A method for preparing modified polyacrylic acid fire retardant coating

By using phosphorus-containing modified vinyl silane and vinyl nanosilica in polyacrylic coatings, the fire resistance and mechanical properties of the coating are improved, and the problem of poor fire resistance of polyacrylic coatings is solved, forming efficient fire resistance and resistance Impact paint.

CN118530641BActive Publication Date: 2024-11-22ANHUI SHENZHOU SPACESHIP ADHESIVE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411004745.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-22
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The fire resistance of existing polyacrylic coatings is poor, and they need to improve their fire resistance and mechanical properties.

Method used

Using phosphorus-containing modified vinyl silane and vinyl nanosilia as key components, a modified polyacrylic emulsion is prepared by emulsion polymerization, and a dispersant and defoaming agent are added to form uniformly dispersed nanosilia particles to improve Fire resistance and mechanical properties.

Benefits of technology

It significantly improves the fire resistance and mechanical properties of the coating, reduces the agglomeration and organicization of nano-silica to enhance compatibility, and the reaction between phosphorus and silicon elements forms a dense carbon layer and glass-like substance, effectively hindering the spread of fire and absorbing impact. energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118530641B_ABST
    Figure CN118530641B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of coatings, and discloses a method for preparing a modified polyacrylic acid fire retardant coating. The present invention uses (2-carboxyethyl)phenylphosphonic acid and methylvinyldichlorosilane as raw materials to prepare intermediate 1, which is then reacted with thionyl chloride and PEPA to prepare phosphorus-containing modified vinyl silane. Nano silicon dioxide and trimethoxy (4-vinylphenyl) silane are used as raw materials to obtain vinyl nano silicon dioxide. Butyl acrylate and phosphorus-containing modified vinyl silane and vinyl nano silicon dioxide are subjected to emulsion polymerization to obtain a modified polyacrylic acid emulsion, and finally a dispersant is added thereto and mixed uniformly to obtain a modified polyacrylic acid fire retardant coating. The coating prepared by the present invention has good fire retardancy and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a method for preparing a modified polyacrylic acid fire retardant coating. Background Art

[0002] Fire retardant coating is a functional coating that is applied to the surface of a combustible substrate to reduce the flammability of the coated substrate surface, prevent the spread of fire, and improve the fire resistance limit of the combustible substrate. It is easy to use, has high fireproof efficiency, and is highly adaptable. Therefore, it is widely used in construction, transportation, cultural relics, electrical appliances, cables, military industry, aerospace, etc. Polyacrylic acid coating has excellent weather resistance, color retention, gloss retention and other properties, but its fire resistance is poor, so it is crucial to improve the fire resistance of polyacrylic acid coating.

[0003] 1-Oxo-4-hydroxymethyl-2,6,7-trioxa-1-phosphabicyclo[2.2.2]octane (PEPA), also known as pentaerythritol phosphate, has a high phosphorus content and is an excellent flame retardant intermediate. Nanosilica is an amorphous white powder material with unsaturated dangling bonds and hydroxyl groups in different bonding states on its surface. Due to its small size and large surface area, its application in coatings can effectively increase the reaction area, enhance the strength of the foaming layer, and improve fire resistance.

[0004] For example, the patent with application publication number CN 105273556 A discloses a method for preparing a polyacrylate / nano-silica composite emulsion coating. The invention prepares a modified nano-silica sol, uses it and acrylate as reactants, and obtains a composite emulsion through in-situ hydrolysis. A thickener is then added thereto to prepare a polyacrylate / nano-silica composite emulsion coating. The prepared coating has good heat resistance, waterproof and anti-fouling properties, but does not improve the waterproof performance of the coating. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing a modified polyacrylic acid fire retardant coating, and the prepared coating has good fire retardant effect and mechanical properties.

[0007] (II) Technical solution

[0008] A method for preparing a modified polyacrylic acid fire retardant coating, the preparation method is as follows:

[0009] (1) Butyl acrylate, methyl methacrylate, phosphorus-modified vinyl silane, and vinyl nano-silica are added to deionized water, stirred and dispersed, and then sodium dodecyl sulfonate and an emulsifier are added thereto. Stirring and emulsifying is continued for 40-80 minutes. After stirring, the temperature is raised to 70-80°C, and ammonium persulfate and sodium bicarbonate are added thereto. The reaction is stirred for 3-6 hours. After the reaction is completed, the mixture is cooled to room temperature, and the pH is adjusted to 8-9 with aqueous ammonia to obtain a modified polyacrylic acid emulsion.

[0010] (2) Add a dispersant and a defoaming agent into deionized water, stir and disperse, then add the modified polyacrylic acid emulsion thereto and stir and mix evenly to obtain a modified polyacrylic acid fire retardant coating.

[0011] Preferably, in step (1), the dosage ratio of butyl acrylate, methyl methacrylate, phosphorus-modified vinyl silane, vinyl nano-silica, sodium dodecyl sulfonate, emulsifier, ammonium persulfate and sodium bicarbonate is 100g: (100-150)g: (10-80)g: (10-80)g: (10-20)g: (5-10)g: (1-4)g: (0.2-0.5)g.

[0012] Preferably, in step (2), the usage ratio of the dispersant, the defoaming agent and the modified polyacrylic acid emulsion is (2-8) g: (1-6) g: 100 g.

[0013] Preferably, in step (1), the preparation method of phosphorus-modified vinyl silane is:

[0014] S1. Under a nitrogen atmosphere, add (2-carboxyethyl)phenylphosphonic acid, methylvinyldichlorosilane and pyridine to acetonitrile solvent, stir and disperse, heat to 70-85°C, stir and react for 6-12h. After the reaction is completed, evaporate under reduced pressure, wash with ethanol and dry to obtain intermediate 1.

[0015] S2. Under a nitrogen atmosphere, add intermediate 1 and dichlorothionyl to acetonitrile solvent, heat to 70-80°C, react for 2-4 hours, cool to 0-5°C after the reaction, add PEPA and triethylamine, stir and disperse, heat to 70-80°C, react for 2-5 hours, cool to room temperature after the reaction, filter, wash with deionized water, and dry to obtain phosphorus-modified vinyl silane.

[0016] Preferably, in S1, the usage ratio of (2-carboxyethyl)phenylphosphonic acid, methylvinyldichlorosilane and pyridine is (2-2.4) g:1 g:(2-2.6) g.

[0017] Preferably, in S2, the usage ratio of intermediate 1, thionyl chloride, PEPA and triethylamine is 1 g: (0.45-0.6) g: (0.6-1) g: (0.5-0.8) g.

[0018] Preferably, in the step (1), the preparation method of vinyl nano-silica is: under a nitrogen atmosphere, adding nano-silica to a toluene solvent, ultrasonically dispersing for 20-50 minutes at room temperature, then adding trimethoxy (4-vinylphenyl) silane thereto, reacting at 75-85°C for 20-30 hours, after the reaction is completed, filtering under negative pressure, washing with ethanol, and drying to obtain vinyl nano-silica.

[0019] Preferably, the usage ratio of the nano-silicon dioxide and trimethoxy(4-vinylphenyl)silane is 10 g: (0.12-2) mol.

[0020] 3. Beneficial technical effects

[0021] The invention uses (2-carboxylethyl)phenylphosphonic acid and methylvinyldichlorosilane as raw materials and pyridine as an acid-binding agent to prepare an intermediate 1, and the intermediate 1 is sequentially reacted with thionyl chloride and PEPA through chlorination and esterification to prepare phosphorus-containing modified vinyl silane. Nano silicon dioxide and trimethoxy (4-vinylphenyl) silane are reacted to obtain vinyl nano silicon dioxide. Butyl acrylate and phosphorus-containing modified vinyl silane and vinyl nano silicon dioxide are subjected to emulsion polymerization to obtain a modified polyacrylic acid emulsion, and finally a dispersant is added thereto and mixed uniformly to obtain a modified polyacrylic acid fire retardant coating.

[0022] The nano silicon dioxide used in the present invention is agglomerated, and the present invention makes it organic, reduces the degree of agglomeration, increases its compatibility with organic substances, and is evenly dispersed in the coating to better exert its fireproof effect. Moreover, when subjected to external force impact, the nano silicon dioxide rigid particles evenly dispersed in the coating can absorb more energy as stress concentration points, thereby improving the mechanical properties of the coating, and the rigid structure such as benzene ring contained therein can also absorb impact energy when subjected to external force, thereby increasing the mechanical properties of the coating.

[0023] The coating prepared by the present invention contains more phosphorus and silicon. When the phosphorus is heated, it can produce strong dehydrating substances such as polyphosphoric acid and metaphosphoric acid, which promotes the dehydration of the coating into carbon and forms a dense carbon layer. The silicon contained therein can form a glass-like substance when heated, covering the surface of the material, hindering the material transportation and energy transfer, thereby improving the fireproof performance of the coating. The coating prepared by the present invention has good fireproof performance and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a preparation route for phosphorus-modified vinyl silane;

[0025] Figure 2 It is the preparation route of vinyl nano-silica. DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.

[0027] The preparation method of 1-oxo-4-hydroxymethyl-2,6,7-trioxa-1-phosphabicyclo[2.2.2]octane (PEPA) is as follows: 33.6 g of pentaerythritol is added to 100 mL of 1,4-dioxane solvent, stirred and dispersed, heated to 80° C., 38.3 g of phosphorus oxychloride is added thereto, reacted for 2 hours, and after the reaction is completed, cooled to room temperature, filtered, recrystallized, and dried to obtain PEPA.

[0028] The emulsifier is emulsifier OP-10; the dispersant is dispersant SK-5040; and the defoamer is water-based defoamer SD-202. Embodiment 1

[0029] (1) Under a nitrogen atmosphere, 10 g of (2-carboxyethyl)phenylphosphonic acid, 5 g of methylvinyldichlorosilane, and 13 g of pyridine were added to 200 mL of acetonitrile solvent, stirred and dispersed, and the temperature was raised to 85°C. The reaction was stirred for 10 h. After the reaction was completed, the mixture was evaporated under reduced pressure, washed with ethanol, and dried to obtain intermediate 1.

[0030] (2) Under a nitrogen atmosphere, 10 g of the intermediate 1 and 5.5 g of thionyl chloride were added to 200 mL of acetonitrile solvent, the temperature was raised to 75°C, and the reaction was carried out for 3 h. After the reaction was completed, the mixture was cooled to 5°C, 8 g of PEPA and 3 g of triethylamine were added thereto, the mixture was stirred and dispersed, the temperature was raised to 75°C, and the reaction was carried out for 5 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with deionized water, and dried to obtain phosphorus-modified vinyl silane.

[0031] (3) Under a nitrogen atmosphere, 10 g of nano-silica was added to 100 mL of toluene solvent and ultrasonically dispersed at room temperature for 40 min. Then, 1 mol of trimethoxy(4-vinylphenyl)silane was added and reacted at 75 °C for 30 h. After the reaction, the mixture was filtered under negative pressure, washed with ethanol, and dried to obtain vinyl nano-silica.

[0032] (4) Add 40 g of butyl acrylate, 40 g of methyl methacrylate, 4 g of phosphorus-modified vinyl silane, and 4 g of vinyl nano-silica to 180 mL of deionized water, stir and disperse, then add 8 g of sodium dodecyl sulfate and 3 g of emulsifier, continue stirring and emulsifying for 80 min, after stirring, raise the temperature to 80 ° C, add 0.4 g of ammonium persulfate and 0.2 g of sodium bicarbonate, stir and react for 5 h, after the reaction is completed, cool to room temperature, use ammonia water to adjust the pH to 9, and obtain a modified polyacrylic acid emulsion.

[0033] (5) Add 3 g of dispersant and 1 g of defoamer into 50 mL of deionized water, stir and disperse, then add 50 g of modified polyacrylic acid emulsion and stir and mix evenly to obtain a modified polyacrylic acid fire retardant coating. Embodiment 2

[0034] (1) Under a nitrogen atmosphere, 12 g of (2-carboxyethyl)phenylphosphonic acid, 5 g of methylvinyldichlorosilane, and 12 g of pyridine were added to 200 mL of acetonitrile solvent, stirred and dispersed, and the mixture was heated to 70°C and stirred for 12 h. After the reaction was completed, the mixture was evaporated under reduced pressure, washed with ethanol, and dried to obtain intermediate 1.

[0035] (2) Under a nitrogen atmosphere, 10 g of intermediate 1 and 5.5 g of dichlorothionyl were added to 200 mL of acetonitrile solvent, the temperature was raised to 80°C, and the reaction was carried out for 3 h. After the reaction was completed, the mixture was cooled to 0°C, 7 g of PEPA and 6 g of triethylamine were added thereto, the mixture was stirred and dispersed, the temperature was raised to 75°C, and the reaction was carried out for 5 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with deionized water, and dried to obtain phosphorus-modified vinyl silane.

[0036] (3) Under a nitrogen atmosphere, 10 g of nano-silica was added to 100 mL of toluene solvent and ultrasonically dispersed at room temperature for 20 min. Then, 0.12 mol of trimethoxy(4-vinylphenyl)silane was added and reacted at 85 °C for 20 h. After the reaction, the mixture was filtered under negative pressure, washed with ethanol, and dried to obtain vinyl nano-silica.

[0037] (4) Add 40 g of butyl acrylate, 60 g of methyl methacrylate, 11 g of phosphorus-modified vinyl silane, and 11 g of vinyl nano-silica to 160 mL of deionized water, stir and disperse, then add 8 g of sodium dodecyl sulfate and 3 g of emulsifier, continue stirring and emulsifying for 50 min, after stirring, heat to 70 ° C, add 1.6 g of ammonium persulfate and 0.2 g of sodium bicarbonate, stir and react for 3 h, after the reaction, cool to room temperature, use ammonia water to adjust the pH to 9, and obtain a modified polyacrylic acid emulsion.

[0038] (5) Add 2 g of dispersant and 2 g of defoamer into 50 mL of deionized water, stir and disperse, then add 50 g of modified polyacrylic acid emulsion and stir and mix evenly to obtain a modified polyacrylic acid fire retardant coating. Embodiment 3

[0039] (1) Under a nitrogen atmosphere, 11 g of (2-carboxyethyl)phenylphosphonic acid, 5 g of methylvinyldichlorosilane, and 10 g of pyridine were added to 200 mL of acetonitrile solvent, stirred and dispersed, and the temperature was raised to 75°C. The mixture was stirred and reacted for 6 h. After the reaction was completed, the mixture was evaporated under reduced pressure, washed with ethanol, and dried to obtain intermediate 1.

[0040] (2) Under a nitrogen atmosphere, 10 g of intermediate 1 and 4.5 g of thionyl chloride were added to 200 mL of acetonitrile solvent, the temperature was raised to 70°C, and the reaction was carried out for 2 h. After the reaction was completed, the mixture was cooled to 5°C, 6 g of PEPA and 5 g of triethylamine were added thereto, the mixture was stirred and dispersed, the temperature was raised to 70°C, and the reaction was carried out for 4 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with deionized water, and dried to obtain phosphorus-modified vinyl silane.

[0041] (3) Under a nitrogen atmosphere, 10 g of nano-silica was added to 100 mL of toluene solvent and ultrasonically dispersed at room temperature for 50 min. Then, 2 mol of trimethoxy(4-vinylphenyl)silane was added and reacted at 80 °C for 24 h. After the reaction was completed, the mixture was filtered under negative pressure, washed with ethanol, and dried to obtain vinyl nano-silica.

[0042] (4) Add 40 g of butyl acrylate, 50 g of methyl methacrylate, 18 g of phosphorus-modified vinyl silane, and 18 g of vinyl nano-silica into 200 mL of deionized water, stir and disperse, then add 4 g of sodium dodecyl sulfate and 2 g of emulsifier, continue stirring and emulsifying for 40 min, after stirring, heat to 80 ° C, add 1 g of ammonium persulfate and 0.08 g of sodium bicarbonate, stir and react for 6 h, after the reaction is completed, cool to room temperature, use ammonia water to adjust the pH to 8, and obtain a modified polyacrylic acid emulsion.

[0043] (5) Add 2 g of dispersant and 3 g of defoamer into 50 mL of deionized water, stir and disperse, then add 50 g of modified polyacrylic acid emulsion and stir and mix evenly to obtain modified polyacrylic acid fire retardant coating. Embodiment 4

[0044] (1) Under a nitrogen atmosphere, 11 g of (2-carboxyethyl)phenylphosphonic acid, 5 g of methylvinyldichlorosilane, and 12 g of pyridine were added to 200 mL of acetonitrile solvent, stirred and dispersed, and the temperature was raised to 75°C. The reaction was stirred for 10 h. After the reaction was completed, the mixture was evaporated under reduced pressure, washed with ethanol, and dried to obtain intermediate 1.

[0045] (2) Under a nitrogen atmosphere, 10 g of the intermediate 1 and 6 g of thionyl chloride were added to 200 mL of acetonitrile solvent, the temperature was raised to 80°C, and the reaction was carried out for 3 h. After the reaction was completed, the mixture was cooled to 5°C, 7 g of PEPA and 8 g of triethylamine were added thereto, the mixture was stirred and dispersed, the temperature was raised to 80°C, and the reaction was carried out for 4 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with deionized water, and dried to obtain phosphorus-modified vinyl silane.

[0046] (3) Under a nitrogen atmosphere, 10 g of nano-silica was added to 100 mL of toluene solvent and ultrasonically dispersed at room temperature for 40 min. Then, 1.5 mol of trimethoxy(4-vinylphenyl)silane was added and reacted at 70 °C for 28 h. After the reaction, the mixture was filtered under negative pressure, washed with ethanol, and dried to obtain vinyl nano-silica.

[0047] (4) Add 40 g of butyl acrylate, 50 g of methyl methacrylate, 25 g of phosphorus-modified vinyl silane, and 25 g of vinyl nano-silica into 180 mL of deionized water, stir and disperse, then add 8 g of sodium dodecyl sulfate and 4 g of emulsifier, continue stirring and emulsifying for 60 min, after stirring, heat to 75 ° C, add 1 g of ammonium persulfate and 0.15 g of sodium bicarbonate, stir and react for 4 h, after the reaction is completed, cool to room temperature, use ammonia water to adjust the pH to 8, and obtain a modified polyacrylic acid emulsion.

[0048] (5) Add 1 g of dispersant and 2 g of defoamer into 50 mL of deionized water, stir and disperse, then add 50 g of modified polyacrylic acid emulsion and stir and mix evenly to obtain a modified polyacrylic acid fire retardant coating. Embodiment 5

[0049] (1) Under a nitrogen atmosphere, 12 g of (2-carboxyethyl)phenylphosphonic acid, 5 g of methylvinyldichlorosilane, and 12 g of pyridine were added to 200 mL of acetonitrile solvent, stirred and dispersed, and the temperature was raised to 80°C. The mixture was stirred and reacted for 9 h. After the reaction was completed, the mixture was evaporated under reduced pressure, washed with ethanol, and dried to obtain intermediate 1.

[0050] (2) Under a nitrogen atmosphere, 10 g of the intermediate 1 and 5 g of thionyl chloride were added to 200 mL of acetonitrile solvent, the temperature was raised to 75°C, and the reaction was carried out for 4 h. After the reaction was completed, the mixture was cooled to 0°C, 10 g of PEPA and 6 g of triethylamine were added thereto, the mixture was stirred and dispersed, the temperature was raised to 70°C, and the reaction was carried out for 2 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with deionized water, and dried to obtain phosphorus-modified vinyl silane.

[0051] (3) Under a nitrogen atmosphere, 10 g of nano-silica was added to 100 mL of toluene solvent and ultrasonically dispersed at room temperature for 40 min. Then, 0.1 mol of trimethoxy(4-vinylphenyl)silane was added and reacted at 85 °C for 20 h. After the reaction, the mixture was filtered under negative pressure, washed with ethanol, and dried to obtain vinyl nano-silica.

[0052] (4) Add 40 g of butyl acrylate, 60 g of methyl methacrylate, 32 g of phosphorus-modified vinyl silane, and 32 g of vinyl nano-silica into 180 mL of deionized water, stir and disperse, then add 8 g of sodium dodecyl sulfate and 2 g of emulsifier, continue stirring and emulsifying for 80 min, after stirring, heat to 80 ° C, add 1 g of ammonium persulfate and 0.2 g of sodium bicarbonate, stir and react for 6 h, after the reaction is completed, cool to room temperature, use ammonia water to adjust the pH to 9, and obtain a modified polyacrylic acid emulsion.

[0053] (5) Add 4 g of dispersant and 0.5 g of defoamer into 50 mL of deionized water, stir and disperse, then add 50 g of modified polyacrylic acid emulsion and stir and mix evenly to obtain a modified polyacrylic acid fire retardant coating.

[0054] Comparative Example 1

[0055] The difference between this comparative example and Example 1 is that in step (4), no phosphorus-modified vinyl silane is contained.

[0056] Comparative Example 2

[0057] The difference between this comparative example and Example 1 is that in step (4), no vinyl nano-silica is contained.

[0058] The coating was applied on a clean steel plate of 80 mm × 80 mm × 0.8 mm and dried at 40°C for 12 h to obtain a coating sample.

[0059] Place the coating sample 9 cm above the alcohol burner and conduct a burning experiment. Use a vernier caliper to measure the maximum thickness of the ignition point, which is the height of the expanded carbonaceous layer, and observe the foaming of the carbonaceous layer.

[0060] Table 1: Fire performance test of various embodiments and comparative examples

[0061] Carbon layer hardness Refractory time / min Carbonized layer quality Example 1 Moderate 39 Fast foaming, complete structure, loose Example 2 Moderate 46 Fast foaming, complete structure, dense Example 3 hard 52 Fast foaming, complete structure, dense Example 4 hard 59 Fast foaming, complete structure, dense Example 5 Harder 63 Fast foaming, complete structure, dense Comparative Example 1 crisp 29 Fast foaming, a small amount of cracks, relatively loose Comparative Example 2 crisp 31 Fast foaming, a small amount of cracks, relatively loose

[0062] It can be seen from the table that the fire retardant coating prepared by the present invention has a good fire retardant effect.

[0063] Use a paint film impactor to test the impact resistance of the coating.

[0064] Table 2: Impact resistance test of various embodiments and comparative examples

[0065] Impact resistance / kg·cm Example 1 30 Example 2 40 Example 3 50 Example 4 50 Example 5 45 Comparative Example 1 25 Comparative Example 2 15

[0066] It can be seen from the table that the coating prepared by the present invention has good impact resistance.

[0067] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, any slight modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a modified polyacrylic acid fire retardant coating, characterized in that: The preparation method is as follows: (1) Add butyl acrylate, methyl methacrylate, phosphorus-modified vinyl silane, and vinyl nano-silica to deionized water, stir and disperse, then add sodium dodecyl sulfonate and an emulsifier, continue stirring and emulsifying for 40-80 minutes, after the stirring is completed, heat to 70-80° C., add ammonium persulfate and sodium bicarbonate, stir and react for 3-6 hours, after the reaction is completed, cool to room temperature, and use ammonia water to adjust the pH to 8-9 to obtain a modified polyacrylic acid emulsion. The preparation method of the phosphorus-modified vinyl silane is as follows: S1. Under a nitrogen atmosphere, add (2-carboxyethyl)phenylphosphonic acid, methylvinyldichlorosilane and pyridine to an acetonitrile solvent, stir and disperse, heat to 70-85° C., stir and react for 6-12 hours. After the reaction is completed, distill under reduced pressure, wash with ethanol, and dry to obtain intermediate 1. S2. Under a nitrogen atmosphere, add intermediate 1 and thionyl chloride to acetonitrile solvent, heat to 70-80°C, react for 2-4 hours, cool to 0-5°C after the reaction, add PEPA and triethylamine, stir and disperse, heat to 70-80°C, react for 2-5 hours, cool to room temperature after the reaction, filter, wash with deionized water, and dry to obtain phosphorus-modified vinyl silane; (2) adding a dispersant and a defoaming agent into deionized water, stirring and dispersing the mixture, and then adding the modified polyacrylic acid emulsion into the deionized water and stirring and mixing the mixture evenly to obtain a modified polyacrylic acid fire retardant coating.

2. The method for preparing the modified polyacrylic acid fire retardant coating according to claim 1, characterized in that: In the step (1), the usage ratio of butyl acrylate, methyl methacrylate, phosphorus-modified vinyl silane, vinyl nano-silica, sodium dodecyl sulfonate, emulsifier, ammonium persulfate and sodium bicarbonate is 100g:(100-150)g:(10-80)g:(10-80)g:(10-20)g:(5-10)g:(1-4)g:(0.2-0.5)g.

3. The method for preparing the modified polyacrylic acid fire retardant coating according to claim 1, characterized in that: In the step (2), the usage ratio of the dispersant, the defoaming agent and the modified polyacrylic acid emulsion is (2-8) g: (1-6) g: 100 g.

4. The method for preparing the modified polyacrylic acid fire retardant coating according to claim 1, characterized in that: In the S1, the usage ratio of (2-carboxyethyl)phenylphosphonic acid, methylvinyldichlorosilane and pyridine is (2-2.4) g: 1 g: (2-2.6) g.

5. The method for preparing the modified polyacrylic acid fire retardant coating according to claim 1, characterized in that: In S2, the usage ratio of intermediate 1, thionyl chloride, PEPA and triethylamine is 1 g: (0.45-0.6) g: (0.6-1) g: (0.5-0.8) g.

6. The method for preparing the modified polyacrylic acid fire retardant coating according to claim 1, characterized in that: In the step (1), the preparation method of vinyl nano-silica is as follows: under a nitrogen atmosphere, nano-silica is added to a toluene solvent, and ultrasonically dispersed for 20-50 minutes at room temperature, and then trimethoxy (4-vinylphenyl) silane is added thereto, and reacted at 75-85° C. for 20-30 hours. After the reaction is completed, negative pressure filtration is performed, ethanol washing is performed, and drying is performed to obtain vinyl nano-silica.