylene resin, modifier, antioxidant, modified nano-zinc oxide and dibenzoyl peroxide are used to prepare a hydrophobic film through stirring mixing, twin-screw extrusion, vertical and horizontal stretching and corona treatment. Modified nano-zinc oxide Modified by silane coupling agent to improve interfacial compatibility, the modifier enhances antibacterial and hydrophobic properties through quaternary ammonium salts, C-F bonds, long carbon chains and benzene ring structures.
The antibacterial, hydrophobic and antistatic properties of the film are significantly improved, the cost is reduced, the performance is long-term and stable, and it is suitable for the field of hydrophobic film technology.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of hydrophobic films, and in particular, relates to a hydrophobic film and a preparation method thereof. Background Art
[0002] With the advancement of science and technology, hydrophobic materials have received a lot of attention in recent years due to their unique properties. Inspired by the lotus leaf effect, hydrophobic films made of hydrophobic materials are a type of film with special surface properties, with a contact angle with water greater than 150° and a rolling angle less than 10°. Since the contact area of the liquid on the hydrophobic film is very small, the water droplets rolling on the surface of the film can carry away pollutants, thereby achieving the purpose of cleaning. Due to its excellent performance, it has a wide range of applications in food preservation, packaging materials and metal corrosion protection.
[0003] Common film materials include polytetrafluoroethylene, polyvinyl chloride, polypropylene, high-density polyethylene, polyurethane, etc. Among them, polypropylene film is a plastic product with light weight, environmental friendliness, low price, excellent performance, easy molding and wide application. There are several methods and uses for polypropylene film molding: polypropylene extrusion blown film is a product with simple production equipment, high production efficiency and low price. It is widely used in food packaging, textiles and civilian daily necessities packaging. Extrusion cast film is a film with high transparency, good moisture barrier, excellent heat and cold resistance, and easy heat sealing. It is mainly used for packaging of food, textiles, stationery and other items. Its performance is better than polyethylene blown film, so it is widely used in the packaging of textiles, flowers, food and daily necessities. However, the hydrophobicity of polypropylene film itself is poor. At present, most polypropylene film materials are reusable materials, and in order to keep the materials clean, they need to be washed frequently. However, the water resistance of the film materials currently available on the market is poor, and long-term washing will lead to the reduction of the performance of the film materials; not only that, when used in some fields, the film also needs to have certain antibacterial properties. Therefore, there is an urgent need to invent a polypropylene hydrophobic antibacterial film to meet the higher demands in the field of hydrophobic film technology. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a hydrophobic film and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing a hydrophobic film comprises the following steps:
[0007] The polypropylene resin, modifier, antioxidant, modified nano zinc oxide and dibenzoyl peroxide (initiator) are stirred and mixed evenly, added into a twin-screw extruder, melt blended, extruded, longitudinally stretched and transversely stretched into a film, and then corona treated, rolled up, and slit into a hydrophobic film.
[0008] Furthermore, the raw materials are calculated in parts by weight as follows: 45-55 parts of polypropylene resin, 6-12 parts of modifier, 2-4 parts of antioxidant, 5-10 parts of modified nano zinc oxide, and 0.1-0.3 parts of dibenzoyl peroxide.
[0009] Furthermore, the antioxidant is one of antioxidant 1010 and antioxidant 264.
[0010] Furthermore, the modified nano zinc oxide is prepared by the following steps:
[0011] At room temperature, add nano zinc oxide and water into a flask, stir at high speed for 15 minutes under a high shear mixer emulsifier, add γ-(methacryloyloxy)propyltrimethoxysilane (silane coupling agent KH-570), continue to stir at high speed for 30 minutes under a high shear mixer emulsifier, and after the reaction is completed, filter and vacuum dry to obtain modified nano zinc oxide.
[0012] Furthermore, the usage ratio of nano zinc oxide, water, and γ-(methacryloyloxy)propyltrimethoxysilane is 10.0 g:100 mL:5.5 g.
[0013] Nano zinc oxide has the advantages of being non-toxic, long-lasting active, low cost, good biocompatibility and excellent antibacterial properties. It can not only improve the antibacterial properties of the film, but also the modified nano zinc oxide can increase the roughness of the film and improve the hydrophobic properties of the film. The use of silane coupling agent to modify nano zinc oxide, that is, forming an organic layer on its surface, can greatly improve the interfacial compatibility of nano zinc oxide and the matrix, thereby promoting the uniform dispersion of nano zinc oxide in the matrix, reducing agglomeration, and giving full play to the performance of nano zinc oxide.
[0014] Furthermore, the modifier is prepared by the following steps:
[0015] S1. In a three-necked flask equipped with a stirring device, add cyanuric chloride, sodium hydroxide, triethylamine and toluene in sequence, stir and mix evenly, stir at room temperature for 20 minutes, add pentafluorophenol, control the reaction temperature to 50°C, keep the reaction for 4 hours, and after the reaction is completed, filter, wash the filtrate with saturated brine 3 times, dry with anhydrous magnesium sulfate, filter again, and purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two is 7:1), and remove the eluent by rotary evaporation to obtain intermediate 1; the ratio of cyanuric chloride, sodium hydroxide, triethylamine, toluene and pentafluorophenol is 19.6g:3.9g:30mL:50mL:18.4g;
[0016] Sodium hydroxide reacts with the hydroxyl group on pentafluorophenol to form sodium phenolate with stronger nucleophilicity. Sodium phenolate, as a nucleophilic reagent, attacks the carbon atom connected to the chlorine atom on cyanuric chloride, so that the chlorine atom is replaced, thereby generating an ether bond. By controlling the molar ratio of pentafluorophenol to cyanuric chloride to be close to 1:1 and the cyanuric chloride to be slightly excessive, only one chlorine group on the cyanuric chloride participates in the reaction, and triethylamine removes the hydrogen chloride generated by the reaction to obtain intermediate 1. The specific reaction process is as follows:
[0017]
[0018] S2. At room temperature, under nitrogen protection, in a three-necked flask equipped with a stirring device, allyl chloride, 1-nonylamine, toluene and triethylamine were mixed and stirred uniformly, the reaction temperature was controlled to 65°C, and the reaction was carried out for 6 hours. After the reaction was completed, part of the solvent was first removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 1:7), and the eluent was removed by rotary evaporation to obtain intermediate 2; the ratio of allyl chloride, 1-nonylamine, toluene and triethylamine was 7.6 g:14.3 g:50 mL:15 mL;
[0019] Allyl chloride and 1-nonylamine undergo nucleophilic substitution, and triethylamine removes the hydrogen chloride generated by the reaction to obtain intermediate 2. The specific reaction process is as follows:
[0020]
[0021] S3. At room temperature, in a three-necked flask equipped with a stirring device, intermediate 1, intermediate 2, triethylamine and toluene were mixed and stirred uniformly under nitrogen protection, the reaction temperature was controlled to 75°C, and the reaction was kept warm for 8 hours. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 1:8). The eluent was removed by rotary evaporation to obtain intermediate 3. The ratio of the amount of intermediate 1, intermediate 2, triethylamine and toluene was 37.4 g:33.2 g:30 mL:100 mL.
[0022] Intermediate 1 and intermediate 2 undergo nucleophilic substitution, and the molar ratio of the two is controlled to be close to 2:1 and intermediate 1 is slightly excessive, and triethylamine removes the hydrogen chloride generated by the reaction to obtain intermediate 3; the specific reaction process is as follows:
[0023]
[0024] S4. In a three-necked flask equipped with a stirring device, the intermediate 3, methyl iodide and N,N-dimethylformamide were mixed and stirred uniformly, the reaction temperature was controlled at 80°C, the reaction was carried out for 8 hours, and after sufficient reaction, the mixture was distilled under reduced pressure, washed with anhydrous ethanol and saturated brine in turn, and allowed to stand and dry to obtain a modifier; the ratio of the intermediate 3, methyl iodide and N,N-dimethylformamide was 62.5g:28.2g:150mL;
[0025] A quaternization reaction occurs, and an excess of methyl iodide is added to fully react to obtain a modifier; the structure of the modifier is shown below:
[0026]
[0027] The prepared modifier molecule contains quaternary ammonium salt, CF bond, long carbon chain and benzene ring structure. Among them, quaternary ammonium salt, as an excellent antibacterial structure, can produce strong electrostatic interaction between the positively charged and negatively charged bacteria, and can produce strong adsorption on the bacteria. It has good permeability, low toxicity and stable performance, which can greatly enhance the antibacterial performance of the matrix. In addition, the quaternary ammonium salt ions in the modifier can also improve the antistatic performance of the matrix; the introduction of CF bond, which has a high chemical bond and good stability, can give the matrix significant waterproofness; and can coat the CC main chain, reduce the surface energy of the matrix, and improve the stability of the matrix; in addition, the long carbon chain belongs to the methylene chain segment, has strong hydrophobicity, can improve the hydrophobicity and mechanical properties of the matrix to a certain extent, and can be interspersed in the molecular chain of the matrix to further improve the stability; finally, the introduction of benzene ring as a hydrophobic structure further enhances the hydrophobicity of the matrix;
[0028] It should be noted that the modifier molecule also contains carbon-carbon double bonds, which can produce chemical bonding with the matrix, which not only improves the compatibility of the modifier and the matrix, allowing the performance of the modifier to be fully exerted, but also prevents the migration and shedding of the modifier, ensuring the long-term stability of the modifier's performance.
[0029] Beneficial effects of the present invention:
[0030] 1. The film prepared by the present invention is based on polypropylene and is prepared by one-time extrusion and stretching. The prepared film has excellent performance, and the method is simple, which can effectively reduce costs.
[0031] 2. By modifying nano zinc oxide, the interfacial compatibility between nano zinc oxide and the matrix is improved, the agglomeration of nano zinc oxide is reduced, and the antibacterial and hydrophobic properties of the film are significantly enhanced.
[0032] 3. The prepared modifier can greatly enhance the antibacterial, hydrophobic and to a certain extent antistatic and mechanical properties of the film, and the performance is long-lasting and stable.
[0033] Therefore, the film prepared by the present invention has stable and efficient antibacterial properties, hydrophobicity and a certain degree of antistatic properties and mechanical properties, and has important application value in the field of hydrophobic film technology. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1: Preparation of modifier:
[0036] S1. In a three-necked flask equipped with a stirring device, 19.6 g of cyanuric chloride, 3.9 g of sodium hydroxide, 30 mL of triethylamine and 50 mL of toluene were added in sequence, and the mixture was stirred and mixed evenly. After stirring at room temperature for 20 min, 18.4 g of pentafluorophenol was added, and the reaction temperature was controlled to 50 ° C. The reaction was kept warm for 4 h. After the reaction was completed, the mixture was filtered, and the filtrate was washed 3 times with saturated brine, dried over anhydrous magnesium sulfate, filtered again, and purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 7:1), and the eluent was removed by rotary evaporation to obtain intermediate 1;
[0037] S2. At room temperature, 7.6 g of allyl chloride, 14.3 g of 1-nonylamine, 50 mL of toluene and 15 mL of triethylamine were mixed and stirred evenly in a three-necked flask equipped with a stirring device under nitrogen protection. The reaction temperature was controlled to 65° C. and the reaction was carried out for 6 h. After the reaction was completed, part of the solvent was first removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 1:7), and the eluent was removed by rotary evaporation to obtain intermediate 2;
[0038] S3, at room temperature, under nitrogen protection, in a three-necked flask equipped with a stirring device, 37.4 g of intermediate 1, 33.2 g of intermediate 2, 30 mL of triethylamine and 100 mL of toluene were mixed and stirred evenly, the reaction temperature was controlled to 75°C, and the reaction was kept warm for 8 hours. After the reaction was completed, it was filtered, and part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 1:8), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0039] S4. In a three-necked flask equipped with a stirring device, mix 62.5 g of intermediate 3, 28.2 g of methyl iodide and 150 mL of N,N-dimethylformamide and stir evenly. Control the reaction temperature at 80°C and react for 8 hours. After sufficient reaction, distill under reduced pressure, wash with anhydrous ethanol and saturated brine in turn, and stand to dry to obtain a modifier.
[0040] Example 2: Preparation of Modifying Agent:
[0041] S1. In a three-necked flask equipped with a stirring device, 39.2 g of cyanuric chloride, 7.8 g of sodium hydroxide, 60 mL of triethylamine and 100 mL of toluene were added in sequence, and the mixture was stirred and mixed evenly. After stirring at room temperature for 20 min, 36.8 g of pentafluorophenol was added, and the reaction temperature was controlled to 50 ° C. The reaction was kept warm for 4 h. After the reaction was completed, the mixture was filtered, and the filtrate was washed 3 times with saturated brine. The organic phase was dried over anhydrous magnesium sulfate, filtered again, and purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 7:1). The eluent was removed by rotary evaporation to obtain intermediate 1;
[0042] S2. At room temperature, 15.2 g of allyl chloride, 28.6 g of 1-nonylamine, 100 mL of toluene and 30 mL of triethylamine were mixed and stirred evenly in a three-necked flask equipped with a stirring device under nitrogen protection. The reaction temperature was controlled to 65° C. and the reaction was carried out for 6 h. After the reaction was completed, part of the solvent was first removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 1:7), and the eluent was removed by rotary evaporation to obtain intermediate 2;
[0043] S3, at room temperature, under nitrogen protection, in a three-necked flask equipped with a stirring device, 74.8 g of intermediate 1, 66.4 g of intermediate 2, 60 mL of triethylamine and 200 mL of toluene were mixed and stirred evenly, the reaction temperature was controlled to 75°C, and the reaction was kept warm for 8 hours. After the reaction was completed, it was filtered, and part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 1:8), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0044] S4. In a three-necked flask equipped with a stirring device, 125 g of intermediate 3, 56.4 g of methyl iodide and 300 mL of N,N-dimethylformamide were mixed and stirred evenly, the reaction temperature was controlled at 80°C, and the reaction was carried out for 8 hours. After sufficient reaction, the mixture was distilled under reduced pressure, washed with anhydrous ethanol and saturated brine in turn, and allowed to stand and dry to obtain a modifier.
[0045] Example 3: Preparation of modified nano zinc oxide:
[0046] At room temperature, add 10.0 g of nano zinc oxide and 100 mL of water into a flask, stir at high speed for 15 min under a high shear mixer, add 5.5 g of silane coupling agent KH-570, continue stirring at high speed for 30 min under a high shear mixer, and after the reaction is complete, filter and vacuum dry to obtain modified nano zinc oxide.
[0047] Example 4: Preparation of modified nano zinc oxide:
[0048] At room temperature, add 20.0g of nano zinc oxide and 200mL of water into a flask, stir at high speed for 15min under a high shear mixer emulsifier, add 11.0g of silane coupling agent KH-570, continue stirring at high speed for 30min under a high shear mixer emulsifier, and after the reaction is completed, filter and vacuum dry to obtain modified nano zinc oxide.
[0049] Example 5: 45g of polypropylene resin, 6g of the modifier prepared in Example 1, 2g of antioxidant 1010, 5g of the modified nano zinc oxide prepared in Example 3 and 0.1g of dibenzoyl peroxide were stirred and mixed uniformly, added to a twin-screw extruder, melt blended, extruded, longitudinally stretched and transversely stretched into a film, then corona treated, rolled up, and slit to form a hydrophobic film.
[0050] Example 6: 50g of polypropylene resin, 9g of the modifier prepared in Example 2, 3g of antioxidant 264, 7.5g of the modified nano zinc oxide prepared in Example 4 and 0.2g of dibenzoyl peroxide were stirred and mixed uniformly, added to a twin-screw extruder, melt blended, extruded, longitudinally stretched and transversely stretched into a film, then corona treated, rolled up, and slit to form a hydrophobic film.
[0051] Example 7: 55g of polypropylene resin, 12g of the modifier prepared in Example 2, 4g of antioxidant 264, 10g of the modified nano zinc oxide prepared in Example 4 and 0.3g of dibenzoyl peroxide were stirred and mixed uniformly, added to a twin-screw extruder, melt blended, extruded, longitudinally stretched and transversely stretched into a film, then corona treated, rolled up, and slit to form a hydrophobic film.
[0052] Comparative Example 1: No modifier was added, and the remaining steps were the same as those in Example 7.
[0053] Comparative Example 2: Use a commercially available waterproof composite polypropylene film produced by Langfang Yimei Energy Saving Technology Co., Ltd.
[0054] Examples 5-7 and Comparative Examples 1-2 were made into corresponding shapes according to different test standards and the following performance tests were performed:
[0055] The tensile strength was determined using the national standard GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets";
[0056] Adopt national standard GB / T 1410-2006 "Test method for volume resistivity and surface resistivity of solid insulating materials"
[0057] The national standard GB / T 31402-2015 "Test method for antibacterial performance of plastic surfaces" was adopted, and the film method was used to detect the inhibitory effect on Escherichia coli and Staphylococcus aureus; the method is as follows: Escherichia coli or Staphylococcus aureus bacteria were inoculated on the plate culture medium, covered with a film and preserved for 24 hours, and then live bacteria were cultured; the parallel experimental results of the blank samples were compared to obtain the antibacterial rate of the sample;
[0058] Use a contact angle tester to measure the hydrophobic angle of the sample before and after being placed at room temperature for 30 days;
[0059] The measured results are shown in the following table:
[0060]
[0061] It can be seen from the above table that the antibacterial, hydrophobic, antistatic and mechanical properties of the film prepared in this embodiment are higher than those of the comparative example, and the performance is long-lasting and stable, which has important application value in the field of hydrophobic film technology.
[0062] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0063] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A hydrophobic film, characterized in that: The raw materials included are as follows in parts by weight: 45-55 parts of polypropylene resin, 6-12 parts of modifier, 2-4 parts of antioxidant, 5-10 parts of modified nano zinc oxide, and 0.1-0.3 parts of dibenzoyl peroxide; The modifier is prepared by the following steps: S1. In a three-necked flask, add cyanuric chloride, sodium hydroxide, triethylamine and toluene in sequence, mix well, stir at room temperature for 20 minutes, add pentafluorophenol, react at 50°C for 4 hours, and after the reaction is completed, filter, wash, dry, filter again, purify by column chromatography, and rotary evaporate to obtain intermediate 1; the ratio of cyanuric chloride, sodium hydroxide, triethylamine, toluene and pentafluorophenol is 19.6g:3.9g:30mL:50mL:18.4g; S2. At room temperature, allyl chloride, 1-nonylamine, toluene and triethylamine were mixed and stirred evenly under nitrogen protection, and reacted at 65°C for 6 hours. After the reaction was completed, the mixture was rotary evaporated, purified by column chromatography, and rotary evaporated to obtain intermediate 2; the ratio of allyl chloride, 1-nonylamine, toluene and triethylamine was 7.6 g:14.3 g:50 mL:15 mL; S3, at room temperature, under nitrogen protection, the intermediate 1, intermediate 2, triethylamine and toluene were mixed and stirred uniformly, reacted at 75°C for 8 hours, and after the reaction was completed, filtered, rotary evaporated, purified by column chromatography, and rotary evaporated to obtain intermediate 3; the ratio of intermediate 1, intermediate 2, triethylamine and toluene was 37.4g:33.2g:30mL:100mL; S4. Mix and stir the intermediate 3, iodomethane and N,N-dimethylformamide evenly, react at 80°C for 8h, and after sufficient reaction, distill under reduced pressure, wash, and stand to dry to obtain a modifier; the usage ratio of the intermediate 3, iodomethane and N,N-dimethylformamide is 62.5g:28.2g:150mL.
2. A hydrophobic film according to claim 1, characterized in that: The modified nano zinc oxide is prepared by the following steps: At room temperature, nano zinc oxide and water were mixed, stirred at high speed for 15 minutes in a high shear mixer emulsifier, γ-(methacryloyloxy)propyltrimethoxysilane was added, and the mixture was stirred at high speed for 30 minutes in a high shear mixer emulsifier. After the reaction was completed, the mixture was filtered and vacuum dried to obtain modified nano zinc oxide.
3. A hydrophobic film according to claim 2, characterized in that: The usage ratio of nano zinc oxide, water and γ-(methacryloyloxy)propyltrimethoxysilane is 10.0 g:100 mL:5.5 g.
4. The method for preparing a hydrophobic film according to claim 1, characterized in that: The following steps are involved: The polypropylene resin, modifier, antioxidant, modified nano zinc oxide and dibenzoyl peroxide are stirred and mixed evenly, added into a twin-screw extruder, melt blended, extruded, longitudinally stretched and transversely stretched into a film, and then corona treated, rolled up, and slit into a hydrophobic film.