High performance polyurethane vibration isolator and preparation method thereof
Embedding modified graphene into polyurethane material solves the problem of insufficient strength and acid and alkali resistance of polyurethane vibration isolators in harsh environments, significantly improves its mechanical properties and durability, extends its service life, and maintains noise reduction. Effect.
Patent Information
- Application Number
- CN202411000453.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Existing polyurethane vibration isolators have problems such as low tensile strength, weak acid and alkali resistance, and short service life in high and low temperature and salt spray corrosion environments.
Through modified graphene embedding technology, combined with polytetrahydrofuran diol, isocyanate and silane coupling agent, component A and component B are prepared, and a high-performance polyurethane vibration isolator is produced through a molding vulcanization process. Modified graphene is embedded In the polyurethane molecular chain, the mechanical properties and environmental resistance of the material are enhanced.
The tensile strength, wear resistance and acid and alkali resistance of the polyurethane vibration isolator are significantly improved, and the service life is extended. It can effectively cope with the challenges of harsh marine environments and maintain good noise reduction performance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the field of polyurethane vibration isolators, and in particular to a high-performance polyurethane vibration isolator and a preparation method thereof. Background Art
[0002] Polyurethane isolators are vibration-damping devices made of polyurethane materials, specially designed to absorb and isolate mechanical vibrations to protect the equipment and structures connected to them from vibration interference while reducing noise levels. In the field of marine resource development, especially in applications such as submarine cables, cable bend limiters, and marine equipment, polyurethane isolators are favored for their excellent wear resistance, water resistance, low temperature resistance, and good damping performance. These characteristics make polyurethane an ideal choice to replace traditional rubber isolators, especially in harsh marine environments such as high and low temperatures, salt spray corrosion, and long-term vibration.
[0003] Polyurethane vibration isolators can effectively absorb and attenuate vibrations generated during equipment operation, reduce noise transmission, and improve the quality of the working and living environments. They prevent vibrations from being transmitted to equipment and structures, reduce mechanical wear, and extend equipment life. They maintain stable vibration isolation performance in high and low temperature, humid, and corrosive environments.
[0004] In the development of marine resources, submarine cables, cable bend limiters, marine vibration isolators and other scenes urgently need materials with good performance such as wear resistance, water resistance, low temperature resistance, vibration reduction and noise reduction. At present, metal rubber vibration isolators are commonly used on ships. They have good vibration isolation effects under harsh working conditions such as high and low temperature environments, vibration environments, and salt spray corrosion environments. However, as the use time of rubber vibration isolators increases, material aging and performance degradation will occur, resulting in a shorter service life of rubber vibration isolators.
[0005] CN104231596A discloses a polyurethane elastomer material for vibration isolators and a preparation method thereof. The application uses polyisocyanate and polyether polyol as reaction raw materials, trihydroxymethylpropane monoallyl ether or glycerol α-allyl ether containing unsaturated double bonds as chain extenders to synthesize polyurethane raw rubber, uses the synthesized raw rubber as the matrix material, adds reinforcing fillers, sulfur and accelerators to the raw rubber system to obtain polyurethane mixed rubber, and then obtains low internal friction and high performance polyurethane elastomer material for vibration isolators by molding vulcanization. However, the vibration isolator made of the material disclosed in the application still has problems such as low tensile strength and weak acid and alkali resistance. Summary of the invention
[0006] In order to solve the problems of low strength, weak acid and alkali resistance and short service life of polyurethane vibration isolators in the prior art, the present application provides a high-performance polyurethane vibration isolator and a preparation method thereof. The present invention adopts modified graphene embedding technology to target the special needs of the field of marine resource development. The modified polyurethane vibration isolator exhibits excellent wear resistance and hydrolysis resistance, and can effectively cope with the challenges of harsh marine environment.
[0007] The present application provides a high-performance polyurethane vibration isolator, comprising component A and component B:
[0008] Among them, component A includes:
[0009] 30-60 parts of polytetrahydrofuran diol
[0010] Isocyanate 20-50 parts
[0011] Silane coupling agent 2-5 parts
[0012] Modified graphene 3-10 parts
[0013] Component B:
[0014] Chain extender 10-30 parts.
[0015] The present application also provides a method for preparing a high-performance polyurethane vibration isolator, comprising the following steps:
[0016] S1. Under mechanical stirring, concentrated sulfuric acid is added dropwise to a mixed solution of octamethylcyclotetrasiloxane and γ-chloropropylmethyldiethoxysilane monomers, and the temperature is raised to react after the addition is completed. After the reaction is completed, the chloropropyl polysiloxane is extracted with distilled water and dichloromethane, and the lower organic solution is collected. After repeated extractions, the collected organic solution is subjected to rotary evaporation to remove the solvent to obtain chloropropyl polysiloxane;
[0017] S2, adding sodium hydroxide solution to the graphene aqueous solution, dissolving the chloropropyl polysiloxane obtained in S1 in chloroform solution after stirring, then adding the above graphene-NaOH solution, ultrasonically dispersing, standing to collect the lower organic solution, and rotary evaporating the collected organic solution to remove the solvent to obtain polysiloxane-modified graphene;
[0018] S3, adding polytetrahydrofuran diol to a mixed solution of isocyanate, silane coupling agent and modified graphene obtained in step S2, heating and reacting to obtain component A;
[0019] S4. Mix component A and component B evenly, form them in a mold, demould them, and mature them to obtain a polyurethane vibration isolator.
[0020] Furthermore, the polytetrahydrofuran diol in step S3 is pretreated, vacuum-dehydrated at 100-120° C. for 1.5-2.0 h, and then cooled to 45-55° C., the reaction temperature is 70-80° C., and the reaction time is 2-2.5 h.
[0021] Furthermore, the NCO content of component A obtained in step S3 is 5 to 15 wt %.
[0022] Furthermore, in step S1, the mass ratio of the octamethylcyclotetrasiloxane and γ-chloropropylmethyldiethoxysilane monomers is 1-5:1, and the amount of concentrated sulfuric acid added is 10%-50% of the mass of the octamethylcyclotetrasiloxane and γ-chloropropylmethyldiethoxysilane monomers.
[0023] Furthermore, in step S2, the added mass of graphene is 20-50% of chloropropyl polysiloxane, and the concentration of the graphene aqueous solution is 1 mg / mL.
[0024] Furthermore, the polytetrahydrofuran diol described in step S3 has a mean molecular weight of 1000-2000, and the isocyanate is diphenylmethane diisocyanate.
[0025] Furthermore, the silane coupling agent described in step S3 is γ-aminopropyltriethoxysilane, and the chain extender is one or more of dimethylthiotoluene diamine, trimethylolpropane, and 1,4-butanediol.
[0026] Furthermore, in step S4, the mold temperature during molding is 80-90° C., the molding pressure is 5-10 MPa, the demoulding time is 20-30 min, the aging temperature is 75-90° C., and the aging time is 18-24 h.
[0027] Furthermore, the reaction temperature in step S1 is 55°C to 75°C, the reaction time is 5-7h, and the rotary evaporation temperature is 35 to 45°C.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] In the present invention, component A is made up of polytetrahydrofuran diol, isocyanate, silane coupling agent and modified graphene, and component B is chain extender. Polytetrahydrofuran diol gives material good elasticity as soft segment, and isocyanate reacts with it to form hard segment, providing necessary mechanical strength and hardness. The effect of silane coupling agent is to strengthen the interfacial bonding force between polyurethane and graphene, and chain extender is then used for regulating molecular weight and crosslinking degree, affects the physical properties of the finished product.
[0030] The present invention uses modified graphene to enhance the performance of polyurethane vibration isolators. By reacting and reducing graphene with chloropropyl polysiloxane, polysiloxane-modified graphene is obtained. This process not only enhances the dispersibility of graphene, but also embeds it uniformly into the polyurethane molecular chain through in-situ polymerization. Graphene, as a two-dimensional nanomaterial, is known for its extremely high strength, excellent conductivity and thermal stability, and can significantly improve the mechanical properties and environmental resistance of composite materials.
[0031] The introduction of modified graphene significantly improves the tensile strength and wear resistance of polyurethane vibration isolators. The high strength and two-dimensional layer structure of graphene form physical cross-linking points inside the material, effectively inhibiting crack propagation and improving the overall load-bearing capacity and durability of the material. Through modification, the good compatibility between graphene and the polyurethane matrix enhances the acid and alkali resistance of the vibration isolator. This is particularly important in marine environments, as it can resist seawater corrosion and extend service life.
[0032] The high damping properties of polyurethane itself, coupled with the addition of modified graphene, not only do not weaken but may improve the efficiency of absorbing mechanical vibrations due to the increase in the overall rigidity of the material, thereby more effectively reducing noise levels and protecting connected equipment from vibration damage.
[0033] The present invention successfully solves the problems of low strength and weak acid and alkali resistance of traditional polyurethane isolators through specific modified graphene embedding technology, and achieves significant improvements in mechanical properties, environmental resistance and service life. In response to the special needs of the field of marine resource development, the modified polyurethane isolators show excellent wear resistance and hydrolysis resistance, and can effectively cope with the challenges of harsh marine environments. The process is simple, conducive to large-scale production, ensuring the efficiency and repeatability of the preparation process, and is conducive to industrial production and cost control. DETAILED DESCRIPTION
[0034] The technical scheme of the present invention and its effects are further described below by specific examples. The following examples are only used to illustrate the content of the present invention and are not used to limit the protection scope of the present invention. Simple changes made to the present invention by applying the concept of the present invention are all within the scope of the protection claimed by the present invention.
[0035] The equipment used in the preparation method of the present invention can be the well-known equipment in the art. The raw materials used in the present invention are commercially available unless otherwise specified.
[0036] The raw materials used in the embodiment are as follows:
[0037] Industrial grade octamethylcyclotetrasiloxane D4 produced by Sigma-Aldrich (Shanghai) Trading Co., Ltd.;
[0038] Industrial-grade γ-chloropropylmethyldiethoxysilane YDH-701 produced by Sigma-Aldrich (Shanghai) Trading Co., Ltd.;
[0039] Polytetrahydrofuran diol Polytetrahydrofuran PTMG 1000 produced by BASF (China) Co., Ltd.;
[0040] Polytetrahydrofuran diol Polytetrahydrofuran PTMG 2000 produced by BASF (China) Co., Ltd.;
[0041] γ-aminopropyltriethoxysilane KH-550 produced by Jinan Huanzheng Chemical Co., Ltd.;
[0042] Graphene oxide produced by Xiamen Kaina Graphene Technology Co., Ltd.
[0043] Example 1
[0044] S1. Under mechanical stirring, 20 g of concentrated sulfuric acid was added dropwise to a mixed solution of 60 g of octamethylcyclotetrasiloxane and 40 g of γ-chloropropylmethyldiethoxysilane monomer. After the addition was completed, the system temperature was raised to 60°C and the reaction was carried out for 6 hours. After the reaction was completed, 25 mL of distilled water and 25 mL of dichloromethane were used to separate and extract the chloropropyl polysiloxane, the aqueous phase was removed, and the lower organic solution was collected by standing. The reaction was repeated three times, and the collected solution was subjected to rotary evaporation at 40°C to remove the solvent to obtain chloropropyl polysiloxane.
[0045] S2, add 20g of 0.1mol / L NaOH solution to 200g of 1mg / mL graphene aqueous solution to make it weakly alkaline, so that the oxygen-containing groups on the surface of graphene oxide are reacted. Dissolve 10g of chloropropyl polysiloxane obtained in S1 in 100g of chloroform solution, then add the above graphene-NaOH solution, ultrasonically disperse for 1h, let stand to collect the lower organic solution, and remove the solvent by rotary evaporation at 40°C to obtain polysiloxane-modified graphene.
[0046] S3, 30 parts of polytetrahydrofuran diol PTMG-1000 were vacuum dehydrated at 120°C for 1.5h, cooled to 55°C, added with 50 parts of MDI-100, 4 parts of KH-550 and 6 parts of modified graphene obtained in step S2, heated to 80°C and reacted for 2h to obtain a prepolymer with an NCO content of 7.5%, i.e. component A, and component B was 20 parts of dimethylthiotoluenediamine.
[0047] S4. Mix component A and component B evenly, pour them into the mold quickly, keep the mold at 85±5℃, react and mold under a pressure of 10MPa, demould after 30min, and then mature at 80℃ for 24h to obtain the polyurethane vibration isolator.
[0048] Example 2
[0049] S1. Under mechanical stirring, 24 g of concentrated sulfuric acid was added dropwise to a mixed solution of 200 g of octamethylcyclotetrasiloxane and 40 g of γ-chloropropylmethyldiethoxysilane monomer. After the addition was completed, the system temperature was raised to 55°C and the reaction was carried out for 7 hours. After the reaction was completed, 25 mL of distilled water and 25 mL of dichloromethane were used to separate and extract the chloropropyl polysiloxane, the aqueous phase was removed, and the lower organic solution was collected by standing. The process was repeated three times, and the collected solution was subjected to rotary evaporation at 35°C to remove the solvent to obtain chloropropyl polysiloxane.
[0050] S2, add 20g of 0.1mol / L NaOH solution to 200g of 1mg / mL graphene aqueous solution to make it weakly alkaline, so that the oxygen-containing groups on the surface of graphene oxide are reacted. Dissolve 10g of chloropropyl polysiloxane obtained in S1 in 100g of chloroform solution, then add the above graphene-NaOH solution, ultrasonically disperse for 1h, let stand to collect the lower organic solution, and remove the solvent by rotary evaporation at 40°C to obtain polysiloxane-modified graphene.
[0051] S3, vacuum dehydrate 30 parts of polytetrahydrofuran diol PTMG-1000 at 120 ° C for 1.5 hours, cool to 55 ° C, add 40 parts of MDI-100, 2 parts of KH-550 and 10 parts of modified graphene obtained in step S2, heat to 80 ° C and react for 2 hours to obtain a prepolymer with an NCO content of 7.5%, i.e. component A, and component B is 30 parts of dimethylthiotoluene diamine.
[0052] S4. Mix component A and component B evenly, pour them into the mold quickly, keep the mold at 85±5℃, react and mold under a pressure of 10MPa, demould after 30min, and then mature at 80℃ for 24h to obtain the polyurethane vibration isolator.
[0053] Example 3
[0054] S1. Under mechanical stirring, 40 g of concentrated sulfuric acid is added dropwise to a mixed solution of 40 g of octamethylcyclotetrasiloxane and 40 g of γ-chloropropylmethyldiethoxysilane monomer. After the addition is completed, the system temperature is raised to 75°C and the reaction is carried out for 5 hours. After the reaction is completed, the chloropropyl polysiloxane is subjected to liquid separation and extraction with 25 mL of distilled water and 25 mL of dichloromethane, the aqueous phase is removed, and the lower organic solution is collected by standing. The process is repeated three times, and the collected solution is subjected to rotary evaporation at 45°C to remove the solvent to obtain chloropropyl polysiloxane.
[0055] S2, add 20g of 0.1mol / L NaOH solution to 200g of 1mg / mL graphene aqueous solution to make it weakly alkaline, so that the oxygen-containing groups on the surface of graphene oxide are reacted. Dissolve 10g of chloropropyl polysiloxane obtained in S1 in 100g of chloroform solution, then add the above graphene-NaOH solution, ultrasonically disperse for 1h, let stand to collect the lower organic solution, and remove the solvent by rotary evaporation at 40°C to obtain polysiloxane-modified graphene.
[0056] S3, 60 parts of polytetrahydrofuran diol PTMG-1000 were vacuum dehydrated at 120°C for 1.5h, cooled to 55°C, added with 20 parts of MDI-100, 5 parts of KH-550 and 3 parts of modified graphene obtained in step S2, heated to 80°C and reacted for 2h to obtain a prepolymer with an NCO content of 7.5%, i.e. component A, and component B was 10 parts of dimethylthiotoluene diamine.
[0057] S4. Mix component A and component B evenly, pour them into the mold quickly, keep the mold at 85±5℃, react and mold under a pressure of 10MPa, demould after 30min, and then mature at 80℃ for 24h to obtain the polyurethane vibration isolator.
[0058] Example 4
[0059] S1. Under mechanical stirring, 20 g of concentrated sulfuric acid was added dropwise to a mixed solution of 60 g of octamethylcyclotetrasiloxane and 40 g of γ-chloropropylmethyldiethoxysilane monomer. After the addition was completed, the system temperature was raised to 60°C and the reaction was carried out for 6 hours. After the reaction was completed, 25 mL of distilled water and 25 mL of dichloromethane were used to separate and extract the chloropropyl polysiloxane, the aqueous phase was removed, and the lower organic solution was collected by standing. The reaction was repeated three times, and the collected solution was subjected to rotary evaporation at 40°C to remove the solvent to obtain chloropropyl polysiloxane.
[0060] S2, add 20g of 0.1mol / L NaOH solution to 200g of 1mg / mL graphene aqueous solution to make it weakly alkaline, so that the oxygen-containing groups on the surface of graphene oxide are reacted. Dissolve 10g of chloropropyl polysiloxane obtained in S1 in 100g of chloroform solution, then add the above graphene-NaOH solution, ultrasonically disperse for 1h, let stand to collect the lower organic solution, and remove the solvent by rotary evaporation at 40°C to obtain polysiloxane-modified graphene.
[0061] S3, 40 parts of polytetrahydrofuran diol PTMG-2000 were vacuum dehydrated at 110°C for 2h, and then the temperature was reduced by 50°C, 40 parts of MDI-100, 5 parts of KH-550 and 8 parts of modified graphene obtained in step S2 were added, and the temperature was raised to 75°C for reaction for 2h to obtain a prepolymer with an NCO content of 5%, i.e., component A, and component B was 20 parts of trimethylolpropane.
[0062] S4. Mix component A and component B evenly, pour them into the mold quickly, keep the mold at 85±5℃, react and mold under 8MPa pressure, demould after 30min, and then mature at 80℃ for 24h to obtain the polyurethane vibration isolator.
[0063] Example 5
[0064] S1. Under mechanical stirring, 20 g of concentrated sulfuric acid was added dropwise to a mixed solution of 60 g of octamethylcyclotetrasiloxane and 40 g of γ-chloropropylmethyldiethoxysilane monomer. After the addition was completed, the system temperature was raised to 60°C and the reaction was carried out for 6 hours. After the reaction was completed, 25 mL of distilled water and 25 mL of dichloromethane were used to separate and extract the chloropropyl polysiloxane, the aqueous phase was removed, and the lower organic solution was collected by standing. The reaction was repeated three times, and the collected solution was subjected to rotary evaporation at 40°C to remove the solvent to obtain chloropropyl polysiloxane.
[0065] S2, add 20g of 0.1mol / L NaOH solution to 200g of 1mg / mL graphene aqueous solution to make it weakly alkaline, so that the oxygen-containing groups on the surface of graphene oxide are reacted. Dissolve 10g of chloropropyl polysiloxane obtained in S1 in 100g of chloroform solution, then add the above graphene-NaOH solution, ultrasonically disperse for 1h, let stand to collect the lower organic solution, and remove the solvent by rotary evaporation at 40°C to obtain polysiloxane-modified graphene.
[0066] S3, vacuum dehydrate 40 parts of polytetrahydrofuran diol PTMG-2000 at 100°C for 2h, cool to 45°C, add 50 parts of MDI-100, 2 parts of KH-550 and 3 parts of modified graphene obtained in step S2, heat to 70°C and react for 2.5h to obtain a prepolymer with an NCO content of 5%, i.e. component A, and component B is 20 parts of 1,4-butanediol.
[0067] S4. Mix component A and component B evenly, pour them into the mold quickly, keep the mold at 85±5℃, react and mold under a pressure of 5MPa, demould after 30min, and then mature at 80℃ for 24h to obtain a polyurethane vibration isolator.
[0068] Comparative Example 1
[0069] S1. Preparation of components A and B: by weight, 30 parts of polytetrahydrofuran diol were vacuum dehydrated at 120° C. for 1.5 h, cooled to 55° C., and then 50 parts of MDI-100, 4 parts of KH-550 and 6 parts of graphene were added, and the temperature was raised to 80° C. for reaction for 2 h to obtain a prepolymer with an NCO content of 7.5%, i.e., component A. Component B is 20 parts of dimethylthiotoluenediamine;
[0070] S2. Mix component A and component B evenly, pour them into the mold quickly, keep the mold at 85±5℃, react and mold under a pressure of 10MPa, demould after 30min, and then mature at 80℃ for 24h to obtain the polyurethane vibration isolator.
[0071] Comparative Example 2
[0072] S1. Preparation of modified graphene: Mix isopropyl triisostearoyl titanate, water and anhydrous ethanol in a mass ratio of 1:1:20, add glacial acetic acid to adjust the pH value to 3-5, then add 50% TTS graphene oxide, react at 80°C for 24 hours, then add sodium borohydride with a mass 20 times that of graphene oxide, and react at 60°C for 24 hours. After the reaction is completed, filter the reaction product, wash the filter cake three times with secondary water, collect the obtained black substance, and vacuum dry the product overnight to obtain modified graphene.
[0073] S2. Vacuum dehydrate 30 parts of polytetrahydrofuran diol at 120°C for 1.5h, cool to 55°C, add 50 parts of MDI-100, 4 parts of KH-550 and 6 parts of modified graphene, heat to 80°C and react for 2h to obtain a prepolymer with an NCO content of 7.5%, i.e. component A, and component B is 10 parts of dimethylthiotoluene diamine.
[0074] S3. Mix component A and component B evenly, pour them into the mold quickly, keep the mold at 85±5℃, react and mold under a pressure of 10MPa, demould after 30min, and then mature at 80℃ for 24h to obtain the polyurethane vibration isolator.
[0075] Comparative Example 3
[0076] S1. Under mechanical stirring, 20 g of concentrated sulfuric acid was added dropwise to a mixed solution of 60 g of octamethylcyclotetrasiloxane and 40 g of γ-chloropropylmethyldiethoxysilane monomer. After the addition was completed, the system temperature was raised to 60°C and the reaction was carried out for 6 hours. After the reaction was completed, 25 mL of distilled water and 25 mL of dichloromethane were used to separate and extract the chloropropyl polysiloxane, the aqueous phase was removed, and the lower organic solution was collected by standing. The reaction was repeated three times, and the collected solution was subjected to rotary evaporation at 40°C to remove the solvent to obtain chloropropyl polysiloxane.
[0077] S2, add 20g of 0.1mol / L NaOH solution to 200g of 1mg / mL graphene aqueous solution to make it weakly alkaline, so that the oxygen-containing groups on the surface of graphene oxide are reacted. Dissolve 10g of chloropropyl polysiloxane obtained in S1 in 100g of chloroform solution, then add the above graphene-NaOH solution, ultrasonically disperse for 1h, let stand to collect the lower organic solution, and remove the solvent by rotary evaporation at 40°C to obtain polysiloxane-modified graphene.
[0078] S3, 30 parts of polytetrahydrofuran diol PTMG-1000 were vacuum dehydrated at 120°C for 1.5h, cooled to 55°C, added with 40 parts of MDI-100, 4 parts of KH-550 and 15 parts of modified graphene obtained in step S2, heated to 80°C and reacted for 2h to obtain a prepolymer with an NCO content of 5%, i.e. component A, and component B was 20 parts of dimethylthiotoluenediamine.
[0079] S4. Mix component A and component B evenly, quickly pour them into a mold, keep the mold at 85±5°C, react and mold under a pressure of 10MPa, demould after 30 minutes, and then mature at 80°C for 24 hours to obtain a polyurethane vibration isolator. The polyurethane vibration isolators prepared in Examples 1-5 and Comparative Examples 1-3 were tested for performance; the test results are shown in the following table.
[0080]
[0081]
[0082] The Shore A hardness is tested according to GB / T531.1-2008 standard.
[0083] The tensile strength and elongation are tested according to GB / T528-1998 standard.
[0084] Akron abrasion test is carried out according to GB / T 1689-2014 standard.
[0085] Acid and alkali resistance was tested according to GB / T 13353-92 standard. 10% sulfuric acid solution and 10% sodium hydroxide solution were selected. The samples were immersed for 7 days respectively and then taken out to test the mechanical properties and mass change rate.
[0086] Hydrolysis resistance test steps: hang the sample in a constant temperature and humidity chamber for humid heat aging, with a constant temperature of 70℃±2℃ and a relative humidity of more than 95%. After 3 weeks of humid heat treatment, take out the test piece and place it at a temperature of 23℃±2℃ and a relative humidity of 45%~55% for 2 hours to test the performance of the sample.
[0087] Compared with Example 1, Comparative Example 1 does not add polysiloxane-modified graphene, but adds an equal amount of graphene instead. Compared with Example 1, Comparative Example 2 does not add polysiloxane-modified graphene, but adds an equal amount of triisostearoyl titanate isopropyl modified graphene oxide instead. Compared with Example 2, Comparative Example 3 adds 15 parts of polysiloxane-modified graphene instead. It can be seen that the polyurethane vibration isolator obtained in the comparative example is not as good as the polyurethane vibration isolator obtained in the example in terms of hardness, tensile strength, Akron abrasion, acid and alkali resistance, and hydrolysis resistance.
Claims
1. A high performance polyurethane vibration isolator, characterized in that: Including component A and component B: Among them, component A includes: 30-60 parts of polytetrahydrofuran diol 20-50 parts of diphenylmethane diisocyanate Silane coupling agent 2-5 parts 3 to 10 parts of polysiloxane-modified graphene; Component B: 10-30 parts of chain extender; The preparation method of the polysiloxane-modified graphene is: A sodium hydroxide solution is added to the graphene aqueous solution, and after stirring, chloropropyl polysiloxane is dissolved in a chloroform solution, and then the graphene-NaOH solution is added, ultrasonic dispersion is performed, and the lower organic solution is collected by standing, and the collected organic solution is subjected to rotary evaporation to remove the solvent to obtain polysiloxane-modified graphene; The graphene is graphene oxide.
2. The method for preparing the high-performance polyurethane vibration isolator according to claim 1, characterized in that: The following steps are involved: S1. Under mechanical stirring, concentrated sulfuric acid is added dropwise to a mixed solution of octamethylcyclotetrasiloxane and γ-chloropropylmethyldiethoxysilane monomers, and the temperature is raised to react after the addition is completed. After the reaction is completed, the chloropropyl polysiloxane is extracted with distilled water and dichloromethane, and the lower organic solution is collected. After repeated extractions, the collected organic solution is subjected to rotary evaporation to remove the solvent to obtain chloropropyl polysiloxane; S2, adding sodium hydroxide solution to the graphene aqueous solution, dissolving the chloropropyl polysiloxane obtained in S1 in chloroform solution after stirring, then adding the above graphene-NaOH solution, ultrasonically dispersing, standing to collect the lower organic solution, and rotary evaporating the collected organic solution to remove the solvent to obtain polysiloxane-modified graphene; S3, adding polytetrahydrofuran diol to a mixed solution of diphenylmethane diisocyanate, a silane coupling agent and the polysiloxane-modified graphene obtained in step S2, and heating the mixture to react to obtain component A; S4. Mix component A and component B evenly, form them in a mold, demould them, and mature them to obtain a polyurethane vibration isolator.
3. The method for preparing the high-performance polyurethane vibration isolator according to claim 2, characterized in that: The polytetrahydrofuran diol described in step S3 is pre-treated, vacuum-dehydrated at 100-120° C. for 1.5-2.0 h, and then cooled to 45-55° C., the reaction temperature is 70-80° C., and the reaction time is 2-2.5 h.
4. The method for preparing the high-performance polyurethane vibration isolator according to claim 2, characterized in that: The NCO content of component A obtained in step S3 is 5 to 15 wt %.
5. The method for preparing the high-performance polyurethane vibration isolator according to claim 2, characterized in that: In step S1, the mass ratio of octamethylcyclotetrasiloxane and γ-chloropropylmethyldiethoxysilane monomers is 1-5:1, and the amount of concentrated sulfuric acid added is 10%-50% of the mass of octamethylcyclotetrasiloxane and γ-chloropropylmethyldiethoxysilane monomers.
6. The method for preparing the high-performance polyurethane vibration isolator according to claim 2, characterized in that: The added mass of the graphene in step S2 is 20-50% of the chloropropyl polysiloxane, and the concentration of the graphene aqueous solution is 1 mg / mL.
7. The method for preparing the high-performance polyurethane vibration isolator according to claim 2, characterized in that: The polytetrahydrofuran diol mean molecule amount of step S3 is 1000 ~ 2000.
8. The method for preparing the high-performance polyurethane vibration isolator according to claim 2, characterized in that: The silane coupling agent described in step S3 is γ-aminopropyltriethoxysilane, and the chain extender is one or more of dimethylthiotoluene diamine, trimethylolpropane, and 1,4-butanediol.
9. The method for preparing the high-performance polyurethane vibration isolator according to claim 2, characterized in that: The mold temperature during molding in step S4 is 80-90° C., the molding pressure is 5-10 MPa, the demoulding time is 20-30 min, the aging temperature is 75-90° C., and the aging time is 18-24 h.
10. The method for preparing the high-performance polyurethane vibration isolator according to claim 2, characterized in that: The reaction temperature in step S1 is 55°C to 75°C, the reaction time is 5-7h, and the rotary evaporation temperature is 35 to 45°C.