A high-strength welding method for arc-shaped surface accessories
By processing arc-shaped grooves at the outer welding flange block of the steel pipe and multi-pass layered welding technology, the problem of insufficient weld strength in the existing welding methods is solved, high strength and stable welding effects are achieved, and the steel pipe is ensured The structure's hydrostatic test passed.
Patent Information
- Application Number
- CN202410987480.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing welding method of the external welding flange block of the steel pipe results in poor weld strength, making it difficult for the steel pipe structure to pass the hydrostatic test.
The high-strength welding method of arc surface accessories includes processing arc-shaped grooves on the accessories to be welded, grinding, rust removal, decontamination and preheating, and using H08CrMoA heat-resistant steel wire with a diameter of 2mm for groove welding filling. , using argon as the protective gas, multi-pass welding in layers, and heat preservation and slow cooling treatment to improve the welding strength.
Through creative arc groove welding and multi-pass layered welding technology, the strength and stability of the weld are improved, the possibility of cracks and bubbles is reduced, and the length of the contact line between the accessory and the pipe fitting is ensured after welding , which meets the high-strength welding requirements.
Smart Images

Figure CN118543936B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of welding technology, and in particular to a high-strength welding method for arc-shaped surface accessories. Background Art
[0002] Pipelines are special equipment used to transport hazardous media and are widely used in industries such as petroleum, chemical, electric power, and construction. With the development of my country's national economy, the demand for pipelines continues to increase, and the requirements for construction quality are also getting higher and higher. Among them, high-strength pipeline welding is an extremely important part of pipeline production and installation.
[0003] If the curved outer wall of the pipe fitting needs to be welded with block materials, such as flanges, refer to Figure 1 As shown, in order to facilitate the installation of sensors and other equipment, the root position of the flange block, including the root position of the upper hole of the flange block and the steel pipe, needs to be welded during the production process of the pipe fittings. After welding, the two square holes in the middle of the flange block also need to be milled through. During the fine milling process, the weld may be milled, resulting in reduced welding strength.
[0004] Usually, flange blocks are welded with ordinary fillet welds, and the grooves are chamfered. After fine milling, this welding method is tested and small pores and cracks will appear at the weld position. The weld strength is poor, making it difficult for the steel pipe structure to pass the water pressure test. Summary of the invention
[0005] The technical problem to be solved by the present invention is that the weld strength formed by the existing welding method of the steel pipe external welding flange block is poor.
[0006] To this end, the present invention provides a high-strength welding method for arc-shaped surface accessories.
[0007] The technical solution adopted by the present invention to solve its technical problem is:
[0008] A high-strength welding method for arc-shaped surface accessories comprises the following steps:
[0009] Processing a circular arc groove on the accessory to be welded, when the outer diameter of the pipe fitting is less than 300mm, the arc surface radius of the circular arc groove is 4-5mm;
[0010] Grind and remove rust and dirt from the parts to be welded;
[0011] Preheat the welding area;
[0012] The accessories are welded to the pipe fittings, and the welds are polished. When welding the accessories to the pipe fittings, H08CrMoA heat-resistant steel welding wire with a diameter of 2mm is used for groove welding filling. The welding joints are staggered. Argon is used as the protective gas during welding. The ventilation speed is 5-6L / min, and the temperature of the welding position is continuously measured with a temperature measuring gun so that the interlayer temperature is maintained at 280°C; wherein, the welding filling includes multiple welds, and the multiple welds form the bottom layer, the middle layer and the top layer of the weld. The bottom layer, the middle layer and the top layer are welded with different current intensities. The current intensity when welding the bottom layer is less than the current intensity when welding the middle layer, and the current intensity when welding the middle layer is less than the current intensity when welding the top layer. The weld at the bottom layer is closest to the bottom of the groove and is welded with a small current of 60±20A. The weld at the middle layer has a welding current of 80±20A, and the weld at the top layer has a welding current of 100±20A.
[0013] The welding parts are kept warm and slowly cooled, and finally heat treated and tempered;
[0014] When keeping warm and cooling slowly, perform multiple cooling and then heating. First, slowly cool the part to be welded to A1℃, then heat it to B1℃, then slowly cool it to A2℃, then heat it to B2℃, then slowly cool it to A n ℃, and then heat the welded area to B n ℃, repeatedly until the welding part cools down to room temperature naturally, among which A n <……<A2<A1,B n <……<B2<B1,B n+1 =A n ;
[0015] During the insulation and slow cooling, the temperature of the welding position is measured. When the temperature of the welding position is measured to have dropped to 180°C, the welding position is heated to 250°C, and then the heating is stopped and the temperature measurement is continued. When the temperature of the welding position is measured to have dropped to 120°C, the welding position is heated to 180°C again, and then the heating is stopped and the temperature measurement is continued. When the temperature of the welding position is measured to have dropped to 60°C, the welding position is heated to 120°C again, and then the heating is stopped until the welding position is naturally cooled to room temperature.
[0016] Furthermore, before preheating and welding, the accessory is connected to the pipe (1) by spot welding to perform pre-positioning.
[0017] Furthermore, the filling material for spot welding is H08CrMoA heat-resistant steel welding wire with a diameter of 1.2mm. During spot welding, argon is used as the shielding gas, the ventilation speed is 5-6L / min, the current polarity is direct current electrode positive connection, the welding current is 120±30A, the welding voltage is 20±3V, and the welding speed is 16cm / min.
[0018] Furthermore, during preheating, the portion to be welded is heated to 200-250°C.
[0019] The beneficial effect of the present invention is that the present invention creatively adopts arc-shaped grooves for welding, so that after welding and filling, a longer contact line is formed between the accessories and the pipe fittings, and the weld strength can be maintained even after fine milling.
[0020] During the welding process, the spot welding is first used for positioning, and then the preheating welding is performed to improve the welding accuracy; when welding the seams, different current intensities are used for multi-pass layered welding to reduce the possibility of bubbles and cracks in the weld at the bottom of the groove. The appropriate welding speed is used to heat the weld position evenly during the welding process, which can also reduce the occurrence of cracks. After welding the seams, repeated insulation and slow cooling are used to improve the welding strength at the bottom of the groove, slow down the cooling rate of the weld and the heat-affected zone, and reduce the possibility of cracks in the weld position. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0022] Figure 1 It is a schematic diagram of the pipe structure in the background technology of the present invention.
[0023] Figure 2 It is a structural schematic diagram of the flange block in the present invention.
[0024] Figure 3 It is a schematic diagram of the welding relationship between the flange block and the pipe fitting in the present invention.
[0025] Figure 4 It is a schematic diagram of the groove structure in the present invention.
[0026] Figure 5 This is a photo of the weld after fine milling using the A-type groove for welding in the present invention.
[0027] Figure 6 This is a photograph of the weld after fine milling using the arc-shaped groove for welding in the present invention.
[0028] Figure 7 It is a schematic diagram of the weld bead of the sample for flaw detection test in the present invention.
[0029] Figure 8Schematic diagram of a weld in an embodiment of the present invention.
[0030] Reference numerals
[0031] 1. Pipe fittings; 2. Flange blocks; 3. Bottom layer; 4. Top layer; 5. Arc-shaped groove. DETAILED DESCRIPTION
[0032] The present invention will now be described in further detail with reference to the accompanying drawings. These drawings are simplified schematic diagrams, which only illustrate the basic structure of the present invention in a schematic manner, and therefore only show the components related to the present invention.
[0033] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0034] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0035] A high-strength welding method for arc-shaped surface accessories comprises the following steps:
[0036] Step 1: Processing a welding groove on the accessory to be welded (the flange block 2 in this embodiment).
[0037] like Figure 2 , 3As shown, a welding arc groove 5 is processed at the root position of the flange block 2, and the arc groove 5 protrudes toward the pipe fitting 1. The outer circle of the pipe fitting 1 usually used to make the target missile rocket launcher shell is greater than 200mm. When the outer circle diameter of the pipe fitting 1 is less than 200mm~300mm, the arc surface radius of the arc groove 5 is 4-5mm; when the outer circle diameter of the pipe fitting 1 is 300mm~500mm, the arc surface radius of the arc groove 5 is 6-8mm.
[0038] In this embodiment, the pipe fitting 1 used is a 30CrMnSiA steel pipe, the outer diameter of the pipe fitting 1 is 203mm, the inner diameter is 174mm, the flange block 2 is made of 30CrMnSiA steel plate, and the welding groove between the bottom of the upper hole of the flange block 2 and the arc fitting surface of the outer wall of the pipe fitting 1 is processed into an R5 arc groove 5, that is, the arc radius of the arc surface of the groove is 5mm, and the two inner square holes are surrounded by a single side of 1mm margin (in the fine milling process, the fine milling only mills off a single side at most 1mm), such as Figure 4 As shown, the cross-sectional area of the weld produced between the flange block 2 and the cylinder barrel is increased compared with the a-type groove (V-type groove), which improves the strength of the weld. Compared with the b-type groove (V-type groove with a larger angle) and the c-type groove (an arc groove bent in the direction away from the pipe fitting 1), the arc groove 5 in the present application has a deep penetration and can minimize the use of welding fillers, facilitate penetration, and achieve relatively economical and effective welding. Compared with the c-type groove (an arc groove bent in the direction away from the pipe fitting 1), when welding is implemented, the arc groove 5 has fewer welding dead angles, and is not prone to leaking welds or poor welding quality due to incomplete penetration.
[0039] Figure 5 This is a photo of the weld between the flange block 2 and the pipe fitting 1 after fine milling using the above-mentioned a-type groove. Figure 6 This is a photo of the weld between the flange block 2 and the pipe fitting 1 after fine milling using the arc-shaped groove 5 in this embodiment. Figure 5 As shown in the figure, after fine milling, there is a gap in the weld position, the A-type groove opening is small, and the internal welding is difficult during welding. Therefore, there may be incomplete penetration and leakage during welding. Figure 6 The arc groove 5 is adopted in the welding position, and the opening area thereof is larger, the field of vision is good during welding, the welding gun is easy to insert, and the weld is complete after fine milling, indicating that the welding is completely penetrated, the welding quality is better, and the weld strength is higher.
[0040] Step 2, pre-welding treatment, grinding and removing rust and dirt from the parts to be welded, specifically including the groove position and the position to be welded on the pipe 1.
[0041] Step three, splice the flange block 2 to the position to be welded on the pipe fitting 1, and spot weld the arc groove 5 to fix it. The filling material for spot welding is H08CrMoA heat-resistant steel welding wire with a diameter of 1.2mm. During spot welding, argon with a purity of 99.99% is used as the protective gas, the ventilation speed is 5-6L / min, the current polarity is direct current electrode positive connection, the welding current is 120±30A, the welding voltage is 20±3V, and the welding speed is 16cm / min.
[0042] Step 4: preheating. Use a drying gun to heat the parts to be welded (the arc groove 5 position and the pipe 1 to be welded) to 200-250°C.
[0043] Step 5: Welding. Welding must comply with the welding standards specified in QJ1842A-2014, and the weld grade must be II.
[0044] H08CrMoA heat-resistant steel welding wire with a diameter of 2mm is used for groove welding filling. The welding joints cannot be in the same position. WPS argon arc welding machine is used for welding. Argon with a purity of 99.99% is used as the protective gas. The ventilation speed is 5-6L / min, and a temperature gun is used to continuously measure the temperature of the welding position to keep the interlayer temperature at 280℃. The weld position needs a smooth transition. The oxide scale needs to be cleaned at all times during the welding process to ensure normal welding.
[0045] Since the welding strength test of the weld position is a destructive test, before welding the flange block 2 and the pipe fitting 1, the flange block 2 and the pipe fitting 1 are welded in the same way using the sample. The specific welding sequence is as follows: Figure 5 shown.
[0046] Specifically, the welding seam filling includes 17 welds, all of which are filled with 2mm heat-resistant steel wire, the current polarity is direct current electrode positive connection, the arc voltage is 18±2V, and the welding speed is 16cm / min. Figure 3 The position of the 1st to 3rd welds closest to the bottom of the groove is the bottom layer 3 of the weld, and a small current is used for welding, and the welding current is 60±20A. The 4th to 8th welds are the middle layer of the weld, and the welding current is 80±20A. The 9th to 17th welds are the top layer 4 of the weld, and the welding current is 100±20A. After adopting the arc groove 5, compared with the original V-shaped groove, the cross-sectional area of the position to be filled is increased, thereby increasing the number of welds, and the number of welds in each layer of the middle layer and the top layer 4 is increased, so that the welding strength is enhanced.
[0047] According to Figure 7The flaw detection of the welding results of the sample shown adopts a welding method of multi-pass layered welding with different current intensities. A lower current intensity is used for welding at the bottom layer 3 of the weld to reduce the possibility of bubbles and cracks in the weld at the bottom of the groove. A suitable welding speed is used to ensure uniform heating of the weld position during the welding process, which can also reduce the occurrence of cracks.
[0048] In this embodiment, the actual welding sequence between the flange block 2 and the pipe fitting 1 is as follows: Figure 8 As shown, since the welding space between the actual flange block 2 and the pipe fitting 1 is small, the actual welding is performed in two layers, the weld of the bottom layer 3 is welded with a small current of 80±20A, and the welding current of the top layer 4 is 100±20A. In this application, since the top layer 4 will be milled during the later fine milling, a slightly larger welding current is used for welding, thereby increasing the welding speed.
[0049] Step 6: Post-welding treatment
[0050] S6.1 After welding is completed, the weld position needs to be rounded and polished to remove burrs.
[0051] S6.2 After welding is completed, keep warm and cool slowly. After cooling down for several times, heat up again. First, slowly cool down the part to be welded to A1℃, then heat the part to be welded to B1℃, then slowly cool down the part to be welded to A2℃, then heat the part to be welded to B2℃, and then slowly cool down the part to be welded to A n ℃, and then heat the welded area to B n ℃, repeatedly until the welding part cools down to room temperature naturally, among which A n <……<A2<A1,B n <……<B2<B1,B n+1 -B n =M, 50<M<200, B n+1 =A n .
[0052] In this embodiment, M is 60°C, and the slow cooling and insulation are carried out by cooling down three times and then heating. The specific operations are as follows: use a temperature measuring gun to measure the temperature of the welding position. When it is measured that the temperature of the welding position naturally drops to 180°C, immediately use a drying gun to heat the welding position to 250°C, then stop heating, and continue to measure the temperature; when it is measured that the temperature of the welding position naturally drops to 120°C, immediately use a drying gun to heat the welding position to 180°C again, then stop heating, and continue to measure the temperature; when it is measured that the temperature of the welding position naturally drops to 60°C, use a drying gun to heat the welding position to 120°C again, then stop heating, until the welding position naturally cools to room temperature.
[0053] After welding, the weldment is kept warm and slowly cooled, which can slow down the cooling rate of the weld and the heat-affected zone, and play a similar role to preheating. In this application, after three stages of warming and slow cooling, the temperature of the welded part is gradually reduced, which can better slow down the cooling rate of the weld and the heat-affected zone, facilitate the release of residual stress, reduce the stress level at the weld position, and make the fusion between welds and between welds and parent materials better, improve the penetration effect of welding, and thus reduce the possibility of cracks at the weld position. Compared with wrapping the welding position with insulation material to cool it down slowly, the natural cooling after repeated heating can quickly cool the welding part to room temperature, reduce the generation of cracks and ensure the quality of the weld.
[0054] Step 7: Preliminary testing
[0055] S7.1 First, visually inspect the welded area to check for defects at the weld location, and make repairs according to the defect repair and repair welding specified in Chapter 6 of QJ1842A.
[0056] S7.2 Measure the welding position to confirm whether the size of the welding part is consistent with the predetermined size.
[0057] Step eight, annealing. After the weld is trimmed and tested in step seven, defects need to be repaired again. Annealing should be performed within 8 hours after repair welding.
[0058] Step nine, perform X-ray inspection on the weld. The weld formed by the above steps meets the Level II requirements of QJ1842A-2011 standard.
[0059] Step ten, heat treatment.
[0060] It should be noted that if no correction or repair welding is required after the preliminary inspection in step seven, step eight is skipped and step nine and this step are performed.
[0061] Heat treatment and tempering are carried out within 8 hours after welding and processing (further processing steps such as fine milling are carried out).
[0062] After the above welding, the mechanical properties of the weld after testing and heat treatment are as follows: Basic metal tensile strength ≥1080MPa; tensile strength of welded joint ≥971MPa; elongation at break ≥10%; welding bending angle ; Depth of double-sided decarburized layer ≤0.15mm.
[0063] The welding strength (i.e., the performance parameters of the quenched and tempered test piece) can meet the requirements, and its tensile strength also meets the test requirements. In the bending test, when the weld position is cold bent at 25°C, no opening defects are found in any direction on the tensile surface at the weld position, that is, the weld strength between the arc surface and the attachment after welding using the method of the present invention is better.
[0064] In summary, the present invention changes the ordinary V-shaped groove and U-shaped groove at the welding groove part, and creatively adopts the arc-shaped groove 5 for welding, so that after welding and filling, a longer contact line is formed between the accessory and the pipe 1. Even after fine milling, it can maintain better welding strength and meet the welding strength required by the target rocket launcher when in use.
[0065] During the welding process, the spot welding is first used for positioning, and then the preheating welding is performed to improve the welding accuracy; when welding the seams, different current intensities are used for multi-pass layered welding to reduce the possibility of bubbles and cracks in the weld at the bottom of the groove. The appropriate welding speed is used to heat the weld position evenly during the welding process, which can also reduce the occurrence of cracks. After welding the seams, repeated insulation and slow cooling are used to improve the welding strength at the bottom of the groove, slow down the cooling rate of the weld and the heat-affected zone, and reduce the possibility of cracks in the weld position.
[0066] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.
Claims
1. A high-strength welding method for arc-shaped surface accessories, characterized in that: The following steps are included: A circular arc groove (5) is processed on the accessory to be welded, the arc surface of the accessory to be welded is in contact with the arc of the outer wall of the pipe (1), the circular arc groove (5) is arranged at the root of the accessory to be welded close to the pipe (1), the circular arc groove (5) protrudes toward the pipe (1), and when the outer diameter of the pipe (1) is less than 300 mm, the radius of the arc surface of the circular arc groove (5) is 4-5 mm; Grind and remove rust and dirt from the parts to be welded; Preheat the welding area; The accessory is welded to the pipe (1), and the weld is polished. When the accessory is welded to the pipe (1), a H08CrMoA heat-resistant steel welding wire with a diameter of 2 mm is used for groove welding filling. The welding joints are arranged in a staggered manner. Argon is used as a protective gas during welding. The ventilation speed is 5-6L / min, and a temperature measuring gun is used to continuously measure the temperature of the welding position so that the interlayer temperature is maintained at 280°C; wherein the welding filling includes multiple weld passes, and the multiple weld passes form the bottom layer (3), the middle layer and the top layer of the weld. (4), the bottom layer (3), the middle layer and the top layer (4) are welded with different current intensities, the current intensity of the bottom layer (3) during welding is smaller than that of the middle layer, the current intensity of the middle layer during welding is smaller than that of the top layer (4), the weld bead of the bottom layer (3) is closest to the bottom of the groove and is welded with a small current of 60±20A, the weld bead of the middle layer is welded with a current of 80±20A, and the weld bead of the top layer (4) is welded with a current of 100±20A; The welding parts are kept warm and slowly cooled, and finally heat treated and tempered; During the insulation and slow cooling, the temperature of the welding position is measured. When the temperature of the welding position is measured to have dropped to 180°C, the welding position is heated to 250°C, and then the heating is stopped and the temperature measurement is continued. When the temperature of the welding position is measured to have dropped to 120°C, the welding position is heated to 180°C again, and then the heating is stopped and the temperature measurement is continued. When the temperature of the welding position is measured to have dropped to 60°C, the welding position is heated to 120°C again, and then the heating is stopped until the welding position is naturally cooled to room temperature.
2. The high-strength welding method for arc-shaped surface attachments according to claim 1, characterized in that: Before preheating and welding, the accessory is connected to the pipe (1) by spot welding to perform pre-positioning.
3. The high-strength welding method for arc-shaped surface attachments according to claim 1, characterized in that: The filling material for spot welding is H08CrMoA heat-resistant steel welding wire with a diameter of 1.2mm. During spot welding, argon is used as the protective gas, the ventilation speed is 5-6L / min, the current polarity is direct current electrode positive connection, the welding current is 120±30A, the welding voltage is 20±3V, and the welding speed is 16cm / min.
4. The high-strength welding method for arc-shaped surface attachments according to claim 1, characterized in that: During preheating, heat the area to be welded to 200-250°C.
Citation Information
Cited By
Welding process for double-layer special-shaped metal product
CN122353074A
A welding process for a double-layered profiled metal product