A class of zinc carboxylate catalysts, their preparation method and their application in the alcoholysis of polyethylene terephthalate.
By designing a "Y"-shaped zinc carboxylate catalyst and synergistic catalysis with organic bases, the problem of insufficient activity of zinc salt catalysts in existing technologies has been solved, achieving efficient and environmentally friendly regeneration of the PET alcoholysis process, with high product purity and recyclable catalyst.
Patent Information
- Application Number
- CN202410667517.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-05-28
AI Technical Summary
In the existing technology, zinc salt catalysts have insufficient catalytic activity in the PET alcoholysis process. In particular, the research on the anionic part is limited to chloride ions, acetate ions and sulfate ions, which results in the zinc acetate catalyst failing to achieve a more efficient effect.
By designing a "Y"-shaped zinc carboxylate catalyst, the transition state stability of the catalyst is improved by utilizing the conjugation and hyperconjugation effects, and combined with organic base synergistic catalysis, efficient catalysis is achieved in the PET alcoholysis process.
With low catalyst dosage, zinc carboxylate catalysts efficiently catalyze the alcoholysis of PET over a wide temperature range, producing high-purity BHET products that can directly regenerate PET. The catalyst and solvent can be recycled, reducing resource waste and achieving a green and environmentally friendly recycling process.
Smart Images

Figure CN118543369B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer material degradation and recycling technology, and relates to the preparation of a class of zinc carboxylate catalysts and their application in PET alcoholysis. Background Technology
[0002] Polyethylene terephthalate (PET) is a long-chain polyester polymer synthesized by reacting ethylene glycol (EG) with terephthalic acid (PTA) or dimethyl terephthalate (DMT). It is widely used in food packaging, textiles, and films, with an annual production exceeding 60 million tons. However, due to PET's strong chemical and biological stability, large quantities of post-consumer waste PET are difficult to degrade naturally through air or microorganisms, becoming a major source of "white pollution." Therefore, exploring the recycling and reuse of waste PET is not only helpful in reducing resource waste but also of great significance in curbing environmental pollution.
[0003] Conventional PET recycling methods are mainly divided into physical and chemical methods. Physical methods involve melting and extruding PET waste to produce some plastic products. However, due to chain-breaking reactions caused by the presence of water and trace acidic contaminants, the molecular weight of physically recycled PET decreases, leading to a decline in performance. Chemical methods, on the other hand, degrade PET waste into monomers to regenerate virgin plastic products. Considering the quality of recycled products, chemical methods are more attractive and have been extensively studied.
[0004] The main chemical degradation methods for PET include hydrolysis (acidic / alkaline / neutral), alcoholysis, ammonia / amine hydrolysis, and high-temperature pyrolysis. Among these methods, ethylene glycol alcoholysis has advantages such as mild reaction conditions, low solvent volatility, and a wide range of product applications. Furthermore, the process for preparing recycled PET from its product, bis(2-hydroxyethyl) terephthalate (BHET), is simple and has great industrialization potential.
[0005] The ethylene glycol alcoholysis of PET is generally carried out under the catalysis of metal salts. Due to its advantages of low toxicity, low cost, and high activity, zinc salts have become the most widely used metal salts in PET alcoholysis. However, current research on metal salts mainly focuses on metal cations, while the anionic portion is limited to common acid anions such as chloride, acetate, and sulfate, resulting in the failure to find a more efficient metal salt catalyst than zinc acetate. Summary of the Invention
[0006] To address the aforementioned problems, this invention improves the catalytic activity of zinc carboxylate by adjusting the electronic and steric effects of the carboxylate ion, thereby achieving efficient catalytic hydrolysis of PET with low catalyst dosage.
[0007] To achieve the above objectives, the technical solution of the present invention is as follows: A class of zinc carboxylate catalysts exhibits higher catalytic activity by enhancing the stability of the transition state during the catalytic alcoholysis of PET through conjugation and hyperconjugation effects. The anion moiety of this zinc carboxylate catalyst has a "Y"-shaped structure, meaning that the carbon atom directly bonded to the carboxyl group, in addition to its own potential hydrogen atom, is simultaneously connected to two other atoms or groups via covalent bonds (including single and double bonds), with at least one of these bonds not being a hydrogen atom. This allows for improved stability of the transition state during PET activation by zinc carboxylate through σ-π hyperconjugation or π-π conjugation effects. These catalysts include both aliphatic and aromatic branches. The general structure of the anion moiety of the zinc carboxylate catalyst is as follows: Among them, R 1 The possible values are H, F, Cl, Br, I, CH3, CH2CH3, or CF3; R 2 H, F, Cl, Br, I, OH, CH2, CH3, CH2CH3, CH2CH2CH3, CF3, OCH3, OCH2CH3, vinyl or phenyl; R 3 The substituents are H, F, Cl, Br, I, OH, SH, CH3, CH2CH3, CH(CH3)2, C(CH3)3, OCH3, OCH2CH3, CH2F, CH2Cl, CH2Br, CH2I, CHF2, CHCl2, CF3, CCl3, CN, NO2, COCH3, COOH, NH2, NHCH3, N(CH3)2, ethynyl or phenyl, and the substituent positions include ortho, meta and para positions of the carboxyl group, with mono- or poly-substituted substituents.
[0008] The preparation process of a type of zinc carboxylate catalyst is as follows: carboxylic acid is dissolved and mixed with zinc oxide, and heated to ensure complete reaction. Most of the solvent is removed by concentration, and a poor solvent is added for recrystallization. The mixture is then filtered, washed, and the resulting solid is collected and dried under vacuum to obtain the corresponding zinc carboxylate catalyst. The synthesized zinc carboxylate is characterized by nuclear magnetic resonance spectroscopy and infrared spectroscopy.
[0009] In the above-mentioned preparation process of zinc carboxylate, the solvents used to dissolve the carboxylic acid include deionized water, methanol, ethanol, chloroform or tetrahydrofuran; the reaction temperature is 60 ~ 95℃; the reaction time is 8 ~ 24 h; and the unsuitable solvents used for recrystallization are diethyl ether, acetonitrile or acetone.
[0010] Application of the above-mentioned zinc carboxylate catalyst in the alcoholysis of polyethylene terephthalate: The zinc carboxylate catalyst with a "Y"-shaped structure can catalyze the alcoholysis of PET and ethylene glycol with high activity over a wide temperature range and a large variation range of PET / ethylene glycol feed ratio. The reaction rate can be increased by adding a reaction solvent, and the catalyst, residual ethylene glycol and reaction solvent can be recycled.
[0011] The temperature range for the PET ethylene glycol alcoholysis reaction is 150~200℃, and the reaction time is 10~600 min; the molar ratio of PET to ethylene glycol is 1:2~1:50 according to its repeating unit, and the molar ratio of catalyst to PET repeating unit is 0.0001:1~0.05:1.
[0012] The reaction solvent for the PET glycol alcoholysis reaction is dimethyl sulfoxide, γ-valerol, or... N -Methylpyrrolidone, the molar ratio of the reaction solvent to the PET repeating unit is 2:1 ~ 10:1.
[0013] The aforementioned zinc carboxylate catalyst can catalyze the alcoholysis of PET alone or in synergistic catalysis with an organic base. The preparation process of the zinc carboxylate catalyst / organic base complex is as follows: the organic base is 1,8-diazabicyclo[5.4.0]undec-7-ene; the organic base and zinc carboxylate are mixed at a certain molar ratio, and heated and stirred to form a homogeneous liquid mixture.
[0014] In the above-mentioned preparation process of zinc carboxylate catalyst / organic base complex, the molar ratio of organic base to zinc carboxylate catalyst is 2:1 to 8:1; the heating temperature is 30 to 120℃; and the heating time is 2 to 12 h.
[0015] The general process of catalytic PET alcoholysis according to this invention is as follows: (1) The waste PET plastic is initially cleaned, cut, deeply cleaned, and dried; (2) Mix the treated PET plastic, ethylene glycol (EG), catalyst and reaction solvent, and heat to carry out the PET alcoholysis reaction; (3) After the reaction is complete, cool to -5~5℃ to allow the product bis(2-hydroxyethyl) terephthalate (BHET) to crystallize out, and filter to separate the reaction solution from the crude product; (4) The crude product is pulped and then filtered again to separate BHET from the solvent; (5) Recrystallize the BHET obtained in step (4) to obtain high-purity BHET; (6) Fractionation step (4) The filtrate obtained by filtration is used to collect the low-boiling-point liquid and the high-boiling-point liquid respectively; (7) The low-boiling-point liquid obtained in step (6) can be reused in the pulping operation; (8) Mix the high-boiling-point liquid obtained in step (6) with the filtrate obtained in step (3) and add EG.
[0016] (9) Repeat steps (2) to (8).
[0017] In the above PET alcoholysis process, the cleaning solvents used in step (1) include deionized water and ethanol, and the size of the cut PET bottle flakes is 0.1-1 cm. 2 .
[0018] In the above PET alcoholysis process, the solvents used in step (4) pulping include petroleum ether, diethyl ether, petroleum ether / ethyl acetate mixed solution, petroleum ether / dichloromethane mixed solution, petroleum ether / dimethyl carbonate mixed solution, etc.
[0019] In the above PET alcoholysis process, the solvents used for recrystallization in step (5) include deionized water, tetrahydrofuran, ethyl acetate, ethanol, etc.
[0020] The significant advantages of this invention are: compared to traditional zinc acetate catalysts, it exhibits higher catalytic activity, effectively catalyzing the alcoholysis reaction of PET even at lower concentrations; the catalyst maintains high efficiency across a wide temperature range; the electronic and steric effects of the carboxylate anion can be easily adjusted by changing the substituents; it produces a good synergistic effect with organic bases, resulting in a "1 + 1 > 2" catalytic effect; the resulting BHET product has high purity and whiteness, and can be directly used for repolymerization to generate PET, achieving efficient recycling of waste polyester plastics; the catalyst, reaction solvent, and residual ethylene glycol can be recycled, reducing resource waste and making the polyester chemical recycling process more environmentally friendly. By adding an additional solvent, PET can be dissolved in the reaction system, transforming the PET alcoholysis reaction from a heterogeneous reaction to a homogeneous reaction, thus increasing the PET alcoholysis rate. Attached Figure Description
[0021] Figure 1 For product BHET 1 H NMR spectrum.
[0022] Figure 2 The infrared spectrum of product BHET.
[0023] Figure 3 Zinc 2-methylpropionate 1 H NMR spectrum.
[0024] Figure 4 The image shows the infrared spectrum of zinc 2-methylpropionate.
[0025] Figure 5Zinc o-bromobenzoate 1 HNMR spectrum.
[0026] Figure 6 The infrared spectrum is that of zinc o-bromobenzoate.
[0027] Figure 7 This is a BHET yield graph from Example 6.
[0028] Figure 8 This is a BHET yield graph from Example 7.
[0029] Figure 9 This is a BHET yield graph from Example 9. Detailed Implementation
[0030] Example 1: This example illustrates the general preparation process of aliphatic zinc carboxylate.
[0031] The preparation process of zinc 2-methylpropionate is shown in the following formula. The specific steps are as follows: First, 2-methylpropionic acid (30.0 g, 0.34 mol) is dissolved in 500 mL of chloroform, and then zinc oxide (13.9 g, 0.17 mol) is added. The reaction is carried out at 60℃ for 24 hours. The chloroform is evaporated under vacuum until about 50 mL remains. The remaining solution is added dropwise to 500 mL of acetonitrile and stirred for 3 hours. The mixture is filtered, and the filter cake is washed three times with acetonitrile. The filter cake is then dried under vacuum to obtain the product zinc 2-methylbutyrate.
[0032] Example 2: This example illustrates the general preparation process of zinc aromatic carboxylate.
[0033] The preparation process of zinc o-bromobenzoate is shown in the following formula. The specific steps are as follows: First, zinc o-bromobenzoate (50.0 g, 0.25 mol) is dissolved in 500 mL of methanol, then zinc oxide (10.1 g, 0.125 mol) is added, and the reaction is carried out at 65℃ for 12 hours. The methanol is evaporated under vacuum until about 50 mL remains. The remaining solution is added dropwise to 500 mL of diethyl ether, stirred for 3 hours, filtered, and the filter cake is washed three times with diethyl ether. The filter cake is then dried under vacuum to obtain the product zinc o-bromobenzoate.
[0034] Example 3: This example illustrates the improved catalytic activity of "Y"-shaped zinc carboxylate for PET alcoholysis compared to other configurations.
[0035] 0.50 g of PET waste beverage bottle fragments, 0.65 g of ethylene glycol, and 2.09 g of γ-valerate were added to a round-bottom flask. Then, zinc aliphatic carboxylate with different configuration substituents, equivalent to 0.01% of the molar amount of the PET repeating unit, was added. The reaction was carried out at 190 °C for 4 h to obtain the alcoholysis product. The PET conversion rate and BHET yield were determined by 1H NMR spectroscopy. The results are shown in Table 1. The catalytic activity was highest when the substituent was CH(CH3)2, indicating that the "Y"-shaped structure can effectively catalyze the alcoholysis reaction of PET.
[0036] Table 1. Catalytic performance of zinc aliphatic carboxylate catalysts with different substituents for PET alcoholysis
[0037] Example 4: This embodiment modulates the activity of aliphatic "Y"-shaped zinc carboxylate in catalyzing the alcoholysis of PET by altering the steric effect of substituents.
[0038] 0.50 g of PET waste beverage bottle fragments, 0.65 g of ethylene glycol, and 2.09 g of γ-valerol were added to a round-bottom flask. Then, aliphatic "Y"-shaped zinc carboxylate with similar electronic effects but different steric effects, equivalent to 0.01% of the molar amount of the PET repeating unit, was added. The mixture was reacted at 190 °C for 4 h to obtain the alcoholysis product. The PET conversion rate and BHET yield were determined by 1H NMR spectroscopy. The results are shown in Table 2. The catalytic activity was highest when the substituent was CH3.
[0039] Table 2. Effects of changing the steric effect of substituents on the catalytic activity of aliphatic "Y"-shaped zinc carboxylate in the alcoholysis of PET.
[0040] Example 5: This embodiment is used to illustrate R 2 The catalytic effect of "Y"-shaped zinc carboxylate when CH2 is present.
[0041] 0.50g of PET waste beverage bottle fragments, 0.65g of ethylene glycol and 2.09g of γ-valerol were added to a round-bottom flask, and then zinc acrylate and zinc 2-methacrylate, respectively, were added at 0.05% of the molar amount of PET repeating unit. The mixture was reacted at 190℃ for 2h to obtain alcoholysis products with BHET yields of 81% and 82%, respectively.
[0042] Example 6: This example illustrates the effect of the electronic effects of para-substituents on the catalytic activity of zinc aromatic carboxylate.
[0043] 0.50 g of PET waste beverage bottle fragments, 0.65 g of ethylene glycol, and 2.09 g of γ-valerol were added to a round-bottom flask. Then, zinc benzoate with different electronegative substituents at the para position (OCH3, CH3, H, Br, CN, NO2, respectively) was added, equivalent to 0.01% of the molar amount of the PET repeating unit. The reaction was carried out at 190 °C for 4 h to obtain the alcoholysis product. The yield of BHET was determined by 1H NMR spectroscopy. Figure 7 As shown, the catalytic activity is highest when the substituent is a Br atom.
[0044] Example 7: This example illustrates the effect of the electronic effects of meta-substituents on the catalytic activity of zinc aromatic carboxylate.
[0045] 0.50 g of PET waste beverage bottle fragments, 0.65 g of ethylene glycol, and 2.09 g of γ-valerol were added to a round-bottom flask. Then, zinc benzoate with different electronegative substituents at the meta position (CH3, H, OCH3, Br, CN, NO2, respectively) was added, equivalent to 0.01% of the molar amount of the PET repeating unit. The reaction was carried out at 190 °C for 4 h to obtain the alcoholysis product. The yield of BHET was determined by 1H NMR spectroscopy. Figure 8 As shown, the catalytic activity is highest when the substituent is OCH3.
[0046] Example 8: This example illustrates the effect of the electronic effects of ortho-substituents on the catalytic activity of zinc benzoate.
[0047] 0.50 g of PET waste beverage bottle fragments, 0.65 g of ethylene glycol, and 2.09 g of γ-valerol were added to a round-bottom flask. Then, catalysts with different electronegativity substituents at the ortho position, equivalent to 0.01% of the molar amount of the PET repeating unit, were added. The reaction was carried out at 190 °C for 4 h to obtain the alcoholysis product. The PET conversion rate and BHET yield were determined by 1H NMR spectroscopy. The results are shown in Table 3. The catalytic activity was highest when the substituent was a Cl atom.
[0048] Table 3. Effects of electronic effects of ortho-substituents on the catalytic activity of zinc benzoate.
[0049] Example 9: This example illustrates the effect of the steric effect of ortho-substituents on the catalytic activity of zinc benzoate.
[0050] 0.50 g of PET waste beverage bottle fragments, 0.65 g of ethylene glycol, and 2.09 g of γ-valerol were added to a round-bottom flask. Then, zinc benzoate with similar electronic effects and significantly different steric hindrances (F, Cl, Br, I) was added, equivalent to 0.01% of the molar amount of the PET repeating unit. The reaction was carried out at 190 °C for 4 h to obtain the alcoholysis product. The yield of BHET was determined by 1H NMR spectroscopy. The results are as follows. Figure 9 The best catalytic effect is obtained when the substituent is Br.
[0051] Example 10: This example illustrates the effect of zinc carboxylate and organic base synergistically catalyzing the alcoholysis of PET.
[0052] 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) and zinc o-bromobenzoate (Zn( o -BrBA)2) Mixed at a molar ratio of 4:1 and heated at 60℃ for 8 hours to obtain DBU / Zn( o -BrBA)2= 4 / 1 complex.
[0053] Add 0.50g of PET waste beverage bottle fragments, 0.65g of ethylene glycol, and 2.09g of γ-valerol to a round-bottom flask, then add DBU / Zn (equivalent to 0.5% of the molar amount of the PET repeating unit). o The BrBA)2= 4 / 1 complex catalyst was reacted at 190℃ for 10 minutes to obtain the alcoholysis product. The PET conversion rate reached 100%, and the BHET yield was 87%.
[0054] Example 11: This example illustrates the catalytic activity of zinc carboxylate and its complex with an organic base at lower temperatures. 0.50 g of PET waste beverage bottle fragments, 0.65 g of ethylene glycol, and 2.09 g of γ-valerol were added to a round-bottom flask, followed by the addition of Zn (0.5% of the molar amount of the PET repeating unit). o -BrBA)2、DBU / Zn( o Two catalysts, -BrBA)2= 4 / 1, were used to react at 170℃ for 1 h to obtain alcoholysis products with BHET yields of 33% and 84%, respectively.
[0055] Example 12: This example illustrates the catalytic activity of zinc carboxylate at a relatively high PET dosage. 20.0 g of PET waste beverage bottle fragments, 77.6 g of ethylene glycol, and 83.4 g of γ-valerol were added to a round-bottom flask, followed by the addition of Zn (0.5% of the molar amount of the PET repeating unit). o-BrBA)2 was reacted at 195℃ for 1 h to obtain the alcoholysis product. The PET conversion rate was 100% and the BHET yield was 96%.
[0056] Example 13: This example illustrates the effect of different amounts of ethylene glycol on the catalytic effect of PET alcoholysis. 5.0g of PET waste beverage bottle fragments, 20.9g of γ-valerol, and 0.5% Zn (equivalent to the molar amount of a PET repeating unit) were used. o -BrBA)2 was added to a round-bottom flask, and ethylene glycol equivalent to 2, 4, 6, 8, 10, 12, 15, 20, and 50 times the molar amount of PET repeating unit was added respectively. The reaction was carried out at 195℃ for 2 h to obtain alcoholysis products. The PET conversion rate reached 100% in all cases, and the BHET yields were 72%, 87%, 90%, 93%, 95%, 96%, 97%, 98%, and >99%, respectively.
[0057] Example 14: This embodiment illustrates the decolorization effect of the PET alcoholysis process of the present invention on PET of different colors. 20.0g of PET waste beverage bottle fragments, 77.6g of ethylene glycol, and 83.4g of γ-valerol were added to a round-bottom flask, followed by the addition of DBU / Zn (equivalent to 0.1% of the molar amount of the PET repeating unit). o -BrBA)2= 4 / 1, reacted at 195℃ for 2h to obtain alcoholysis products. The yield and color of BHET were determined and the results are shown in Table 4. Different PET bottle flakes all had high BHET yield and good color.
[0058] Table 4. Decolorization effect of PET alcoholysis process on PET of different colors
[0059] Example 15: This example illustrates the cyclical effect of the reaction process. 20.0g of PET waste beverage bottle fragments, 77.6g of ethylene glycol, and 83.4g of... γ - Add valerol to a round-bottom flask, then add DBU / Zn (equivalent to 0.1% of the molar amount of the PET repeating unit). o -BrBA)2= 4 / 1, reacted at 195℃ for 2h to obtain the alcoholysis product. Cooled to -5℃ to allow BHET to crystallize out, filtered, and the filtrate and filter cake were collected separately. EG was added to the filtrate to a total volume of 38.8 g, and then 20.0 g of PET flakes were added for a second reaction. This process was repeated multiple times. The conversion rate of PET, the yield of BHET, and the color were measured in each cycle. The results are shown in Table 5. In all three cycles, the PET conversion rate reached 100%, the BHET yield was greater than 90%, and the products all exhibited excellent color.
[0060] Table 5. Cycle effect of the reaction process
Claims
1. The application of zinc carboxylate catalyst in the alcoholysis of polyethylene terephthalate, characterized in that, The zinc carboxylate catalyst has a Y-shaped anion moiety. The zinc carboxylate catalyst includes both aliphatic and aromatic branches. In the aliphatic branch, the carbon atom directly bonded to the carboxyl group, in addition to its own hydrogen atom, is covalently bonded to two other atoms or groups. At least one of these other two atoms or groups is not a hydrogen atom. The structure of the anion moiety of the zinc carboxylate catalyst is as follows: wherein R 1 is H, F, Cl, Br, I, CH3, CH2CH3, or CF3; R 2 H, F, Cl, Br, I, OH, CH2, CH3, CH2CH3, CH2CH2CH3, CF3, OCH3, OCH2CH3, vinyl or phenyl; R 3 The substituents are H, F, Cl, Br, I, OH, SH, CH3, CH2CH3, CH(CH3)2, C(CH3)3, OCH3, OCH2CH3, CH2F, CH2Cl, CH2Br, CH2I, CHF2, CHCl2, CF3, CCl3, CN, NO2, COCH3, COOH, NH2, NHCH3, N(CH3)2, ethynyl or phenyl, and the substituent positions include ortho, meta and para positions of the carboxyl group, with mono- or poly-substituted substituents; Using a Y-shaped zinc carboxylate catalyst, the reaction rate was increased by adding a reaction solvent within a temperature range of 150~200℃ and a reaction time of 10~600 min. PET was calculated according to its repeating unit, with a PET to ethylene glycol molar ratio of 1:2~1:50 and a catalyst to PET repeating unit molar ratio of 0.0001:1~0.05:
1. This resulted in high-activity catalysis of the PET-ethylene glycol alcoholysis reaction, achieving the recycling of the catalyst, residual ethylene glycol, and reaction solvent.
2. The application according to claim 1, characterized in that, The reaction solvent for the PET glycol alcoholysis reaction is dimethyl sulfoxide, γ-valerol, or... N -Methylpyrrolidone, the molar ratio of the reaction solvent to the PET repeating unit is 2:1 ~ 10:
1.
3. The application according to claim 1, characterized in that, The zinc carboxylate catalyst described above can catalyze the alcoholysis of PET alone, or it can catalyze the alcoholysis of PET in synergistic catalysis with organic bases.
4. According to claim 3, the preparation process of the zinc carboxylate catalyst / organic base complex is as follows: the organic base and the zinc carboxylate catalyst are mixed at a certain molar ratio, and heated and stirred to form a uniform liquid mixture; the organic base is 1,8-diazabicyclo[5.4.0]undec-7-ene; the molar ratio of the organic base to the zinc carboxylate catalyst is 2:1 to 8:1; the heating temperature is 30 to 120°C; and the heating time is 2 to 12 h.
5. The application according to claim 1, wherein the process is as follows: (1) The waste PET plastic is initially cleaned, cut, deeply cleaned, and dried; (2) Mix the treated waste PET plastic, ethylene glycol, catalyst and reaction solvent, and heat to carry out PET alcoholysis reaction; (3) After the reaction is complete, cool to -5~5℃ to allow the product bis(2-hydroxyethyl) terephthalate BHET to crystallize out, and filter to separate the reaction solution from the crude product; (4) The crude product is pulped and then filtered again to separate BHET from the solvent; (5) Recrystallize the BHET obtained in step (4) to obtain high-purity BHET; (6) Fractionation step (4) The filtrate obtained by filtration is used to collect the low-boiling-point liquid and the high-boiling-point liquid respectively; (7) The low-boiling-point liquid obtained in step (6) can be reused in the pulping operation; (8) Mix the high-boiling-point liquid obtained in step (6) with the filtrate obtained in step (3) and add ethylene glycol; (9) Repeat steps (2) to (8).
6. The application according to claim 5, characterized in that, The solvents used for cleaning the waste PET plastics include deionized water and ethanol.
7. The application according to claim 6, characterized in that, The solvents used in pulping are petroleum ether, diethyl ether, a mixture of petroleum ether and ethyl acetate, a mixture of petroleum ether and dichloromethane, and a mixture of petroleum ether and dimethyl carbonate.
8. The application according to claim 6, characterized in that, The solvent used for recrystallization is deionized water, tetrahydrofuran, ethyl acetate, or ethanol.
Citation Information
Patent Citations
Method for recovering waste polyester based on alcoholysis of bi-component catalyst
CN114890898A
Arylalkanoic acid process improvement
US4623736A