A high weather-resistant masterbatch for colored polyester and its preparation method and application

By using special polyesters with high viscosity and low-end carboxyl content, composite antioxidants and composite light stabilizers in colored polyesters, combined with triazine UV absorbers and fumed silica, the compound stabilizers formed solve the problem of color The problem of insufficient weather resistance of polyester materials is achieved by achieving high weather resistance and color stability of the material.

CN118530570BActive Publication Date: 2024-10-18POLY PLASTIC MASTERBATCH SUZHOU
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411008311.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-18
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Existing colored polyester products have limitations in terms of high weather resistance, especially due to their complex composition and the sensitivity of dyes to pH, which results in limited effectiveness of existing anti-aging methods and difficulty in achieving high weather resistance.

Method used

A highly weather-resistant masterbatch for colored polyester is used, including special polyester with high viscosity and low-end carboxyl content, composite antioxidants and composite light stabilizers, through the combination of primary antioxidants, auxiliary antioxidants and free radical scavengers. , using triazine UV absorbers and triazine hindered amines, combined with fumed silica adsorbents, to form a compound stabilizer to improve the weather resistance of polyester materials.

Benefits of technology

It significantly improves the weather resistance of colored polyester materials during thermal processing and long-term use, reduces the effects of photoaging and thermal degradation, maintains the color stability and performance of the material, and is suitable for the preparation of colored polyester fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118530570B_ABST
    Figure CN118530570B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of polymer materials, and relates to a highly weather-resistant masterbatch for colored polyester, and a preparation method and application thereof. The highly weather-resistant masterbatch for colored polyester comprises a polyester resin, a compound stabilizer and a dispersant; the characteristic viscosity of the polyester resin is 0.95-1.05dl / g, and the terminal carboxyl content is ≤15mol / t; the compound stabilizer comprises a composite antioxidant and a composite light stabilizer by weight; the composite antioxidant comprises a primary antioxidant, an auxiliary antioxidant and a free radical scavenger; the composite light stabilizer comprises a triazine ultraviolet absorber and a triazine hindered amine; the preparation method comprises mixing the components, melt-extruding, drawing, and pelletizing to obtain a highly weather-resistant masterbatch for colored polyester; the application is to use the highly weather-resistant masterbatch for colored polyester of the present invention to prepare polyester fibers. The colored polyester products (polyester fibers) prepared using the highly weather-resistant masterbatch for colored polyester of the present invention have good weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a highly weather-resistant masterbatch for colored polyester and a preparation method and application thereof. Background Art

[0002] Polyester materials represented by polyethylene terephthalate (PET) are a type of engineering plastics with excellent performance and wide applications. As a crystalline saturated polyester resin, PET's high crystallinity, rigid groups containing a large number of benzene rings, and inert chemical structure together give PET materials good fatigue resistance, abrasion resistance, and chemical resistance while maintaining high transparency. In addition, PET materials not only have excellent fiber-forming properties and are easy to process into high-strength fibers, but also have excellent film-forming properties and can form films with high transparency and stable performance. These characteristics, coupled with its low cost, make PET one of the largest varieties of chemical fibers.

[0003] However, the high crystallinity and rigid structure of PET also lead to low dyeing efficiency, serious pollution, and great pressure on environmental protection. The masterbatch method for liquid dyeing can reduce the amount of dyes used to a certain extent and reduce pollution during the dyeing process. Therefore, more and more colored polyester products are dyed with masterbatch method.

[0004] At present, it is difficult for solution-dyed colored polyester products to achieve high weather resistance. The main reasons are as follows:

[0005] 1. Polyester stock solution coloring is a high-concentration colorant dispersion obtained by melt-mixing excess colorant with polyester. Therefore, the performance of the colorant and polyester will deteriorate during the thermal processing.

[0006] 2. Esterification reaction is a reversible reaction. During the processing and long-term use of polyester materials, the ester bonds will be hydrolyzed, resulting in the breakage of the polymer main chain and the generation of terminal carboxyl and terminal hydroxyl products. These hydrolysis products will be further oxidized by the light, heat, water and air in the environment, greatly affecting the appearance and color of polyester products.

[0007] 3. PET is seriously affected by light aging. The carbonyl group in it can be destroyed by sunlight. The breakage of carbonyl group causes photodegradation or cross-linking reaction of PET. The latter will further affect the distribution of crystalline and amorphous phases of polyester products, increase the crystallinity and make the material brittle.

[0008] 4. The metal ions in the catalyst remaining during the polyester synthesis process and the metal ions remaining during the purification of the colorant will catalyze and accelerate the photoaging process.

[0009] At present, the common methods used to improve the weather resistance of ordinary polyester products are as follows:

[0010] 1. Improve hydrolysis resistance: By adding carbodiimide or some alkaline substances to neutralize the terminal carboxyl substances generated in the hydrolysis process, the further hydrolysis of the ester bond can be inhibited, thereby improving the anti-aging performance of polyester products.

[0011] 2. Utilize the extinction effect: By adding high-refractive-index inorganic powders such as titanium dioxide, strong light reflection is formed on the fiber surface after exposure to sunlight, reducing the effects of light aging on polyester itself.

[0012] 3. Adding photostabilizers: Adding photostabilizers represented by UV absorbers can interrupt the various processes in the photooxidation chain reaction by absorbing high-energy rays, capturing and quenching free radicals, so as to slow down the occurrence of photoaging.

[0013] 4. Add antioxidants.

[0014] However, although the above-mentioned means of improving weather resistance are widely used in ordinary polyester products, due to the complex and diverse components of colored polyester products, the method of only anti-aging treatment for the polymer itself has significant limitations, and its effect is relatively limited. For example, when using alkaline substances to inhibit hydrolysis, the alkali is also a catalyst for the esterification reaction. Therefore, this type of anti-hydrolysis agent has the defect of a low upper limit of addition. At the same time, most of the dyes used in colored polyester products are sensitive to pH values. Alkaline substances will change the color of the dyes and even react with each other, which is risky to use in colored polyester products. Matting yarn has a high titanium dioxide content and strong hiding power, which significantly affects the color development of colorants in colored polyester products. The light stabilizer scheme currently used in the market has not been formulated for the characteristics of colored polyester products themselves. Therefore, the amount of general light stabilizer added is large, and the effect is general. There is also a darker base color, which affects actual use. In addition, in actual production, many colored high weather-resistant products contain carbon black to adjust the hue or configure gray, black and other colors. However, carbon black particles have a large specific surface area, and the surface often adsorbs a certain amount of organic matter and heavy metal ions. These adsorbed substances will produce a certain degree of free radicals. Free radicals are one of the main factors that cause thermal degradation of polyester. At the same time, the heavy metal ions in carbon black will accelerate the aging of polyester under the synergistic effect of carbon black's light absorption effect, making it difficult for light gray polyester products to achieve a high level of weather resistance.

[0015] Therefore, it is of great significance to study a high weather-resistant masterbatch for colored polyester and its preparation method in view of the composition and structural characteristics of colored polyester products to solve the above problems. Summary of the invention

[0016] The purpose of the present invention is to solve the problems existing in the prior art and provide a highly weather-resistant masterbatch for colored polyester and a preparation method and application thereof.

[0017] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0018] A highly weather-resistant masterbatch for colored polyester, comprising, by weight, 65-70 parts of polyester resin, 30-34.5 parts of compound stabilizer, and 0.1-0.5 parts of dispersant (e.g., Tegomer P121);

[0019] The polyester resin is a special polyester with high viscosity and low terminal carboxyl content. The intrinsic viscosity of the polyester resin is 0.95-1.05dl / g, the terminal carboxyl content is ≤15mol / t, and the ash content is ≤0.01wt%;

[0020] By weight, the compound stabilizer includes 30-40 parts of compound antioxidant and 55-65 parts of compound light stabilizer;

[0021] Composite antioxidants include primary antioxidants, secondary antioxidants, and free radical scavengers;

[0022] Composite light stabilizers include triazine UV absorbers and triazine hindered amines.

[0023] The high-viscosity and low-end carboxyl content special polyester selected in the present invention can reduce polyester degradation during the thermal processing when manufacturing polyester masterbatch, reduce the impact of viscosity reduction caused by screw shearing, make the obtained weather-resistant masterbatch keep the physical properties close to those of conventional polyester chips, and avoid the adverse effects of using alkaline anti-hydrolysis agents.

[0024] The main purpose of the current mainstream technology in selecting antioxidants is to inhibit the thermal degradation of polyester during thermal processing and protect its color; therefore, a single antioxidant (such as hindered phenol) or a combination of a primary antioxidant and a secondary antioxidant (such as hindered phenol + phosphite) is often used. However, in colored polyester products, especially colored polyester masterbatches, the proportion of color pigments is relatively large, so the thermal protection of colorants cannot be ignored. In addition, due to the catalytic effect of colorants, polymer thermal degradation will be aggravated, which makes the protection effect of additives used in the existing technical route poor, and it is difficult to fully demonstrate the characteristics of highly weather-resistant colorants.

[0025] The compound antioxidant of the present invention includes a primary antioxidant, a secondary antioxidant, and a free radical scavenger, which can synergistically further inhibit the performance degradation of polyester masterbatch during thermal processing. The present invention is committed to maintaining the stability of intermediate products at each stage of the chain reaction of polyester materials being thermally cracked into free radicals or oxidized into peroxides, and can minimize thermal degradation and aging during processing. The free radical scavenger can be used as a first-stage protection to quench alkyl free radicals at the beginning of the thermal degradation chain reaction to terminate the aging reaction, the primary antioxidant can be used as a second-stage protection to quench hydroxyl free radicals and peroxy free radicals generated by the reaction of alkyl free radicals with oxygen / water and generate quinone products, and the secondary antioxidant can reduce the quinone products generated by the primary antioxidant to reduce the overall color pollution of the product while allowing the primary antioxidant to play its role again.

[0026] Due to the wide variety of polyester products and the complex photoaging process, the current mainstream technology generally uses single-spectrum UV absorbers for basic protection when selecting photoaging additives. For example, the commonly used triazole UV absorbers have absorption capabilities throughout the entire UV spectrum. They compete with polyester products to absorb high-energy UV rays and convert them into heat dissipation, thereby achieving the effect of protecting polymer materials. However, due to the poor long-term stability of the five-membered ring structure of triazole UV absorbers, after polyester products are exposed to high-duration radiation, their absorption performance will gradually decrease, resulting in a weakened protective effect. In a few cases, a UV absorber is combined with a hydrophobic hindered amine containing a long carbon chain (such as UV 5050H) for protection; when the protective effect of the UV absorber fails or is insufficient, this combination can effectively terminate the aging chain reaction by quenching the free radicals generated by the polyester under the action of light; due to the incompatibility of the long carbon chain and polyester, this method reduces the contact between the basic group in the hindered amine and the polyester, thereby reducing the potential impact on the rupture of the ester bond; however, this incompatibility also leads to poor dispersion of the long carbon chain hindered amine in polyester products. Both of the above solutions are not suitable for colored high weather-resistant polyester products.

[0027] The composite light stabilizer of the present invention comprises a triazine ultraviolet absorber and a triazine hindered amine. The triazine group can achieve long-term protection due to its own high stability, thereby meeting the product requirements of long-term use of colored high weather-resistant polyester. The triazine hindered amine is a large molecular weight, low alkalinity hindered amine, has low reaction activity with ester bonds, good migration resistance, will not precipitate during polyester processing, does not promote polyester degradation, and does not destroy the strength of polyester products; therefore, in the case of low addition, the triazine ultraviolet absorber can simultaneously provide good weathering protection for polyester products and color colorants, and further reduce the influence of the auxiliary agent on the color, and reduce the occurrence of color staining. When the triazine hindered amine is used alone, it also has the problem of general dispersibility in polyester, but the composite light stabilizer also contains a triazine ultraviolet absorber, and the triazine ultraviolet absorber and the triazine hindered amine have better compatibility, can disperse each other, and then be evenly distributed in the polyester product, and further achieve a synergistic protection effect in the polymer to fully demonstrate the auxiliary agent's anti-light aging effect on the colored polyester product.

[0028] As the preferred technical solution:

[0029] The high weather-resistant masterbatch for colored polyester as described above, wherein the main antioxidant is one or more of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N'-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl] propionyl hydrazide, bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid][oxalylbis(azanediyl)]bis(ethane-2,1-diyl) ester.

[0030] The preferred primary antioxidant of the present invention is different from the commonly used hindered phenol auxiliary agents (such as pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) in traditional polyesters. In addition to containing hindered phenol groups that can stabilize peroxy radical products, the primary antioxidant also has an oxalamide or hydrazide structure. These structures have multiple continuous metal ion coordination sites and can chelate metal ions. According to the composition characteristics of colored polyester products, the catalytic activity of metal ions introduced in each link is effectively reduced, thereby reducing the aging effect of residual metal ions on colored polyester products. In colored polyester products containing carbon black, the preferred primary antioxidant acts as a free radical scavenger, which can effectively neutralize free radical substances (hydroxyl radicals) adsorbed by carbon black, and can also chelate metal ions in carbon black.

[0031] In the highly weather-resistant masterbatch for colored polyester as described above, the auxiliary antioxidant is one or more of tris(2,4-di-tert-butyl)phenyl phosphite, bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite, and 3,9-bis(2,4-dicumylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane.

[0032] In the highly weather-resistant masterbatch for colored polyester as described above, the free radical scavenger is 5,7-di-tert-butyl-3-(3,4-dimethylphenyl)benzofuran-2(3H)-one.

[0033] In the highly weather-resistant masterbatch for colored polyester as described above, the triazine ultraviolet absorber is one or more of 2,4-bis(2,4-xylyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, 2-(4,6-diphenyl-1,3,5-triazine-2)-5-n-hexyloxyphenol, 2,4-bis(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine, 2,4-bis[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxybenzene)-1,3,5-triazine, and 2,4,6-tris(4'-butoxy-2'-hydroxyphenyl)-triazine. The triazine ultraviolet absorber can be a long-wave absorber or a short-wave absorber. The long-wave absorber and the short-wave absorber can be used in combination to achieve comprehensive coverage of the entire ultraviolet light region, improve absorption efficiency, and further improve the protection effect.

[0034] The existing technology mainly applies 2,4-di[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxybenzene)-1,3,5-triazine and 2,4,6-tris(4'-butoxy-2'-hydroxyphenyl)-triazine to optical barrier films, but not to polyester.

[0035] In the highly weather-resistant masterbatch for colored polyester as described above, the triazine hindered amine is one or more of poly[N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-CO-2,4-dichloro-6-morpholine-1,3,5-triazine], methylated polymer of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine and morpholine-2,4,6-trichloro-1,3,5-triazine, and reaction product of N,N''-1,2-ethanediyldi(1,3-propylenediamine) with cyclohexane and peroxide N-butyl-2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine.

[0036] The prior art does not apply poly[N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-CO-2,4-dichloro-6-morpholine-1,3,5-triazine] and methylated polymer of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine and morpholine-2,4,6-trichloro-1,3,5-triazine to polyester. Generally, the reaction product of N,N''-1,2-ethanediyldi(1,3-propylenediamine) with cyclohexane and peroxide N-butyl-2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine is used as a flame retardant.

[0037] The highly weather-resistant masterbatch for colored polyester as described above, in parts by weight, the compound stabilizer also includes 3-5 parts of adsorbent.

[0038] The highly weather-resistant masterbatch for colored polyester as described above, wherein the adsorbent is fumed silica, preferably high specific surface area fumed silica, with a BET specific surface area of ​​≥350 m 2 / g.

[0039] The preparation process of the high weather-resistant masterbatch for colored polyester as described above and the compound stabilizer is as follows: after mixing the composite antioxidant, the composite light stabilizer, the adsorbent and the organic solvent (such as dichloromethane), stirring evenly and removing the organic solvent, the compound stabilizer is obtained, and the mass of the organic solvent is 0.1-0.5 times the total mass of the composite antioxidant, the composite light stabilizer and the adsorbent.

[0040] The present invention mixes the components of the compound stabilizer with an organic solvent to achieve pre-dispersion of the compound stabilizer, thereby improving its stability during subsequent processing; in order to enhance the pre-dispersion effect, we try to select chemical substances with similar structures and polarities to form the compound stabilizer. During the pulping process, part of the compound stabilizer can be dissolved in the organic solvent, so that the components of the compound stabilizer reach a eutectic state, thereby enhancing the synergy of the compound stabilizer in protecting colored polyester products during processing and use; among them, high specific surface area fumed silica is used as a preferred adsorbent, which can effectively adsorb the eutectic compound stabilizer, further enhancing the effect of the compound stabilizer in improving weather resistance in the masterbatch.

[0041] The high weather-resistant masterbatch for colored polyester as described above has an intrinsic viscosity of 0.5710-0.6381 dl / g.

[0042] The present invention also provides a method for preparing a highly weather-resistant masterbatch for colored polyester as described in any of the above items, wherein the components are uniformly mixed in proportion, melt-extruded, drawn into strips, and pelletized to obtain the highly weather-resistant masterbatch for colored polyester.

[0043] The present invention also provides an application of a highly weather-resistant masterbatch for colored polyester as described in any one of the above items, which is used for preparing polyester fibers, and the addition amount is 0.1-10wt%.

[0044] Beneficial effects:

[0045] The present invention selects special polyester with high viscosity and low terminal carboxyl content to reduce polyester degradation during thermal processing when manufacturing polyester masterbatch, so that the obtained weather-resistant masterbatch has physical properties close to those of conventional polyester chips, and avoids the adverse effects of using alkaline anti-hydrolysis agents.

[0046] The compound antioxidant of the invention comprises a primary antioxidant, a secondary antioxidant and a free radical scavenger, which can synergistically inhibit the performance degradation of polyester masterbatch during thermal processing and reduce thermal degradation and aging to the greatest extent.

[0047] The composite light stabilizer of the present invention comprises a triazine ultraviolet absorber and a triazine hindered amine, the triazine group has high stability, can provide long-term protection, and meets the long-term use requirements of colored high weather-resistant polyester. The triazine ultraviolet absorber and the triazine hindered amine have good compatibility and can be evenly distributed in polyester products to achieve synergistic protection.

[0048] The colored polyester product (polyester fiber) prepared by using the high weather-resistant masterbatch for colored polyester of the present invention has good weather-resistant performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1The graph is a graph of the ultraviolet absorbance of different triazine ultraviolet absorbers in the present invention; in the graph, "1164" is 2,4-bis(2,4-xylyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, "1577" is 2-(4,6-diphenyl-1,3,5-triazine-2)-5-n-hexyloxyphenol, "1600" is 2,4-bis(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine, "460" is 2,4-bis[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxybenzene)-1,3,5-triazine, and "3480" is 2,4,6-tris(4'-butoxy-2'-hydroxyphenyl)-triazine;

[0050] Figure 2 It is the ultraviolet absorbance curve diagram of different triazine ultraviolet absorber combinations in the present invention. DETAILED DESCRIPTION

[0051] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0052] The following are the test methods for the relevant performance indicators in each embodiment and comparative example:

[0053] Intrinsic viscosity: tested according to GB / T 14190-2017 standard.

[0054] △E, color card grade: tested according to AATCC16.3 standard.

[0055] UV spectrum test: dissolve triazine UV absorber (single product or combination of various single products) in chloroform to obtain a chloroform solution with a concentration of 10 mg / L and use it as the test sample. Use chloroform as the reference sample and measure the 280-400nm UV-visible light absorbance curve.

[0056] Example 1

[0057] A method for preparing a highly weather-resistant masterbatch for colored polyester, the specific steps are as follows:

[0058] (1) Preparation of raw materials;

[0059] Composite antioxidant: a mixture of a primary antioxidant, a secondary antioxidant and a free radical scavenger in a mass ratio of 5:7.33:1, wherein the primary antioxidant is a mixture of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N'-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl] propionyl hydrazide and bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid][oxalylbis(azanediyl)]bis(ethane-2,1-diyl) ester in a mass ratio of 1:1, the secondary antioxidant is 3,9-bis(2,4-dicumylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and the free radical scavenger is 5,7-di-tert-butyl-3-(3,4-dimethylphenyl)benzofuran-2(3H)-one;

[0060] Composite light stabilizer: a mixture of a triazine UV absorber and a triazine hindered amine in a mass ratio of 1.75:1, the triazine UV absorber is a mixture of 2,4-di(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine and 2,4,6-tri(4'-butoxy-2'-hydroxyphenyl)-triazine in a mass ratio of 1:1.5, and the triazine hindered amine is the reaction product of N,N''-1,2-ethanediylbis(1,3-propylenediamine) with cyclohexane and peroxide N-butyl-2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine (manufacturer is BASF, model number is Flamestab NOR 116);

[0061] Adsorbent: fumed silica, manufactured by Cabot Corporation, model CLARUS 3160;

[0062] Organic solvent: dichloromethane;

[0063] Polyester resin: The manufacturer is Jiangsu Solide New Materials Group Co., Ltd., the variety is glossy tackified polyester chips, the intrinsic viscosity is 0.95-1.05dl / g, and the terminal carboxyl content is ≤15mol / t;

[0064] Dispersant: Tegomer P121, manufactured by Evonik Industries;

[0065] (2) preparing a compound stabilizer;

[0066] By weight, 40 parts of a composite antioxidant, 55 parts of a composite light stabilizer, 5 parts of an adsorbent and an organic solvent are mixed, stirred evenly, and the organic solvent is removed to obtain a composite stabilizer; wherein the amount of the organic solvent added is 0.1 times the total mass of the composite antioxidant, the composite light stabilizer and the adsorbent;

[0067] (3) Preparation of highly weather-resistant masterbatch for colored polyester;

[0068] By weight, 69.5 parts of polyester resin, 30 parts of compound stabilizer and 0.5 parts of dispersant are mixed evenly and put into a twin-screw extruder for melt extrusion, strip drawing and pelletizing to obtain high weather-resistant masterbatch for colored polyester; wherein, the temperature of zone 1 of the twin-screw extruder is 220°C, the temperature of zone 2 is 275°C, the temperature of zone 3 is 275°C, the temperature of zone 4 is 270°C, the temperature of zone 5 is 220°C, the temperature of zone 6 is 220°C, the temperature of zone 7 is 240°C, and the temperature of zone 8 is 260°C; the speed of the twin-screw extruder is 300r / min.

[0069] The intrinsic viscosity of the finally obtained high weather-resistant masterbatch for colored polyester is 0.6310 dl / g.

[0070] A method for preparing colored polyester fiber, the specific process is: according to weight parts, 1 part of the high weather-resistant masterbatch for colored polyester prepared in this embodiment, 10 parts of polyester masterbatch (composed of polyester resin and PB15:3; the manufacturer of the polyester resin is Jiangsu Solide New Materials Group Co., Ltd., the variety is a bright type thickening polyester chip, the intrinsic viscosity is 0.95-1.05dl / g, the terminal carboxyl content is ≤15mol / t; the content of PB15:3 is 0.5wt%) and 89 parts of bright polyester chips (the manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model SB500) are mixed evenly and then melt-spun (temperature 285°C, winding speed 2800r / min) to obtain colored polyester fiber with a specification of 100d / 48f.

[0071] A method for preparing colored semi-gloss polyester fiber, the specific process is: according to weight parts, 1 part of the colored polyester high weather-resistant masterbatch prepared in this embodiment, 10 parts of colored polyester masterbatch (composed of polyester resin and pigment; the manufacturer of the polyester resin is Jiangsu Solide New Materials Group Co., Ltd., the variety is a glossy thickening polyester chip, the intrinsic viscosity is 0.95-1.05dl / g, the terminal carboxyl content is ≤15mol / t; the pigment is an organic pigment or an inorganic pigment, when the pigment is an organic pigment, the content of the organic pigment is 0.5wt%, when the pigment is an inorganic pigment, the content of the inorganic pigment is 5wt%; the organic pigment is PB15:3, PG7, PY147, PY150, PR122 or PR202, the inorganic pigment is PY119, PY184, PB29 or PR101), 5 parts of titanium dioxide masterbatch 100 d / 48 f colored semi-bright polyester fibers were obtained by mixing 84 portions of 100 d / 48 f colored semi-bright polyester chips (composed of polyester resin and titanium dioxide; the manufacturer of polyester resin is Jiangsu Solide New Materials Group Co., Ltd., the variety is bright type tackified polyester chips, the intrinsic viscosity is 0.95-1.05 dl / g, the terminal carboxyl content is ≤15 mol / t; the manufacturer of titanium dioxide is Shandong Dongjia Group, the model is SA-50, the particle size is 240-320 nm, and the content is 5 wt%) and 84 portions of bright polyester chips (the manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., the model is SB500) and then melt-spun (temperature 285 ° C, winding speed 2800 r / min) to obtain colored semi-bright polyester fibers with a specification of 100 d / 48 f. After that, the △E and color card grade of various colored semi-bright polyester fibers after 100-500 h irradiation were tested. The data recorded during the test are shown in Table 1:

[0072] Table 1

[0073] Colored semi-gloss polyester pigment 100h △E 200h △E 300h △E 400h △E 500h △E 500h Color Card Grade 1 PB15:3 0.23 0.91 1.78 1.83 2.27 4 2 PG7 0.16 0.42 0.54 0.69 0.97 4.5 3 PY147 0.29 0.32 0.86 0.96 1.35 4.5 4 PY119 0.42 0.51 0.64 0.65 0.68 4.5 5 PY150 0.85 0.87 0.92 0.95 0.98 4.5 6 PY184 1.14 1.17 1.27 1.33 1.43 4.5 7 PR122 1.79 1.93 2.10 2.17 2.22 4 8 PB29 0.87 1.28 1.46 1.69 1.88 4 9 PR202 1.14 1.43 1.73 1.91 2.08 4 10 PR101 0.17 0.24 0.29 0.38 0.44 4.5

[0074] As can be seen from Table 1, after the colored polyester high weather-resistant masterbatch prepared in this embodiment is mixed with the colored polyester masterbatch, the titanium dioxide masterbatch and the bright polyester chips, the colored semi-bright polyester fibers obtained by melt spinning all show good weather resistance after being irradiated for 100 to 500 hours; the ΔE of each colored semi-bright polyester fiber after irradiation for 500 hours is maintained below 2.27, and the color card grade is above level 4;

[0075] Under the same other conditions, if the colored polyester high weather-resistant masterbatch prepared in this embodiment is replaced with a glossy polyester chip of equal quality (manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model SB500), the ΔE and color card grades of various colored semi-gloss polyester fibers after irradiation for 100-500 hours are shown in Table 2:

[0076] Table 2

[0077] Colored semi-gloss polyester pigment 100h △E 200h △E 300h △E 400h △E 500h △E 500h Color Card Grade 1 PB15:3 1.40 2.57 4.16 5.42 6.88 2 2 PG7 0.48 0.90 1.79 2.27 3.06 3.5 3 PY147 1.35 2.12 3.34 5.19 6.23 2.5 4 PY119 0.52 0.86 1.83 2.60 3.87 3 5 PY150 0.80 1.01 1.67 2.11 2.91 3.5 6 PY184 1.49 1.71 2.19 2.53 3.05 3.5 7 PR122 2.62 4.01 6.73 7.64 9.01 2 8 PB29 1.52 2.68 3.15 3.80 4.57 3 9 PR202 1.89 2.99 3.75 4.34 4.93 2.5 10 PR101 0.61 1.10 1.62 2.07 2.56 3.5

[0078] It can be seen from Table 2 that the ΔE of each colored semi-gloss polyester fiber after 500 hours of irradiation is above 2.56, and the color card grade is below 3.5. Compared with Table 1, the weather resistance of each colored semi-gloss polyester fiber is significantly worse, which fully proves the effectiveness of the high weather resistance masterbatch for colored polyester prepared in this embodiment in improving the weather resistance of the colored semi-gloss polyester fiber prepared by the stock solution coloring method.

[0079] A method for preparing colored semi-gloss polyester fiber, the specific process is: according to weight parts, 1 part of the colored polyester high weather resistance masterbatch prepared in this embodiment, 1 part of the carbon black masterbatch (composed of polyester resin and carbon black; the manufacturer of the polyester resin is Jiangsu Solide New Materials Group Co., Ltd., the variety is a glossy tackified polyester chip, the intrinsic viscosity is 0.95-1.05dl / g, and the terminal carboxyl content is ≤15mol / t; the manufacturer of the carbon black powder is Orion Company, the model is AROSPERSE 11, original particle size is 19nm, content is 1wt%), 5 parts of titanium dioxide masterbatch (composed of polyester resin and titanium dioxide; the manufacturer of polyester resin is Jiangsu Solide New Materials Group Co., Ltd., the variety is glossy tackified polyester chips, the intrinsic viscosity is 0.95-1.05dl / g, the terminal carboxyl content is ≤15mol / t; the manufacturer of titanium dioxide is Shandong Dongjia Group, the model is SA-50, the particle size is 240-320nm, the content is 5wt%), 10 parts of colored polyester masterbatch (composed of polyester resin and pigment; the manufacturer of polyester resin is Jiangsu Solide New Materials Group Co., Ltd., the variety is glossy tackified polyester chips, the intrinsic viscosity is 0.95-1.05dl / g, the terminal carboxyl content is ≤15mol / t; The pigment is an organic pigment or an inorganic pigment. When the pigment is an organic pigment, the content of the organic pigment is 0.5wt%, and when the pigment is an inorganic pigment, the content of the inorganic pigment is 5wt%; the organic pigment is PR122, PR202 or PB15:3, and the inorganic pigment is PR101 or PB29) and 83 portions of bright polyester chips (manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model SB500) are mixed evenly and melt-spun (temperature 285°C, winding speed 2800r / min) to obtain colored semi-bright polyester fibers with a specification of 100d / 48f. After that, the △E and color card grades of various colored semi-bright polyester fibers after irradiation for 100~500h are tested. The data recorded during the test are shown in Table 3:

[0080] Table 3

[0081] Colored semi-gloss polyester pigment 100h △E 200h △E 300h △E 400h △E 500h △E 500h Color Card Grade 1 PR122 1.12 1.27 1.40 1.48 1.55 4 2 PR101 0.23 0.36 0.49 0.58 0.86 4.5 3 PR202 0.85 1.62 2.05 2.31 2.69 3.5 4 PB15:3 0.90 1.09 1.27 1.84 1.94 4 5 PB29 0.80 1.90 2.08 2.75 2.95 3.5

[0082] As can be seen from Table 3, after the colored polyester high weather-resistant masterbatch prepared in this embodiment is mixed with colored polyester masterbatch, titanium dioxide masterbatch, carbon black masterbatch and bright polyester chips, the colored semi-bright polyester fibers obtained by melt spinning show good weather resistance after being irradiated for 100 to 500 hours; even in the case of adding carbon black, the ΔE of each colored semi-bright polyester fiber after 500 hours of irradiation is maintained below 2.95, and the color card grade is above 3.5;

[0083] Under the same other conditions, if the colored polyester high weather-resistant masterbatch prepared in this embodiment is replaced with a glossy polyester chip of equal quality (manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model SB500), the ΔE and color card grades of various colored semi-gloss polyester fibers after irradiation for 100-500 hours are shown in Table 4:

[0084] Table 4

[0085] Colored semi-gloss polyester pigment 100h △E 200h △E 300h △E 400h △E 500h △E 500h Color Card Grade 1 PR122 3.71 5.24 7.83 9.85 11.51 1.5 2 PR101 1.16 1.65 2.17 2.94 4.63 3 3 PR202 2.47 3.28 4.36 5.10 6.31 2.5 4 PB15:3 3.27 4.65 5.22 5.93 7.70 2 5 PB29 2.91 3.42 4.08 4.73 6.24 2.5

[0086] It can be seen from Table 4 that the ΔE of each colored semi-gloss polyester fiber after 500 hours of irradiation is above 4.63, and the color card grade is below level 3. Compared with Table 3, the weather resistance of each colored semi-gloss polyester fiber is significantly worse, which fully proves the effectiveness of the high weather-resistant masterbatch for colored polyester prepared in this embodiment in improving the weather resistance of the colored semi-gloss polyester fiber to which carbon black is added during the preparation process.

[0087] Comparative Example 1

[0088] A method for preparing a masterbatch is basically the same as that in Example 1, except that the polyester resin is produced by Sinopec Yizheng Chemical Fiber Co., Ltd. and the brand is SB500 (the intrinsic viscosity of the polyester resin is 0.6750 dl / g and the terminal carboxyl content is 24 mol / t).

[0089] A method for preparing colored polyester fiber is basically the same as that of Example 1, except that the highly weather-resistant masterbatch for colored polyester is replaced by the masterbatch of Comparative Example 1.

[0090] Comparative Example 2

[0091] A method for preparing a masterbatch is basically the same as that of Example 1, except that the triazine UV absorber (a mixture of 2,4-di(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine and 2,4,6-tri(4'-butoxy-2'-hydroxyphenyl)-triazine in a mass ratio of 1:1.5) is replaced by an equal mass of a triazole UV absorber (UV 360, manufactured by BASF).

[0092] A method for preparing colored polyester fiber is basically the same as that of Example 1, except that the highly weather-resistant masterbatch for colored polyester is replaced by the masterbatch of Comparative Example 2.

[0093] The ΔE of the colored polyester fibers of Example 1, Comparative Example 1 and Comparative Example 2 after 100-500 hours of irradiation was tested, and the data recorded during the test are shown in Table 5:

[0094] Table 5

[0095] 100h △E 200h △E 300h △E 400h △E 500h △E 500h Color Card Grade Example 1 0.89 1.11 1.41 1.52 1.64 4 Comparative Example 1 0.80 0.88 1.46 2.00 2.51 3.5 Comparative Example 2 1.26 2.05 2.95 3.05 3.49 3

[0096] As can be seen from Table 1, the ΔE of the colored polyester fibers of Comparative Examples 1 and 2 after 500 hours of irradiation are both greater than that of Example 1, and the color card grades are both lower than that of Example 1. This is because the viscosity of the polyester resin used in Comparative Example 1 is too low and the terminal carboxyl content is too high. During the thermal processing of manufacturing the polyester masterbatch, the polyester degradation will be aggravated, and the screw shearing will further reduce its viscosity, resulting in significant differences in the physical properties of the obtained masterbatch and the conventional polyester chips, and the weather resistance is reduced; and the triazole ultraviolet absorber used in Comparative Example 2 has a five-membered ring structure and has poor long-term stability. After the polyester product is subjected to a long period of irradiation, its absorption performance will gradually decrease, resulting in a weakened protection effect and a decrease in the weather resistance of the polyester product.

[0097] Example 2

[0098] A method for preparing a highly weather-resistant masterbatch for colored polyester is basically the same as that in Example 1, except that the main antioxidant in the composite antioxidant is bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid][oxalylbis(azanediyl)]bis(ethane-2,1-diyl)ester (the mass proportion of the main antioxidant in the composite antioxidant is the same as that in Example 1).

[0099] The intrinsic viscosity of the finally obtained high weather-resistant masterbatch for colored polyester is 0.6242 dl / g.

[0100] A method for preparing colored polyester fiber is basically the same as that in Example 1, except that the highly weather-resistant masterbatch for colored polyester is the highly weather-resistant masterbatch for colored polyester prepared in this example.

[0101] The △E of the finally obtained colored polyester fiber after 500 hours of irradiation is 1.72, and the color card grade after 500 hours of irradiation is level 4.

[0102] Example 3

[0103] A method for preparing a highly weather-resistant masterbatch for colored polyester is basically the same as that in Example 1, except that: the main antioxidant in the composite antioxidant is a hindered phenol auxiliary (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) commonly used in traditional polyesters, and the mass proportion of the main antioxidant in the composite antioxidant is the same as that in Example 1.

[0104] The intrinsic viscosity of the finally obtained high weather-resistant masterbatch for colored polyester is 0.6381 dl / g.

[0105] A method for preparing colored polyester fiber is basically the same as that in Example 1, except that the highly weather-resistant masterbatch for colored polyester is the highly weather-resistant masterbatch for colored polyester prepared in this example.

[0106] The △E of the finally obtained colored polyester fiber after 500 hours of irradiation is 2.35, and the color card grade after 500 hours of irradiation is level 4.

[0107] Compared with Example 1, the ΔE of the colored polyester fiber after 500 hours of irradiation is larger in Example 3. This is because the main antioxidant in the composite antioxidant used in Example 3 does not have an oxalamide or hydrazide structure, and the obtained high weather-resistant masterbatch for colored polyester is relatively weak in resisting metal ion catalytic aging. Under long-term irradiation conditions, the residual metal ions are more likely to catalyze the degradation of the polyester molecular chain, resulting in an increase in the ΔE of the colored polyester fiber and a decrease in the color card grade.

[0108] Example 4

[0109] A method for preparing a highly weather-resistant masterbatch for colored polyester is basically the same as that in Example 1, except that no organic solvent is added in step (2), that is, 40 parts of a composite antioxidant, 55 parts of a composite light stabilizer and 5 parts of an adsorbent are directly mixed uniformly to obtain a composite stabilizer.

[0110] The intrinsic viscosity of the finally obtained high weather-resistant masterbatch for colored polyester is 0.6279 dl / g.

[0111] A method for preparing colored polyester fiber is basically the same as that in Example 1, except that the highly weather-resistant masterbatch for colored polyester is the highly weather-resistant masterbatch for colored polyester prepared in this example.

[0112] The △E of the finally obtained colored polyester fiber after 500 hours of irradiation is 2.68, and the color card grade after 500 hours of irradiation is 3.5.

[0113] Compared with Example 1, the ΔE of the colored polyester fiber after 500 hours of irradiation is larger in Example 4. This is because Example 4 does not mix the components of the compound stabilizer with the organic solvent to achieve pre-dispersion, resulting in uneven distribution of the components during subsequent processing. During the pulping process, the compound stabilizer cannot be fully dissolved in the organic solvent to reach a eutectic state, thereby weakening its synergistic protective effect on the colored polyester products during processing and use.

[0114] Example 5

[0115] A method for preparing a highly weather-resistant masterbatch for colored polyester is basically the same as that in Example 1, except that the auxiliary antioxidant in the composite antioxidant is a mixture of 3,9-bis(2,4-dicumylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane and bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite in a mass ratio of 1:1 (the mass proportion of the auxiliary antioxidant in the composite antioxidant is the same as that in Example 1).

[0116] The intrinsic viscosity of the finally obtained high weather-resistant masterbatch for colored polyester is 0.6074 dl / g.

[0117] A method for preparing colored polyester fiber is basically the same as that in Example 1, except that the highly weather-resistant masterbatch for colored polyester is the highly weather-resistant masterbatch for colored polyester prepared in this example.

[0118] The △E of the finally obtained colored polyester fiber after 500 hours of irradiation is 2.06, and the color card grade after 500 hours of irradiation is level 4.

[0119] Example 6

[0120] A method for preparing a highly weather-resistant masterbatch for colored polyester is basically the same as that in Example 1, except that the triazine ultraviolet absorber in the composite light stabilizer is 2,4-di(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine (the mass proportion of the triazine ultraviolet absorber in the composite light stabilizer is the same as that in Example 1).

[0121] The intrinsic viscosity of the finally obtained high weather-resistant masterbatch for colored polyester is 0.6326 dl / g.

[0122] A method for preparing colored polyester fiber is basically the same as that in Example 1, except that the highly weather-resistant masterbatch for colored polyester is the highly weather-resistant masterbatch for colored polyester prepared in this example.

[0123] The △E of the finally obtained colored polyester fiber after 500 hours of irradiation is 1.82, and the color card grade after 500 hours of irradiation is level 4.

[0124] Example 7

[0125] A method for preparing a highly weather-resistant masterbatch for colored polyester, the specific steps are as follows:

[0126] (1) Preparation of raw materials;

[0127] Composite antioxidant: a mixture of a primary antioxidant, a secondary antioxidant and a free radical scavenger in a mass ratio of 5.6:5.4:1, wherein the primary antioxidant is a mixture of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N'-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl] propionyl hydrazide and bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid][oxalylbis(azanediyl)]bis(ethane-2,1-diyl) ester in a mass ratio of 1:1, the secondary antioxidant is bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite, and the free radical scavenger is 5,7-di-tert-butyl-3-(3,4-dimethylphenyl)benzofuran-2(3H)-one;

[0128] Composite light stabilizer: a mixture of a triazine UV absorber and a triazine hindered amine in a mass ratio of 2.25:1, the triazine UV absorber is a mixture of 2-(4,6-diphenyl-1,3,5-triazine-2)-5-n-hexyloxyphenol, 2,4-bis[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxybenzene)-1,3,5-triazine and 2,4,6-tris(4'-butoxy-2'-hydroxyphenyl)-triazine in a mass ratio of 2.28:1.72:1, and the triazine hindered amine is a methylated polymer of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine and morpholine-2,4,6-trichloro-1,3,5-triazine (manufacturer is Cytec, model is Cyasorb UV-3529);

[0129] Adsorbent: fumed silica, manufactured by Cabot Corporation, model CLARUS 3160;

[0130] Organic solvent: dichloromethane;

[0131] Polyester resin: The manufacturer is Jiangsu Solide New Materials Group Co., Ltd., the variety is glossy tackified polyester chips, the intrinsic viscosity is 0.95-1.05dl / g, and the terminal carboxyl content is ≤15mol / t;

[0132] Dispersant: Tegomer P121, manufactured by Evonik Industries;

[0133] (2) preparing a compound stabilizer;

[0134] By weight, 30 parts of a composite antioxidant, 65 parts of a composite light stabilizer, 5 parts of an adsorbent and an organic solvent are mixed, stirred evenly, and the organic solvent is removed to obtain a composite stabilizer; wherein the amount of the organic solvent added is 0.3 times the total mass of the composite antioxidant, the composite light stabilizer and the adsorbent;

[0135] (3) Preparation of highly weather-resistant masterbatch for colored polyester;

[0136] By weight, 65 parts of polyester resin, 34.5 parts of compound stabilizer and 0.5 parts of dispersant are mixed evenly and put into a twin-screw extruder for melt extrusion, strip drawing and pelletizing to obtain high weather-resistant masterbatch for colored polyester; wherein, the temperature of zone 1 of the twin-screw extruder is 220°C, the temperature of zone 2 is 275°C, the temperature of zone 3 is 275°C, the temperature of zone 4 is 270°C, the temperature of zone 5 is 220°C, the temperature of zone 6 is 220°C, the temperature of zone 7 is 240°C, and the temperature of zone 8 is 260°C; the speed of the twin-screw extruder is 300r / min.

[0137] The intrinsic viscosity of the finally obtained high weather-resistant masterbatch for colored polyester is 0.5710 dl / g.

[0138] A method for preparing colored polyester fiber, the specific process is: according to weight parts, 1 part of the high weather-resistant masterbatch for colored polyester prepared in this embodiment, 10 parts of polyester masterbatch (composed of polyester resin and PB15:3; the manufacturer of the polyester resin is Jiangsu Solide New Materials Group Co., Ltd., the variety is a bright type thickening polyester chip, the intrinsic viscosity is 0.95-1.05dl / g, the terminal carboxyl content is ≤15mol / t; the content of PB15:3 is 0.5wt%) and 89 parts of bright polyester chips (the manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model SB500) are mixed evenly and then melt-spun (temperature 285°C, winding speed 2800r / min) to obtain colored polyester fiber with a specification of 100d / 48f.

[0139] Example 8

[0140] A method for preparing a highly weather-resistant masterbatch for colored polyester, the specific steps are as follows:

[0141] (1) Preparation of raw materials;

[0142] Composite antioxidant: a mixture of a primary antioxidant, a secondary antioxidant and a free radical scavenger in a mass ratio of 5:6:1, wherein the primary antioxidant is a mixture of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N'-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl] propionyl hydrazide and bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid][oxalylbis(azanediyl)]bis(ethane-2,1-diyl) ester in a mass ratio of 1:1, the secondary antioxidant is tris(2,4-di-tert-butyl)phenyl phosphite, and the free radical scavenger is 5,7-di-tert-butyl-3-(3,4-dimethylphenyl)benzofuran-2(3H)-one;

[0143] Composite light stabilizer: a mixture of triazine UV absorber and triazine hindered amine in a mass ratio of 2:1, the triazine UV absorber is 2,4-bis(2,4-xylyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, 2,4-bis(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine in a mass ratio of 1:1:1.3. A mixture of oxazine and 2,4-bis[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, the triazine hindered amine is poly[N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-CO-2,4-dichloro-6-morpholine-1,3,5-triazine] (manufacturer is Cytec, model is Cyasorb UV-3346, CAS number is 82451-48-7);

[0144] Adsorbent: fumed silica, manufactured by Cabot Corporation, model CLARUS 3160;

[0145] Organic solvent: dichloromethane;

[0146] Polyester resin: The manufacturer is Jiangsu Solide New Materials Group Co., Ltd., the variety is glossy tackified polyester chips, the intrinsic viscosity is 0.95-1.05dl / g, and the terminal carboxyl content is ≤15mol / t;

[0147] Dispersant: Tegomer P121, manufactured by Evonik Industries;

[0148] (2) preparing a compound stabilizer;

[0149] By weight, 36 parts of a composite antioxidant, 60 parts of a composite light stabilizer, 4 parts of an adsorbent and an organic solvent are mixed, stirred evenly, and the organic solvent is removed to obtain a composite stabilizer; wherein the amount of the organic solvent added is 0.5 times the total mass of the composite antioxidant, the composite light stabilizer and the adsorbent;

[0150] (3) Preparation of highly weather-resistant masterbatch for colored polyester;

[0151] By weight, 67.5 parts of polyester resin, 32 parts of compound stabilizer and 0.5 parts of dispersant are mixed evenly and put into a twin-screw extruder for melt extrusion, strip drawing and pelletizing to obtain high weather-resistant masterbatch for colored polyester; wherein, the temperature of zone 1 of the twin-screw extruder is 220°C, the temperature of zone 2 is 275°C, the temperature of zone 3 is 275°C, the temperature of zone 4 is 270°C, the temperature of zone 5 is 220°C, the temperature of zone 6 is 220°C, the temperature of zone 7 is 240°C, and the temperature of zone 8 is 260°C; the speed of the twin-screw extruder is 300r / min.

[0152] The intrinsic viscosity of the finally obtained high weather-resistant masterbatch for colored polyester is 0.6027 dl / g.

[0153] A method for preparing colored polyester fiber, the specific process is: according to weight parts, 1 part of the high weather-resistant masterbatch for colored polyester prepared in this embodiment, 10 parts of polyester masterbatch (composed of polyester resin and PB15:3; the manufacturer of the polyester resin is Jiangsu Solide New Materials Group Co., Ltd., the variety is a bright type thickening polyester chip, the intrinsic viscosity is 0.95-1.05dl / g, the terminal carboxyl content is ≤15mol / t; the content of PB15:3 is 0.5wt%) and 89 parts of bright polyester chips (the manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model SB500) are mixed evenly and then melt-spun (temperature 285°C, winding speed 2800r / min) to obtain colored polyester fiber with a specification of 100d / 48f.

[0154] The ΔE of the colored polyester fibers of Example 7 and Example 8 after irradiation for 100 to 500 hours was tested, and the data recorded during the test are shown in Table 6:

[0155] Table 6

[0156] Colored polyester 100h △E 200h △E 300h △E 400h △E 500h △E 500h Color Card Grade Example 7 0.93 1.33 1.82 1.95 2.14 4 Example 8 0.88 1.56 2.16 2.31 2.43 4

[0157] Comparative Example 3

[0158] A method for preparing a masterbatch is basically the same as that in Example 7, except that: there is no free radical scavenger in the composite antioxidant (the mass ratio of the primary antioxidant to the auxiliary antioxidant is the same as that in Example 7).

[0159] A method for preparing colored polyester fiber is basically the same as that of Example 7, except that the highly weather-resistant masterbatch for colored polyester is replaced by the masterbatch of Comparative Example 3.

[0160] The △E of the finally obtained colored polyester fiber after 500 hours of irradiation is 2.71, and the color card grade after 500 hours of irradiation is 3.5.

[0161] Compared with Example 7, the ΔE of the colored polyester fiber in Comparative Example 3 increases and the color card grade decreases. This is because there is no free radical scavenger in the composite antioxidant used in Comparative Example 3. The lack of the free radical scavenger causes the polyester masterbatch to be unable to effectively quench the alkyl free radicals in the early stage of the thermal degradation chain reaction, thereby failing to terminate the aging reaction in time. This causes the performance of the masterbatch to deteriorate during the thermal processing, resulting in an increase in the ΔE of the colored polyester fiber finally obtained and a decrease in the color card grade, indicating that its weather resistance is poor.

[0162] Comparative Example 4

[0163] A method for preparing a masterbatch is basically the same as that in Example 7, except that: the composite antioxidant contains no primary antioxidant (the mass ratio of the auxiliary antioxidant to the free radical scavenger is the same as that in Example 7).

[0164] A method for preparing colored polyester fiber is basically the same as that of Example 7, except that the highly weather-resistant masterbatch for colored polyester is replaced by the masterbatch of Comparative Example 4.

[0165] The △E of the finally obtained colored polyester fiber after 500 hours of irradiation is 2.68, and the color card grade after 500 hours of irradiation is 3.5.

[0166] Compared with Example 7, the ΔE of the colored polyester fiber in Comparative Example 4 increases and the color card grade decreases. This is because there is no main antioxidant in the composite antioxidant used in Comparative Example 4, which results in the polyester masterbatch being unable to effectively quench the hydroxyl radicals and peroxy radicals generated by the reaction of alkyl radicals with oxygen / water during the thermal degradation chain reaction, thereby causing the performance of the masterbatch to deteriorate during the thermal processing, resulting in an increase in the ΔE of the colored polyester fiber finally obtained and a decrease in the color card grade, indicating that its weather resistance is poor.

[0167] Comparative Example 5

[0168] A method for preparing a masterbatch is basically the same as that in Example 7, except that the triazine hindered amine in the composite light stabilizer is replaced by a hydrophobic hindered amine containing a long carbon chain (UV 5050H, manufactured by BASF), and the mass proportion in the composite light stabilizer is the same as that in Example 7.

[0169] A method for preparing colored polyester fiber is basically the same as that of Example 7, except that the highly weather-resistant masterbatch for colored polyester is replaced by the masterbatch of Comparative Example 5.

[0170] The △E of the finally obtained colored polyester fiber after 500 hours of irradiation is 3.82, and the color card grade after 500 hours of irradiation is level 3.

[0171] Compared with Example 7, the ΔE of the colored polyester fiber in Comparative Example 5 increases and the color card grade decreases. This is because the hindered amine used in Comparative Example 5 is a hydrophobic hindered amine containing a long carbon chain, and the long carbon chain has poor compatibility with polyester, resulting in poor dispersibility of the long carbon chain hindered amine in polyester products. This significantly affects the ΔE and color card grade of the colored polyester fiber finally obtained, and the weather resistance is poor.

[0172] Example 9

[0173] A method for preparing a highly weather-resistant masterbatch for colored polyester, the specific steps are as follows:

[0174] (1) Preparation of raw materials;

[0175] Composite antioxidant: a mixture of a primary antioxidant, a secondary antioxidant and a free radical scavenger in a mass ratio of 5:6:1, wherein the primary antioxidant is a mixture of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N'-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl] propionyl hydrazide and bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid][oxalylbis(azanediyl)]bis(ethane-2,1-diyl) ester in a mass ratio of 1:1, the secondary antioxidant is tris(2,4-di-tert-butyl)phenyl phosphite, and the free radical scavenger is 5,7-di-tert-butyl-3-(3,4-dimethylphenyl)benzofuran-2(3H)-one;

[0176] Composite light stabilizer: a mixture of triazine UV absorber and triazine hindered amine in a mass ratio of 2:1, the triazine UV absorber is 2,4-bis(2,4-xylyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, 2,4-bis(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine in a mass ratio of 1:1:1.3. A mixture of oxazine and 2,4-bis[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, the triazine hindered amine is poly[N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-CO-2,4-dichloro-6-morpholine-1,3,5-triazine] (manufacturer is Cytec, model is Cyasorb UV-3346, CAS number is 82451-48-7);

[0177] Adsorbent: fumed silica, manufactured by Cabot Corporation, model CLARUS 3160;

[0178] Organic solvent: dichloromethane;

[0179] Polyester resin: The manufacturer is Jiangsu Solide New Materials Group Co., Ltd., the variety is glossy tackified polyester chips, the intrinsic viscosity is 0.95-1.05dl / g, and the terminal carboxyl content is ≤15mol / t;

[0180] Dispersant: Tegomer P121, manufactured by Evonik Industries;

[0181] (2) preparing a compound stabilizer;

[0182] By weight, 33 parts of a composite antioxidant, 64 parts of a composite light stabilizer, 3 parts of an adsorbent and an organic solvent are mixed, stirred evenly, and the organic solvent is removed to obtain a composite stabilizer; wherein the amount of the organic solvent added is 0.3 times the total mass of the composite antioxidant, the composite light stabilizer and the adsorbent;

[0183] (3) Preparation of highly weather-resistant masterbatch for colored polyester;

[0184] By weight, 69.9 parts of polyester resin, 30 parts of compound stabilizer and 0.1 parts of dispersant are mixed evenly and put into a twin-screw extruder for melt extrusion, strip drawing and pelletizing to obtain high weather-resistant masterbatch for colored polyester; wherein, the temperature of zone 1 of the twin-screw extruder is 220°C, the temperature of zone 2 is 275°C, the temperature of zone 3 is 275°C, the temperature of zone 4 is 270°C, the temperature of zone 5 is 220°C, the temperature of zone 6 is 220°C, the temperature of zone 7 is 240°C, and the temperature of zone 8 is 260°C; the speed of the twin-screw extruder is 300r / min.

[0185] The intrinsic viscosity of the finally obtained high weather-resistant masterbatch for colored polyester is 0.6245 dl / g.

[0186] A method for preparing colored polyester fiber, the specific process is: according to weight parts, 10 parts of high weather-resistant masterbatch for colored polyester prepared in this embodiment, 10 parts of polyester masterbatch (composed of polyester resin and PB15:3; the manufacturer of polyester resin is Jiangsu Solide New Materials Group Co., Ltd., the variety is bright type thickening polyester chips, the intrinsic viscosity is 0.95-1.05dl / g, the terminal carboxyl content is ≤15mol / t; the content of PB15:3 is 0.5wt%) and 80 parts of bright polyester chips (manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model SB500) are mixed evenly and then melt-spun (temperature 285°C, winding speed 2800r / min) to obtain colored polyester fiber with a specification of 100d / 48f.

[0187] The △E of the finally obtained colored polyester fiber after 500 hours of irradiation is 1.93, and the color card grade after 500 hours of irradiation is level 4.

[0188] The five triazine ultraviolet absorbers selected by the present invention: (2,4-bis(2,4-xylyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, 2-(4,6-diphenyl-1,3,5-triazine-2)-5-n-hexyloxyphenol, 2,4-bis(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine, 2,4-bis[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxybenzene)-1,3,5-triazine, 2,4,6-tris(4'-butoxy-2'-hydroxyphenyl)-triazine) have absorbances of 280-400nm. Figure 1 As shown;

[0189] The triazine ultraviolet absorber combination selected in Examples 1 to 5 (a mixture of 2,4-di(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine and 2,4,6-tri(4'-butoxy-2'-hydroxyphenyl)-triazine in a mass ratio of 1:1.5), the triazine ultraviolet absorber combination selected in Example 7 (2-(4,6-diphenyl-1,3,5-triazine-2)-5-n-hexyloxyphenol, 2,4-di[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxybenzene)-1,3,5-triazine in a mass ratio of 2.28:1.72:1 The absorbance of the triazine ultraviolet absorber combination selected in Examples 8 to 9 (a mixture of 2,4-bis(2,4-diphenyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, 2,4-bis(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine and 2,4-bis[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutyloxyphenyl)-1,3,5-triazine in a mass ratio of 1:1:1.3) at 280 to 400 nm is as follows: Figure 2 shown; from Figure 2 It can be seen that the different triazine ultraviolet absorber combinations selected in the present invention all have high ultraviolet absorption efficiency, and these combinations cover the entire ultraviolet light region, which can not only effectively protect the carbonyl groups in the polyester from being damaged by rays in the wavelength band close to 300nm in the sunlight, but also provide targeted protection in the long-wave part of the ultraviolet region in accordance with the distribution trend of the solar spectrum, thereby achieving comprehensive and effective protection for various pigments.

Claims

1. A highly weather-resistant masterbatch for colored polyester, characterized in that: By weight, it includes 65-70 parts of polyester resin, 30-34.5 parts of compound stabilizer, and 0.1-0.5 parts of dispersant; The intrinsic viscosity of the polyester resin is 0.95-1.05dl / g, and the terminal carboxyl content is ≤15mol / t; By weight, the compound stabilizer includes 30-40 parts of compound antioxidant and 55-65 parts of compound light stabilizer; Composite antioxidants include primary antioxidants, secondary antioxidants, and free radical scavengers; The primary antioxidant is one or more of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N'-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl] propionyl hydrazide and bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate][oxalylbis(azanediyl)]bis(ethane-2,1-diyl) ester; The auxiliary antioxidant is one or more of bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite and 3,9-bis(2,4-dicumylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane; The free radical scavenger is 5,7-di-tert-butyl-3-(3,4-dimethylphenyl)benzofuran-2(3H)-one; Composite light stabilizers include triazine UV absorbers and triazine hindered amines.

2. A highly weather-resistant masterbatch for colored polyester according to claim 1, characterized in that: The triazine ultraviolet absorber is one or more of 2,4-bis(2,4-xylyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, 2-(4,6-diphenyl-1,3,5-triazine-2)-5-n-hexyloxyphenol, 2,4-bis(4-biphenyl)-6-(2,4-dihydroxy)phenyl-1,3,5-triazine, 2,4-bis[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxybenzene)-1,3,5-triazine, and 2,4,6-tris(4'-butoxy-2'-hydroxyphenyl)-triazine.

3. The highly weather-resistant masterbatch for colored polyester according to claim 1, characterized in that: The triazine hindered amine is one or more of poly[N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-CO-2,4-dichloro-6-morpholine-1,3,5-triazine], methylated polymer of N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine and morpholine-2,4,6-trichloro-1,3,5-triazine, and reaction product of N,N″-1,2-ethanediyldi(1,3-propylenediamine) with cyclohexane and peroxide N-butyl-2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine.

4. The highly weather-resistant masterbatch for colored polyester according to claim 1, characterized in that: Calculated by weight, the compound stabilizer also includes 3-5 parts of adsorbent; the adsorbent is fumed silica.

5. A highly weather-resistant masterbatch for colored polyester according to claim 4, characterized in that: The preparation process of the compound stabilizer is as follows: after mixing the compound antioxidant, the compound light stabilizer, the adsorbent and the organic solvent, stirring evenly, and removing the organic solvent, the compound stabilizer is obtained.

6. A method for preparing a highly weather-resistant masterbatch for colored polyester as claimed in any one of claims 1 to 5, characterized in that: After uniformly mixing the components in proportion, the mixture is melt-extruded, drawn into strips, and cut into pellets to obtain highly weather-resistant masterbatch for colored polyester.

7. The use of a highly weather-resistant masterbatch for colored polyester as claimed in any one of claims 1 to 5, characterized in that: Used in the preparation of polyester fiber, the addition amount is 0.1-10wt%.

Citation Information

Patent Citations

  • Polycarbonate combination and preparation method thereof

    CN101906244A

  • Weather-resistant white master batch, weather-resistant polyester material and preparation methods of weather-resistant white master batch and weather-resistant polyester material

    CN102492269A

  • Anti-ultraviolet polyester film

    CN111286161A

  • PET anti-photoaging weather-resistant master batch and preparation method thereof

    CN111675885A

  • High-heat-resistance and high-weather-resistance polypropylene composition and preparation method thereof