Phase difference film, display device and method for preparing phase difference film

By using a retardation film generated by reverse dispersion rod-shaped liquid crystal polymerization in a display device, the liquid crystal molecules have twisted and gradually tilted orientations in the thickness direction, which solves the problem of reduced anti-reflective performance of circular polarizers at tilted viewing angles and achieves Good optical performance at different viewing angles improves the display effect.

CN118534694BActive Publication Date: 2024-10-29CHENGDU RAYBOCH MATERIAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411010534.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-29
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The anti-reflective performance of existing circular polarizers decreases when the viewing angle is tilted, resulting in reduced visibility and contrast of the display panel, affecting the display effect.

Method used

A retardation film generated by reverse dispersion rod-shaped liquid crystal polymerization is used. The liquid crystal molecules have twisted orientation and gradient tilt orientation in the thickness direction. The twist orientation combined with the gradient tilt orientation improves viewing angle dependence and improves optical performance.

Benefits of technology

The phase difference film maintains good optical properties under different viewing angles, improves the reflectivity and visibility of the display device, and improves the display effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118534694B_ABST
    Figure CN118534694B_ABST
Patent Text Reader

Abstract

The phase difference film, display device and preparation method of the phase difference film provided in the present application relate to the technical field of optical materials. The phase difference film is generated by polymerization of inversely dispersed rod-shaped liquid crystals. The liquid crystal arrangement of the liquid crystal molecules in the phase difference film has a twisted orientation in the thickness direction and a gradually inclined orientation in the thickness direction. The viewing angle dependence can be effectively improved by combining the twisted orientation with the gradually inclined orientation, so that the phase difference film can maintain good optical properties at different viewing angles, thereby improving the optical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of optical materials, and in particular to a phase difference film, a display device, and a method for preparing the phase difference film. Background Art

[0002] In recent years, light-emitting devices (such as organic light-emitting devices OLED) have developed rapidly in the display field due to their unique advantages, such as self-luminescence, high contrast, flexibility, and ultra-thinness. However, due to the influence of the current device structure design of light-emitting devices, the corresponding display panel cathode usually uses silver and other metals, which can reflect external light, resulting in reduced visibility and contrast, affecting the display effect. In order to reduce the influence of external light, a layer of circular polarizer can be attached to the display panel.

[0003] However, the circular polarizers currently developed have viewing angle dependence, especially at tilted viewing angles, where their anti-reflection performance decreases and visibility at large viewing angles is reduced, thereby affecting the display effect of the display device. Summary of the invention

[0004] The present application provides a phase difference film, a display device and a method for preparing the phase difference film, which can effectively improve the viewing angle dependence, so that the phase difference film can maintain good optical properties at different viewing angles, thereby improving the optical performance. The technical solution is as follows.

[0005] On the one hand, a phase difference film is provided, which is generated by polymerization of inversely dispersed rod-shaped liquid crystals, and the liquid crystal arrangement of liquid crystal molecules in the phase difference film has a twisted orientation in the thickness direction and a gradually tilted orientation in the thickness direction.

[0006] On the other hand, a display device is provided, which includes a linear polarizer layer, a phase difference film layer corresponding to the phase difference film, and a display panel layer arranged in sequence;

[0007] The first side of the phase difference film layer is a side close to the display panel layer;

[0008] The second side of the phase difference film layer is a side close to the linear polarizer layer;

[0009] The azimuth angle of the phase difference film is the angle between the direction of the director of the liquid crystal molecules projected in the film plane and the absorption axis of the linear polarizer layer.

[0010] On the other hand, a method for preparing a phase difference film is provided, wherein the method is used to prepare the phase difference film; the method comprises:

[0011] Pre-treating the coating surface of the substrate;

[0012] Based on the twist angle and tilt angle of the phase difference film, coating an alignment layer on the pre-treated substrate;

[0013] A liquid crystal layer having an alignment is coated on the alignment layer based on the thickness of the phase difference film.

[0014] The phase difference film provided in the present application is generated by polymerization of inversely dispersed rod-shaped liquid crystals. The liquid crystal molecules in the phase difference film have a twisted orientation in the thickness direction and a gradually tilted orientation in the thickness direction. The viewing angle dependence can be effectively improved by combining the twisted orientation with the gradually tilted orientation, so that the phase difference film can maintain good optical properties at different viewing angles, thereby improving the optical performance.

[0015] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0017] Figure 1 A schematic diagram of a phase difference film provided by an exemplary embodiment of the present application is shown;

[0018] Figure 2 A side view showing a change of a liquid crystal director provided by an exemplary embodiment of the present application;

[0019] Figure 3 A top view showing a change of a liquid crystal director provided by an exemplary embodiment of the present application is shown;

[0020] Figure 4 A side view showing a change of another liquid crystal director provided by an exemplary embodiment of the present application;

[0021] Figure 5 A top view showing a change of another liquid crystal director provided by an exemplary embodiment of the present application is shown;

[0022] Figure 6 A flow chart showing a method for preparing a phase difference film provided by an exemplary embodiment of the present application is shown;

[0023] Figure 7 A schematic diagram showing the angle change of a gradually tilted and twisted director provided by an exemplary embodiment of the present application is shown;

[0024] Figure 8 A schematic diagram of a weight function provided by an exemplary embodiment of the present application is shown;

[0025] Fig. 9 A schematic structural diagram of a display device provided by an exemplary embodiment of the present application is shown. DETAILED DESCRIPTION

[0026] Here, exemplary embodiments are described in detail, and examples thereof are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The implementations described in the following exemplary embodiments do not represent all implementations consistent with the present application.

[0027] The embodiment of the present application provides a phase difference film, which can effectively improve the reflectivity when viewed at an oblique viewing angle. When applied to a display device, it can improve the integrated black effect of the display device and improve visibility. Figure 1 A schematic diagram of a phase difference film provided by an exemplary embodiment of the present application is shown in FIG. Figure 1 As shown, the phase difference film 100 is generated by polymerization of inversely dispersed rod-shaped liquid crystals, and the liquid crystal arrangement of the liquid crystal molecules in the phase difference film has a twisted orientation in the thickness direction and a gradually tilted orientation in the thickness direction.

[0028] The phase difference film can be a rod-shaped liquid crystal polymer (LCP) with twisted orientation in the thickness direction and gradually tilted orientation in the thickness direction, and its corresponding liquid crystal uses reverse wavelength dispersion (RWD) LCP. Twisted orientation refers to the fact that the long axis direction of the rod-shaped liquid crystal molecules is twisted to a certain extent in the thickness direction of the film, forming a spiral arrangement. This structure can effectively change the polarization state of the incident light and produce the desired phase delay effect. Gradual tilt orientation refers to the gradual change of the tilt angle of the liquid crystal molecules in the thickness direction of the film, forming a gradient of tilt angle from one side to the other. This structure can further optimize the propagation path of light in the phase difference film, and can make the phase delay of the phase difference film at an inclined viewing angle close to that at a normal viewing angle, so as to achieve more precise optical performance regulation.

[0029] The liquid crystal used in the phase difference film in the embodiment of the present application is a rod-shaped liquid crystal material with birefringence, and its birefringence phase difference satisfies the following equation:

[0030]

[0031] Wherein, dn(λ) is the refractive index difference of the liquid crystal at a wavelength of λ nm, ne is the refractive index parallel to the slow axis of the liquid crystal (direction of the director), and no is the refractive index perpendicular to the slow axis of the liquid crystal.

[0032] Liquid crystals can be classified into positive dispersion liquid crystal type or reverse dispersion liquid crystal type, wherein positive dispersion refers to a liquid crystal type in which the refractive index difference dn(λ) decreases as the wavelength λ increases, satisfying Formula 1:

[0033]

[0034] Inverse dispersion refers to a type of liquid crystal in which the refractive index difference dn(λ) increases with the increase of wavelength λ, satisfying Formula 2:

[0035]

[0036] The rod-shaped liquid crystal used in the embodiments of the present application is a reverse dispersed liquid crystal, and its dn(450) / dn(550) value can be 0.8 to 0.99, and further, can be 0.8 to 0.85; the dn(650) / dn(550) value can be 1 to 1.2, and further, can be 1 to 1.05.

[0037] Schematically, the polymerizable reverse-dispersive rod-shaped liquid crystal material used in the phase difference film may have a monomer formula that can be realized as any one of the following:

[0038] RWD-1:

[0039]

[0040] RWD-2:

[0041]

[0042] RWD-3:

[0043]

[0044] RWD-4:

[0045]

[0046] RWD-5:

[0047]

[0048] It should be noted that the general formula of the reverse dispersed liquid crystal monomer includes but is not limited to the above-mentioned situations, and can be implemented as any of the above-mentioned forms, or can also be implemented in other forms, and the present application does not limit this.

[0049] In the embodiment of the present application, the changes in the tilt angle and azimuth angle of the liquid crystal molecules in the phase difference film 100 are nonlinear changes; the tilt angle is the angle between the liquid crystal molecule director and the film plane of the phase difference film, and the azimuth angle is the angle between the direction of the liquid crystal molecule director projected in the film plane and the selected reference direction. By setting the nonlinear changes in the tilt angle and azimuth angle, it is possible to achieve non-uniform phase delay of light waves and optimize the propagation characteristics of light waves in the phase difference film, wherein the nonlinear change means that as the film thickness increases, the tilt angle or azimuth angle of the liquid crystal molecules does not change uniformly in proportion, but presents a more complex change pattern, for example, first fast and then slow, or first slow and then fast, or there may be a sudden change or reversal in certain thickness ranges.

[0050] In a possible implementation, the present application embodiment provides the following optional phase difference film design method:

[0051] Design 1:

[0052] The tilt angle of the liquid crystal molecules on the first side of the phase difference film is in the range of -20 to 20°. Furthermore, the tilt angle may be in the range of -10 to 10°, and gradually tilts along the thickness direction.

[0053] The tilt angle of the liquid crystal molecules on the second side of the phase difference film is in the range of 20° to 70°, and further, the tilt angle may be in the range of 35° to 55°;

[0054] The angle range of the azimuth angle of the liquid crystal molecules on the second side of the phase difference film is -10° to 40°, and further, the angle range can be 10° to 30°;

[0055] The twist angle of the liquid crystal molecules of the phase difference film is in the range of 10° to 70°, and further, the angle range can be 30° to 50°; the twist angle is the angle of rotation of the azimuth angle in the film plane;

[0056] The delay value of the phase difference film at a wavelength of 550nm ranges from 150nm to 260nm. Further, the value range can be 170nm to 235nm. The delay value is the delay value of the phase difference film at the corresponding wavelength. The product of the value of and the thickness of the retardation film, that is, the delay of the retardation film at a wavelength of 550nm is the thickness multiplied by its value at a wavelength of 550nm. The value of , where ne and no are the non-trivial refractive index and the ordinary refractive index of the rod-like liquid crystal, respectively;

[0057] The change of the tilt angle is nonlinear, that is, the change of the tilt angle in the unit delay is not fixed. Optionally, the change of the tilt angle of the liquid crystal molecules in the phase difference film in the unit delay is in the range of 0.07° / nm to 0.30° / nm. Further, the range can be 0.18° / nm to 0.28° / nm.

[0058] The change in azimuth angle is also nonlinear, that is, the change in azimuth angle per unit delay is not fixed. Optionally, the change in azimuth angle of the liquid crystal molecules in the phase difference film per unit delay ranges from 0.06° / nm to 0.30° / nm. Further, the range can be 0.10° / nm to 0.27° / nm.

[0059] It should be noted that the value ranges of the various structural parameters in Design 1 are mutually compatible. Optionally, based on different actual needs, the phase difference film can be designed with different structural parameter values ​​within the value ranges of the various structural parameters indicated in Design 1. Taking the phase difference film as an example, Figure 2 A side view showing a change in a liquid crystal director provided by an exemplary embodiment of the present application is shown. Figure 3 FIG. 1 is a top view showing a change in a liquid crystal director provided by an exemplary embodiment of the present application. Figure 2 and Figure 3 As shown, the phase difference film generated based on the value range of each structural parameter shown in Design 1 has a nonlinear increase in tilt angle from the first side to the second side and a nonlinear change in azimuth angle.

[0060] Design 2:

[0061] The tilt angle of the liquid crystal molecules on the second side of the phase difference film is in the range of -20 to 20°. Furthermore, the tilt angle may be in the range of -10 to 10°, and gradually tilts along the thickness direction.

[0062] The tilt angle of the liquid crystal molecules on the first side of the phase difference film is in the range of 20° to 50°, and further, the tilt angle may be in the range of 30° to 45°;

[0063] The angle range of the azimuth angle of the liquid crystal molecules on the first side of the phase difference film is -15° to 40°, and further, the angle range may be -10° to 10°;

[0064] The twist angle of the liquid crystal molecules of the phase difference film is in the range of 15° to 80°, and further, the angle range can be 45° to 75°; the twist angle is the angle of rotation of the azimuth angle in the film plane;

[0065] The delay value of the phase difference film at a wavelength of 550nm ranges from 145nm to 340nm, and further, the value range may be from 190nm to 300nm;

[0066] The change of the tilt angle is nonlinear, that is, the change of the tilt angle in the unit delay is not fixed. Optionally, the change of the tilt angle of the liquid crystal molecules in the phase difference film in the unit delay is in the range of 0.10° / nm to 0.27° / nm. Further, the range can be 0.11° / nm to 0.22° / nm.

[0067] The change in azimuth angle is also nonlinear, that is, the change in azimuth angle per unit delay is not fixed. Optionally, the change in azimuth angle of the liquid crystal molecules in the phase difference film per unit delay ranges from 0.04° / nm to 0.35° / nm. Further, the range can be 0.20° / nm to 0.32° / nm.

[0068] It should be noted that the value ranges of the various structural parameters in Design 2 are mutually compatible. Optionally, based on different actual needs, the phase difference film can be designed with different structural parameter values ​​within the value ranges of the various structural parameters indicated in Design 2. Taking the phase difference film as an example, the phase difference film is set based on the value ranges of the various structural parameters provided in Design 2. Figure 4 A side view showing a change in a liquid crystal director provided by an exemplary embodiment of the present application is shown. Figure 5 FIG. 1 is a top view showing a change in a liquid crystal director provided by an exemplary embodiment of the present application. Figure 4 and Figure 5 As shown, the phase difference film generated based on the value range of each structural parameter shown in Design 2 has a nonlinear decrease in tilt angle from the first side to the second side and a nonlinear change in azimuth angle.

[0069] In the embodiment of the present application, the values ​​of the structural parameters in the phase difference film are determined when the reflectivity of the phase difference film is minimized, and the structural parameters include the thickness, twist angle and tilt angle of the phase difference film. In other words, the values ​​of the structural parameters of the phase difference film can minimize the reflectivity of the phase difference film.

[0070] In summary, the phase difference film provided in the embodiment of the present application is generated by the polymerization of inversely dispersed rod-shaped liquid crystals, and the liquid crystal molecules in the phase difference film have a twisted orientation in the thickness direction and a gradually tilted orientation in the thickness direction; the viewing angle dependence can be effectively improved by combining the twisted orientation with the gradually tilted orientation, so that the phase difference film can maintain good optical properties at different viewing angles, thereby improving the optical performance.

[0071] Figure 6A flow chart showing a method for preparing a phase difference film provided by an exemplary embodiment of the present application is shown. The method is used to prepare Figure 1 The phase difference film shown in the embodiment, the method can be performed by a phase difference film preparation system, and the phase difference film preparation method may include:

[0072] Step 610, pre-treating the coating surface of the substrate.

[0073] Pre-treatment of the coated surface of the substrate includes, but is not limited to, cleaning, drying or plasma treatment, etc.

[0074] The substrate may be a flat plate or a curved plate.

[0075] Step 620 , coating an alignment layer on the pre-treated substrate based on the twist angle and tilt angle of the phase difference film.

[0076] The method forms an alignment layer on the pre-treated substrate, comprising: coating an alignment layer solution on the substrate, and drying and exposing the alignment layer solution.

[0077] Among them, the drying temperature in the drying process can be 80°C to 120°C, and the drying time can be 30s to 180s; the UV exposure in the exposure process can be 5mJ to 300mJ equivalent, and during the exposure, linearly polarized or non-polarized UVB ultraviolet light can be used for exposure at a normal or oblique viewing angle. The exposure process can be a single exposure, or the total exposure dose can be divided into two or more times and exposed in sequence.

[0078] When forming the alignment layer, it is necessary to process the alignment layer based on the twist angle and tilt angle requirements of the phase difference film to generate corresponding directional forces to guide the arrangement direction of the liquid crystal molecules; wherein, the alignment layer can be processed by friction, and the initial orientation of the liquid crystal molecules can be set by controlling the direction, angle or polarization direction of the friction or the optical alignment; optionally, more complex orientation structures can be achieved through multi-layer coating, multi-step friction or the use of special optical alignment modes, including twisted or tilted orientations.

[0079] The coating method of the alignment layer solution may be any one of the following methods: rod coating, blade coating, Roll to Roll coating or slit coating.

[0080] Step 630 : coating a liquid crystal layer with an alignment on the alignment layer based on the thickness of the phase difference film.

[0081] Coating a liquid crystal layer having an alignment on the alignment layer comprises:

[0082] Based on the thickness of the phase difference film, a liquid crystal solution is coated on the alignment layer to form a liquid crystal layer with a spiral structure of a horizontal or oblique plane. The liquid crystal solution contains an inversely dispersed liquid crystal monomer and a chiral agent; wherein the chiral agent refers to a compound with a chiral structure that can distort the liquid crystal, for example, the chiral agent can be LC756, etc.

[0083] During the coating process of the liquid crystal solution, the liquid crystal is anchored by the alignment layer and forms a tilted alignment on the side adjacent to the alignment layer; affected by the surface tension, it tends to be horizontally aligned on the side adjacent to the air; affected by the chiral agent, it forms a spiral structure along the thickness direction of the film; affected by its own unfolding, twisting, and bending single-row potential energy, the tilt angle and azimuth angle per unit thickness change nonlinearly to minimize the single-row potential energy.

[0084] The liquid crystal solution may be coated by any of the following methods: rod coating, blade coating, roll to roll coating or slit coating.

[0085] After the liquid crystal solution is coated, the coated liquid crystal layer is dried, cooled and partially pre-cured to form an anisotropic polymer film layer.

[0086] Among them, pre-curing is achieved by using a standard curing amount, that is, in the process of curing based on the standard curing amount, by limiting the curing time or the form of curing energy, the liquid crystal layer reaches a partially cured state. In the partially cured state, the liquid crystal layer has a certain physical and chemical stability, but has not yet reached its final performance state, so as to facilitate subsequent adjustments.

[0087] The drying temperature when drying the liquid crystal solution can be set below the clearing point temperature of the liquid crystal, which is the temperature at which the liquid crystal changes from its ordered liquid crystal phase to a disordered isotropic liquid phase; the drying temperature can be 50°C to 120°C, and the drying time can be 60s to 300s.

[0088] Afterwards, the dried liquid crystal layer is exposed; the exposure process can be carried out under the protection of an inert gas, the UV exposure during the exposure process can be 300mJ to 3000mJ equivalent, and the radiation source can be an LED (Light Emitting Diode) or a mercury lamp with a main wavelength of 313nm and 365nm.

[0089] For the finished phase difference film, inside the phase difference film, the liquid crystal is anchored by the alignment layer, forming a tilted alignment on the side of the adjacent alignment layer; affected by surface tension, it tends to be horizontally aligned on the side adjacent to the air; affected by the chiral agent, a spiral structure is formed along the film thickness direction; affected by its own unfolding, twisting, and bending elastic potential energy, the tilt angle and azimuth angle per unit thickness change nonlinearly to minimize the elastic potential energy, and the final liquid crystal director is a gradually tilted and twisted arrangement.

[0090] Figure 7 FIG. 4 shows a schematic diagram of the angle change of the gradually tilted and twisted director provided by an exemplary embodiment of the present application. Figure 7 As shown, the flexure, twisting, and bending elastic constants of the liquid crystal are K11=13.2pN, K22=6.5pN, and K33=18.3pN respectively (this value is within the range of elastic coefficients of common liquid crystal molecules). The side of the liquid crystal close to the alignment layer is strongly aligned (that is, the liquid crystal molecule director is locked to the tilted orientation angle of the alignment layer), and the side of the liquid crystal away from the alignment layer is locked to a horizontal orientation due to surface tension. Based on the liquid crystal optical simulation software, the director simulation can be performed to obtain the changes in the liquid crystal tilt angle and azimuth angle in the thickness direction. Figure 7 As shown, the changes in the tilt angle and azimuth angle are nonlinear, that is, the changes in the tilt angle and azimuth angle per unit film thickness are not constant.

[0091] The preparation system may include a preparation device for a phase difference film, which is used to perform steps 610 to 630. The preparation device may be implemented as a robotic arm or an automated assembly line. The preparation system may also include a computer device, which is used to instruct the preparation device to manufacture the phase difference film, and, before preparing the phase difference film, pre-optimize and determine the structural parameters of the phase difference film, wherein the structural parameters include thickness, distortion, and tilt angle, etc., so as to guide the preparation of the phase difference film based on the determined structural parameters of the phase difference film. The process of determining the structural parameters of the phase difference film may be implemented as follows:

[0092] Taking the structural parameters of the phase difference film as optimization variables and the weighted average reflectivity as optimization indicators, the structural parameters of the phase difference film with the smallest weighted average reflectivity are determined as the optimized structural parameters of the phase difference film; the structural parameters include thickness, twist angle and tilt angle;

[0093] The calculation of the weighted average reflectivity includes:

[0094] Based on optical simulation, the reflectivity of the phase difference film under different wavelengths and different incident angles of non-polarized light is calculated;

[0095] Based on a wavelength-related weight function, the reflectivity of the phase difference film for non-polarized light incident at different wavelengths and different incident angles is weighted averaged to obtain a weighted average reflectivity; the weight function is obtained by multiplying the luminosity function after the hue requirement is translated along the wavelength direction and the natural light spectrum; the weight functions under different hue requirements correspond to different peak wavelengths.

[0096] The process of determining the structural parameters of the phase difference film can be performed by a computer device, which uses optical simulation software to simulate the reflectivity of non-polarized light incident on the phase difference film at different wavelengths and incident angles. Schematically, the optical simulation software can be FDTD (Finite-Difference Time-Domain) software, or RCWA (Rigorous Coupled Wave Analysis) software, but is not limited thereto; wherein the value ranges of different wavelengths and incident angles can be set based on actual needs, for example, the values ​​of different wavelengths can cover the entire visible spectrum to comprehensively evaluate the optical performance of the phase difference film under different conditions. The phase difference film has initial structural parameters, such as initial thickness, initial twist angle, and initial tilt angle.

[0097] Before calculating the weighted average reflectance, it is necessary to construct a weight function, which is obtained based on the product of the hue requirement and the natural light spectrum. The hue requirement can be reflected by translating the photometric function along the wavelength direction; the photometric function can be the Y(λ) in the color matching function specified in the CIE (Commission Internationale de l'Eclairage, International Commission on Illumination) 1931 color space, which is used to characterize the sensitivity of the human eye to different wavelengths.

[0098] When the hue requirement indicates a warm hue requirement, the luminosity function is translated toward the blue light direction until the peak wavelength of the luminosity function is the target wavelength indicated by the hue requirement; when the hue requirement indicates a cold hue requirement, the luminosity function is translated toward the red light direction until the peak wavelength of the luminosity function is the target wavelength indicated by the hue requirement; that is, if the hue requirement prefers a warm hue, that is, if the final light leakage is desired to be reddish, the luminosity function is translated toward the blue light direction, so that when the reflectivity is optimized based on the corresponding weight function, due to the higher weight corresponding to the blue light direction, the reflectivity of the blue light will be minimized first, so that the reflected light will be reddish, thereby achieving the effect of reddish light leakage (i.e., warm hue); if the hue requirement prefers a cold hue, that is, if the final light leakage is desired to be blue, the luminosity function is translated toward the red light direction, so that when the reflectivity is optimized based on the corresponding weight function, due to the higher weight corresponding to the red light direction, the reflectivity of the red light will be minimized first, so that the reflected light will be blued, thereby achieving the effect of blue light leakage (i.e., cold hue).

[0099] Optionally, the CIE standard illuminant D65 can be taken as the natural light spectrum; after multiplying the luminosity function after the wavelength shift based on the hue requirement with the natural light spectrum, the final weight function is obtained. For example, the target wavelengths indicated by the hue requirement are 520nm, 550nm, and 580nm respectively. Figure 8 A schematic diagram of a weight function provided by an exemplary embodiment of the present application is shown. Figure 8 As shown, after translating the luminosity function by different distances and multiplying it with the natural light spectrum based on the above method, weight functions with peak wavelengths at 520nm, 550nm, and 580nm are obtained, and each weight function is used to indicate the weight value corresponding to each wavelength at the corresponding peak wavelength.

[0100] After obtaining the weight function, the reflectivity of the initial phase difference film for non-polarized light incident at different wavelengths and different incident angles is weighted averaged based on the weight values ​​of each wavelength at the corresponding peak wavelength indicated by the weight function, and an indicator that can comprehensively evaluate the overall reflective performance of the phase difference film, namely the weighted average reflectivity, is obtained to avoid the influence of wavelength and incident angle on the subsequent structural parameter optimization process.

[0101] The structural parameters of the phase difference film are used as optimization variables, and several groups of structural parameters are randomly generated through an algorithm. For each group of phase difference films with structural parameters, the above optical simulation calculation and weighted average reflectivity calculation process are repeated. After multiple rounds of parameter optimization and comparison, a group of structural parameters that minimize the weighted average reflectivity can be obtained. The structural parameters are determined as the optimized structural parameters of the phase difference film, and the manufacturing of the phase difference film is guided based on the optimized result parameters.

[0102] Among them, a genetic algorithm can be used when performing parameter optimization, that is, for several groups of structural parameters, several groups of structural parameters with the smallest weighted average reflectivity are selected as the parents of the next generation, and new structural parameters are generated through crossover and mutation, and the optimization process is continued until the weighted average reflectivity is minimized. Alternatively, parameter optimization can also use optimization algorithms such as gradient descent and particle swarm optimization, which are not limited in this application.

[0103] In summary, the preparation method of the phase difference film provided in the embodiment of the present application is, during the process of manufacturing the phase difference film, pre-treating the coated surface of the substrate, coating an alignment layer on the pre-treated substrate based on the twist angle and tilt angle of the phase difference film, and coating an aligned liquid crystal layer on the alignment layer based on the thickness of the phase difference film; through the above method, a phase difference film can be manufactured in which the corresponding liquid crystal molecules have a twisted orientation in the thickness direction and a gradually tilted orientation in the thickness direction, so that the produced phase difference film can maintain good optical properties at different viewing angles, thereby improving the optical performance.

[0104] Furthermore, before manufacturing the phase difference film, a weight function with peak values ​​at different wavelengths is used to optimize the optical design of the phase difference film, so that different reflection hues can be obtained.

[0105] The phase difference film provided in the embodiment of the present application can be applied to a display device to enhance the integrated black effect of the display device and improve visibility; Fig. 9 FIG. 1 shows a schematic diagram of a structure of a display device provided by an exemplary embodiment of the present application. Fig. 9 As shown, the display device includes a linear polarizing layer 200, as shown in FIG. Figure 1 The phase difference film of the illustrated embodiment corresponds to the phase difference film layer 100 and the display panel layer 300 .

[0106] like Fig. 9 As shown, the phase difference film layer 100 is located between the linear polarizer layer 200 and the display panel layer 300, wherein the display panel layer can be implemented as a display device such as an organic light-emitting device (Organic Light-Emitting Diode, OLED), a liquid crystal display device (Liquid Crystal Display, LCD), etc. The phase difference film layer can be combined with the linear polarizer layer as an anti-reflection structure of the display panel layer.

[0107] The phase difference film layer 100 and the display panel layer 300 are bonded together via an adhesive layer, wherein the adhesive layer may be made of UV adhesive, pressure sensitive adhesive, etc.

[0108] The liquid crystal type of the phase difference film layer is reverse dispersed rod-shaped liquid crystal.

[0109] The linear polarizer layer is a device that converts incident light into linearly polarized light. The linear polarizer can be an absorptive polarizer, for example, a polymer stretched film (such as polyvinyl alcohol (PVA)) dyed with iodine ions; or, the linear polarizer can also be a polarizer formed by coating anisotropic dye liquid crystals. In addition, the linear polarizer can also be implemented in other forms, which is not limited in the embodiments of the present application.

[0110] With respect to the display panel layer and the linear polarizer layer, the first side of the phase difference film layer is the side close to the display panel layer, and the second side is the side close to the linear polarizer layer. Based on this, corresponding to the design 1 of the phase difference film, the design of the phase difference film layer can be:

[0111] The inclination angle of the phase difference film layer close to the display panel layer is -20~20°, and further, the value range is -10~10°, and it is gradually inclined along the thickness direction;

[0112] The tilt angle of the phase difference film layer close to the linear polarizer layer ranges from 20° to 70°, and further ranges from 35° to 55°;

[0113] The azimuth angle of the phase difference film layer close to the linear polarizer layer ranges from -10° to 40°, and further, ranges from 10° to 30°;

[0114] The twist angle of the phase difference film layer ranges from 10° to 70°, and further, ranges from 30° to 50°;

[0115] The retardation of the phase difference film at 550nm, that is, the film thickness multiplied by its (ne-no) at 550nm, has a value range of 150nm~260nm, and further, a value range of 170nm~235nm;

[0116] The change of the tilt angle is nonlinear, that is, the change of the tilt angle in the unit delay is not constant, and its value range is 0.07° / nm~0.30° / nm, and further, the value range is 0.18° / nm~0.28° / nm;

[0117] Similarly, the change in azimuth angle is also nonlinear, that is, the change in azimuth angle per unit delay is not constant, and its value range is 0.06° / nm~0.30° / nm, and further, its value range is 0.10° / nm~0.27° / nm.

[0118] The weight function for optimizing the above parameters is: take Y(λ) in the color matching function specified in the CIE 1931 color space as the photometric function (i.e., the sensitivity of the human eye to different wavelengths); take the CIE standard illuminant D65 as the natural light spectrum, multiply it by the photometric function, and obtain the final weight function; in Example 1, the peak value of the weight function is at 550nm.

[0119] Alternatively, in Example 2, the luminosity function is shifted a certain distance toward blue light and then multiplied by the D65 spectrum, and the peak value of the obtained weight function is located at 520 nm.

[0120] Alternatively, in Example 3, the luminosity function is shifted a certain distance toward red light and then multiplied by the D65 spectrum, and the peak value of the obtained weighting function is located at 580 nm.

[0121] In addition, based on different actual needs, the above parameters can also be optimized through weight functions located at other wavelengths, and this application does not limit this.

[0122] Corresponding to the design 2 of the phase difference film, the design of the phase difference film layer can be:

[0123] The inclination angle of the phase difference film layer close to the linear polarizer layer is -20°~20°, and further, the value range is -10~10°, and gradually inclined along the thickness direction;

[0124] The tilt angle of the phase difference film layer close to the display panel layer ranges from 20° to 50°, and further ranges from 30° to 45°;

[0125] The azimuth angle of the phase difference film layer close to the linear polarizer layer ranges from -15° to 40°, and further, ranges from -10° to 10°;

[0126] The twist angle of the phase difference film layer ranges from 15° to 80°, and further, ranges from 45° to 75°;

[0127] The delay amount of the phase difference film layer at 550nm, that is, the film thickness multiplied by its (ne-no) at 550nm, ranges from 145nm to 340nm, and further, ranges from 190nm to 300nm.

[0128] The change of the tilt angle is nonlinear, that is, the change of the tilt angle in the unit delay is not constant, and its value range is 0.10° / nm~0.27° / nm, and further, the value range is 0.11° / nm~0.22° / nm.

[0129] Similarly, the change in azimuth angle is also nonlinear, that is, the change in azimuth angle per unit delay is not constant, and its value range is 0.04° / nm~0.35° / nm, and further, its value range is 0.20° / nm~0.32° / nm.

[0130] The weight function for optimizing the above parameters is: take Y(λ) in the color matching function specified in the CIE 1931 color space as the photometric function (i.e., the sensitivity of the human eye to different wavelengths); take the CIE standard illuminant D65 as the natural light spectrum, multiply it by the photometric function, and obtain the final weight function; in Example 4, the peak value of the weight function is at 550nm.

[0131] Alternatively, in Example 5, the luminosity function is shifted a certain distance toward blue light and then multiplied by the D65 spectrum, and the peak value of the obtained weight function is located at 520 nm.

[0132] Alternatively, in Example 6, the luminosity function is shifted a certain distance toward red light and then multiplied by the D65 spectrum, and the peak value of the obtained weighting function is located at 580 nm.

[0133] In addition, based on different actual needs, the above parameters can also be optimized through weight functions located at other wavelengths, and this application does not limit this.

[0134] Comparative examples are set up for comparison with the design of the phase difference film provided in the present application, wherein the value ranges of the parameters of the phase difference film layer in Comparative Examples 1, 2, and 3 are mostly consistent with the value ranges of the parameters of the phase difference film layer in Example 1.

[0135] Among them, in Comparative Example 1, the delay amount of the phase difference film layer at 550nm is not within the range of 150nm~260nm.

[0136] In Comparative Example 2, the tilt angle of the phase difference film layer close to the linear polarizer layer is not within the range of 20° to 70°. Accordingly, the variation of the tilt angle per unit retardation is also outside the range of 0.07° / nm to 0.30° / nm.

[0137] In Comparative Example 3, the twist angle of the phase difference film layer is not within the range of 10° to 70°. Accordingly, the variation of the azimuth angle in the unit delay is also outside the range of 0.06° / nm to 0.30° / nm.

[0138] The value ranges of the parameters of the phase difference film layer in Comparative Examples 4, 5, and 6 are mostly consistent with the value ranges of the parameters of the phase difference film layer in Example 2.

[0139] In Comparative Example 4, the retardation of the phase difference film layer at 550 nm is not within the range of 145 nm to 340 nm.

[0140] In Comparative Example 5, the tilt angle of the phase difference film layer close to the display panel layer is not within the range of 20° to 50°. Accordingly, the change in the tilt angle per unit delay is also outside the range of 0.10° / nm to 0.27° / nm.

[0141] In Comparative Example 6, the twist angle of the phase difference film layer is not within the range of 15° to 80°. Accordingly, the variation of the azimuth angle in the unit delay is also outside the range of 0.04° / nm to 0.35° / nm.

[0142] The above-mentioned embodiments and comparative examples were simulated based on liquid crystal optical simulation software. Taking the display panel as an OLED panel as an example, the simulation structures are linear polarizer, phase difference film, and OLED panel from top to bottom. The light source is incident from the side of the linear polarizer away from the phase difference film, and is incident on the OLED panel after passing through the linear polarizer and the phase difference film respectively. The light is reflected by the OLED panel, and the light is emitted after passing through the phase difference film and the linear polarizer respectively. Based on the simulation model, the spectrum of the incident light is defined as the D65 spectrum, and the brightness value of the scanned outgoing light divided by the brightness value of the incident light is defined as the reflectivity. The u' and v' values ​​in the CIELUV color space are calculated according to the spectrum of the outgoing light to evaluate the hue. The results are shown in Table 1:

[0143] Table 1

[0144]

[0145] It can be concluded from Table 1 that, compared with the comparative example, the embodiment of the present application has a significant improvement in reflectivity when viewed at a full viewing angle and in an oblique direction, improves the wide viewing angle integrated black characteristic, enhances the display effect, and increases visibility.

[0146] In the present application, Example 1 is compared with Examples 2 and 3, and Example 4 is compared with Examples 5 and 6. When viewed at a normal viewing angle and a wide viewing angle in the oblique direction, the reflected hue has obvious movement. Among the u' and v' values ​​calculated based on the CIELUV color space, the u' values ​​of Examples 2 and 5 are relatively large, and are in a reddish interval in the color space. The u' values ​​of Examples 3 and 6 are relatively small, and are in a bluish interval in the color space. The u' values ​​of Examples 1 and 4 are between the two, and are in a neutral interval in the color space. This is consistent with the situation that Examples 1 and 4 are optimized using a 550nm peak weight function, Examples 2 and 5 are optimized using a 520nm peak weight function (optimizing the blue light reflectance as much as possible, so that the final reflected hue is reddish), and Examples 3 and 6 are optimized using a 580nm peak weight function (optimizing the red light reflectance as much as possible, so that the final reflected hue is bluish). As can be seen from the above comparison, the optical design of the phase difference film optimized using different weight functions provided in the embodiments of the present application can adapt to the needs of different hues.

[0147] Those skilled in the art will readily appreciate other embodiments of the present application after considering the specification and practicing the invention disclosed herein. The present application is intended to cover any modification, use or adaptation of the present application, which follows the general principles of the present application and includes common knowledge or customary techniques in the art that are not disclosed in the present application. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present application are indicated by the claims.

[0148] It should be understood that the present application is not limited to the precise structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present application is limited only by the appended claims.

Claims

1. A phase difference film, characterized in that: The phase difference film is generated by polymerization of inversely dispersed rod-shaped liquid crystals, and the liquid crystal arrangement of the liquid crystal molecules in the phase difference film has a twisted orientation in the thickness direction and a gradually tilted orientation in the thickness direction; The changes in the tilt angle and azimuth angle of the liquid crystal molecules in the phase difference film are both nonlinear changes; the tilt angle is the angle between the director of the liquid crystal molecule and the film plane of the phase difference film, and the azimuth angle is the angle between the direction of the projection of the director of the liquid crystal molecule in the film plane and the selected reference direction; The range of the variation of the tilt angle of the liquid crystal molecules in the phase difference film per unit delay is 0.07° / nm~0.30° / nm, or 0.18° / nm~0.28° / nm; the range of the variation of the azimuth angle of the liquid crystal molecules in the phase difference film per unit delay is 0.06° / nm~0.30° / nm, or 0.10° / nm~0.27° / nm. or, The range of the change in the tilt angle of the liquid crystal molecules in the phase difference film per unit delay is 0.10° / nm~0.27° / nm, or 0.11° / nm~0.22° / nm; the range of the change in the azimuth angle of the liquid crystal molecules in the phase difference film per unit delay is 0.04° / nm~0.35° / nm, or 0.20° / nm~0.32° / nm.

2. The phase difference film according to claim 1, characterized in that: When the variation of the tilt angle of the liquid crystal molecules in the phase difference film per unit delay is in the range of 0.07° / nm to 0.30° / nm, or 0.18° / nm to 0.28° / nm; when the variation of the azimuth angle of the liquid crystal molecules in the phase difference film per unit delay is in the range of 0.06° / nm to 0.30° / nm, or 0.10° / nm to 0.27° / nm, the tilt angle of the liquid crystal molecules on the first side of the phase difference film is in the range of -20° to 20°, or -10° to 10°.

3. The phase difference film according to claim 2, characterized in that: The tilt angle of the liquid crystal molecules on the second side of the phase difference film ranges from 20° to 70°, or from 35° to 55°.

4. The phase difference film according to claim 2, characterized in that: The azimuth angle of the liquid crystal molecules on the second side of the phase difference film ranges from -10° to 40°, or from 10° to 30°.

5. The phase difference film according to claim 2, characterized in that: The twist angle of the liquid crystal molecules of the phase difference film ranges from 10° to 70°, or from 30° to 50°; the twist angle is the angle of rotation of the azimuth angle in the film plane.

6. The phase difference film according to claim 2, characterized in that: The delay amount of the phase difference film at a wavelength of 550nm ranges from 150nm to 260nm, or from 170nm to 235nm; the delay amount is the product of the difference between ne and no of the phase difference film at the corresponding wavelength and the thickness of the phase difference film; ne is the non-trivial refractive index of the liquid crystal molecules, and no is the ordinary refractive index of the liquid crystal molecules.

7. The phase difference film according to claim 1, characterized in that: When the variation of the tilt angle of the liquid crystal molecules in the phase difference film per unit delay is in the range of 0.10° / nm to 0.27° / nm, or 0.11° / nm to 0.22° / nm; when the variation of the azimuth angle of the liquid crystal molecules in the phase difference film per unit delay is in the range of 0.04° / nm to 0.35° / nm, or 0.20° / nm to 0.32° / nm, the tilt angle of the liquid crystal molecules on the second side of the phase difference film is in the range of -20° to 20°, or -10° to 10°.

8. The phase difference film according to claim 7, characterized in that: The tilt angle of the liquid crystal molecules on the first side of the phase difference film ranges from 20° to 50°, or from 30° to 45°.

9. The phase difference film according to claim 7, characterized in that: The azimuth angle of the liquid crystal molecules on the first side of the phase difference film ranges from -15° to 40°, or from -10° to 10°.

10. The phase difference film according to claim 7, characterized in that: The twisting angle of the liquid crystal molecules of the phase difference film ranges from 15° to 80°, or from 45° to 75°.

11. The phase difference film according to claim 7, characterized in that: The delay value of the phase difference film at a wavelength of 550nm ranges from 145nm to 340nm, or from 190nm to 300nm.

12. The phase difference film according to claim 1, characterized in that: The values ​​of the structural parameters in the phase difference film are determined when the reflectivity of the phase difference film is minimum; the structural parameters include the thickness, twist angle and tilt angle of the phase difference film.

13. A display device, characterized in that: The display device comprises a linear polarizer layer, a phase difference film layer corresponding to the phase difference film according to any one of claims 1 to 12, and a display panel layer, which are sequentially arranged; The first side of the phase difference film layer is a side close to the display panel layer; The second side of the phase difference film layer is a side close to the linear polarizer layer; The azimuth angle of the phase difference film is the angle between the direction of the director of the liquid crystal molecules projected in the film plane and the absorption axis of the linear polarizer layer.

14. The display device according to claim 13, characterized in that The phase difference film layer and the display panel layer are bonded together via an adhesive layer.

15. A method for preparing a phase difference film, characterized in that: The method is used to prepare the phase difference film according to any one of claims 1 to 12, characterized in that the method comprises: Pre-treating the coating surface of the substrate; Based on the twist angle and tilt angle of the phase difference film, coating an alignment layer on the pre-treated substrate; A liquid crystal layer having an alignment is coated on the alignment layer based on the thickness of the phase difference film.

16. The method according to claim 15, characterized in that The method further comprises: Taking the structural parameters of the phase difference film as optimization variables and the weighted average reflectivity as optimization indicators, the structural parameters of the phase difference film with the smallest weighted average reflectivity are determined as the optimized structural parameters of the phase difference film; the structural parameters include thickness, twist angle and tilt angle; The calculation of the weighted average reflectivity includes: Based on optical simulation, the reflectivity of the phase difference film under different wavelengths and different incident angles of non-polarized light is calculated; Based on a wavelength-related weight function, the reflectivity of the phase difference film for non-polarized light incident at different wavelengths and different incident angles is weighted averaged to obtain a weighted average reflectivity; the weight function is obtained by multiplying the luminosity function after the hue requirement is translated along the wavelength direction and the natural light spectrum; the weight functions under different hue requirements correspond to different peak wavelengths.

17. The method according to claim 16, characterized in that The method further comprises: When the hue requirement indicates a warm hue direction, the luminosity function is translated toward the blue light direction until the peak wavelength of the luminosity function is the target wavelength indicated by the hue requirement; In the case where the hue requirement indicates a cold hue direction, the luminosity function is translated toward the red light direction until the peak wavelength of the luminosity function is the target wavelength indicated by the hue requirement.

Citation Information

Patent Citations

  • Phase delay structure and display device

    CN116819671A

  • Phase delay structure and display device

    CN117008239A

  • Polarizing film and display device using the same

    CN117130088A

  • Phase difference film, polymerizable composition and preparation method of phase difference film

    CN117687141A

  • Composite phase difference optical element, its manufacturing method and liquid crystal display device

    JP2004109899A