A waterproof and wear-resistant coating and its preparation method

By using a carbon-fluorocarbon chain modified epoxy resin to coat granular fillers and flake fillers in an alternating stacked structure, the problem of insufficient waterproofing and wear resistance of water-based polymer coatings is solved, achieving a highly efficient waterproof and wear-resistant effect for the coating.

CN118546595BActive Publication Date: 2026-11-17SHOUBANG CHEM CO LTD GAOMING DISTRICT FOSHAN CITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410953309.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2026-11-17
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Existing water-based polymer coatings have shortcomings in terms of waterproofing and abrasion resistance. In particular, fillers tend to aggregate during the coating preparation process, making it difficult to exert a reinforcing effect. Furthermore, excessive use of fluorinated resins can affect the coating's viscosity and increase costs.

Method used

Particulate fillers are coated with fluorocarbon-modified epoxy resin and combined with sheet fillers to form an interleaved stacked structure. The hydrophobicity of the fluorocarbon chain and the chemical stability of the sheet fillers improve the waterproof and wear-resistant properties of the coating.

Benefits of technology

It improves the waterproofness and abrasion resistance of the coating, while maintaining its fluidity and cost-effectiveness, and enhances the hardness and adhesion of the coating.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The first aspect of this invention provides a method for preparing a waterproof and wear-resistant coating, comprising the following steps: (1) preparing a fluorocarbon chain modified epoxy resin; (2) mixing particulate filler with the fluorocarbon chain modified epoxy resin and then extruding, crushing and sieving to obtain a coated filler with a particle size of 2-10 μm; (3) mixing the coated filler with an aqueous coating emulsion, a flake filler and water to obtain the waterproof and wear-resistant coating. In the above method for preparing the waterproof and wear-resistant coating, the fluorocarbon chain modified epoxy resin coats the particulate filler to form a coated filler. The coated filler can be uniformly mixed in the coating, and the flake filler is distributed in the gaps between the coated filler to form an interleaved stacked structure, which can provide enhanced wear resistance while preventing moisture ingress. Furthermore, because the surface energy of the fluorocarbon chain is low, it easily migrates to the surface of the coated filler, thereby further improving the hydrophobicity of the gaps between the coated filler and further improving the waterproof performance of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coatings, specifically a waterproof and wear-resistant coating and its preparation method. Background Technology

[0002] Water-based polymer coatings are environmentally friendly coatings that use water as a solvent. They have low volatile organic compound (VOC) content, posing less harm to the environment and human health, and are widely used in furniture and interior decoration. After curing, water-based polymer coatings form a continuous film with molecular gaps smaller than 5 nm, effectively preventing water molecules from passing through. However, larger pores may form in certain areas, allowing water molecules to penetrate the film surface and affecting the internal structure of the coating. Conventional water-based polymer coatings generally have poor abrasion resistance, requiring the addition of fillers to improve wear resistance. However, fillers tend to aggregate during coating preparation, hindering their effectiveness in enhancing abrasion resistance. Using fluorinated resins can improve the coating's water resistance and strength; however, using resins with excessively high fluorine content can lead to excessively viscous coatings, affecting application, and significantly increasing costs.

[0003] CN114250029A discloses a waterproof coating and its preparation method. The preparation method includes: (1) preparing nanodiamond powder; (2) preparing aluminum hydroxide-coated nanodiamond powder; (3) preparing flaky mesoporous flakes; (4) preparing a composite dispersion; and (5) preparing a waterproof coating. This invention utilizes a composite dispersion in which flaky mesoporous flakes coated with aluminum hydroxide and charcoal powder are stacked in multiple layers, forming multiple barrier layers. Combined with the synergistic effect of the surface alumina, this further enhances the waterproof and moisture-proof properties. The nanodiamond powder coated within the alumina is uniformly adsorbed into the flakes and charcoal powder, effectively improving the scratch and wear resistance of the coating after film formation. While it possesses improved waterproof and wear-resistant properties, to meet market demands, it is necessary to provide a coating with even better waterproof and wear-resistant properties.

[0004] Therefore, it is necessary to provide a waterproof and wear-resistant coating and its preparation method. Summary of the Invention

[0005] The first aspect of this invention provides a method for preparing a waterproof and wear-resistant coating, comprising the following steps: (1) Preparation of fluorocarbon chain modified epoxy resin; (2) The granular filler is mixed with the fluorocarbon modified epoxy resin and then extruded, crushed and sieved to obtain a coated filler with a particle size of 2-10 μm. (3) The waterproof and wear-resistant coating is obtained by mixing the coating filler with water-based coating emulsion, flake filler and water.

[0006] The above-mentioned method for preparing waterproof and wear-resistant coatings involves coating particulate fillers with fluorocarbon-modified epoxy resin to form a coated filler. This coated filler can be uniformly mixed in the coating, with the lamellar filler distributed within the gaps between the coated fillers, forming a staggered stacked structure. This provides enhanced wear resistance while preventing moisture penetration. Furthermore, due to the low surface energy of the fluorocarbon chains, they easily migrate to the surface of the coated filler, further improving the hydrophobicity of the gaps between the coated fillers and thus enhancing the waterproof performance of the coating. Simultaneously, the fluorocarbon-modified epoxy resin coating the surface of the particulate fillers does not adversely affect the coating. Therefore, the coating prepared by this method exhibits improved wear resistance and waterproof properties.

[0007] Furthermore, the particulate filler is silica. Silica can enhance the hardness and adhesion of the coating.

[0008] Furthermore, the flaky filler is at least one of glass flakes and mica powder. Glass flakes and mica powder have good chemical stability, which can improve the corrosion resistance of the coating.

[0009] Furthermore, the particle size of the sheet-like filler is 5-10 μm. The sheet-like filler with this particle size can form a denser stacked structure with the coated filler, further improving wear resistance and water resistance.

[0010] Furthermore, the fluorocarbon chain modified epoxy resin contains -CF3 (CF2). a (CH2) b Side chains. The above resins exhibit strong hydrophobicity and stability.

[0011] Furthermore, the preparation method of the fluorocarbon chain modified epoxy resin includes: dissolving bisphenol A type epoxy resin in tetrahydrofuran, adding perfluorooctanoic acid and triethylamine dropwise at 50-80°C, reacting for 3-6 hours, cooling and concentrating, and adding ethanol for precipitation to obtain the fluorocarbon chain modified epoxy resin. The above method can yield epoxy resin containing -CF3 (CF2). a (CH2) b Epoxy resin with fluorocarbon side chains.

[0012] Furthermore, the mass ratio of the epoxy resin to the fluorocarboxylic acid is 1:(0.1-0.4). The fluorocarbon chain modified epoxy resin prepared by the above ratio has good mechanical strength and water resistance, as well as good flowability.

[0013] Furthermore, the waterborne coating emulsion comprises at least one of a waterborne acrylic emulsion and a waterborne epoxy resin emulsion.

[0014] Further, by weight, 20-30 parts of the coating emulsion, 2-5 parts of the coating filler, 2-5 parts of the flake filler and 25-35 parts of water are mixed.

[0015] A second aspect of this invention provides a waterproof and abrasion-resistant coating prepared by the above-described preparation method. This coating exhibits improved abrasion resistance and waterproof properties. Detailed Implementation

[0016] To facilitate understanding of this application, a more complete description will be provided below. This application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of this application.

[0017] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of the application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified. In the description of this application, "several" means at least one, such as one, two, etc., unless otherwise explicitly specified.

[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0019] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0020] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0021] Unless otherwise specified, the percentage content mentioned in this application refers to mass percentage for solid-liquid mixtures and solid-phase-solid mixtures, and volume percentage for liquid-phase-liquid mixtures.

[0022] Unless otherwise specified, all percentage concentrations mentioned in this application refer to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of that component.

[0023] Unless otherwise specified, the temperature parameters in this application may be either constant temperature processing or processing within a certain temperature range. The constant temperature processing allows for temperature fluctuations within the precision range controlled by the instrument.

[0024] The term "particle" as used in this application, or a substance with a defined particle size distribution, is not necessarily spherical in shape; it may be irregular and can be either primary or secondary particles. The particle size of irregular particles is calculated as the average of their maximum and minimum diameters.

[0025] Bisphenol A type epoxy resin (molecular weight 10000) was dissolved in 10 times its volume of tetrahydrofuran, heated to 60°C and mixed thoroughly. Perfluorooctanoic acid and triethylamine were added dropwise at a rate of 0.1 mL / min. After reacting for 3 hours, the mixture was cooled to room temperature and concentrated. Ethanol was added to precipitate the resin, and after drying, the fluorocarbon chain modified epoxy resin was obtained.

[0026] The above-mentioned fluorocarbon chain modified epoxy resin and an equal mass of particulate filler (silica, particle size 100nm) were mixed in a mixer, then extruded at 90°C, crushed and sieved (6250 mesh) to obtain a coated filler with a particle size of 2μm.

[0027] The above-mentioned coated filler is mixed with 6 times the mass of water-based acrylic emulsion, 1 times the mass of flake filler (mica powder, particle size 5μm), and 3 times the mass of water and dispersed for 60 minutes to obtain a waterproof and wear-resistant coating.

[0028] Bisphenol A type epoxy resin (molecular weight 10000) was dissolved in 10 times its volume of tetrahydrofuran, heated to 60°C and mixed thoroughly. Perfluorooctanoic acid and triethylamine were added dropwise at a rate of 0.1 mL / min. After reacting for 3 hours, the mixture was cooled to room temperature and concentrated. Ethanol was added to precipitate the resin, and after drying, the fluorocarbon chain modified epoxy resin was obtained.

[0029] The above-mentioned fluorocarbon chain modified epoxy resin and an equal mass of particulate filler (silica, particle size 100nm) were mixed in a mixer, then extruded at 90°C, crushed and sieved (6250 mesh) to obtain a coated filler with a particle size of 10μm.

[0030] The above-mentioned coated filler is mixed with 6 times the mass of water-based epoxy resin emulsion, 1 times the mass of flake filler (mica powder, particle size 5μm) and 3 times the mass of water and dispersed for 60 minutes to obtain a waterproof and wear-resistant coating.

[0031] Bisphenol A type epoxy resin (molecular weight 10000) was dissolved in 10 times its volume of tetrahydrofuran, heated to 60°C and mixed thoroughly. Perfluorooctanoic acid and triethylamine were added dropwise at a rate of 0.1 mL / min. After reacting for 3 hours, the mixture was cooled to room temperature and concentrated. Ethanol was added to precipitate the resin, and after drying, the fluorocarbon chain modified epoxy resin was obtained.

[0032] The above-mentioned fluorocarbon chain modified epoxy resin and an equal mass of particulate filler (silica, particle size 100nm) were mixed in a mixer, then extruded at 90℃, crushed and sieved (1250 mesh) to obtain a coated filler with a particle size of 10μm.

[0033] The above-mentioned coated filler is mixed with 6 times the mass of water-based acrylic emulsion, 1 times the mass of flake filler (glass flakes, 10μm) and 3 times the mass of water and dispersed for 60 minutes to obtain a waterproof and wear-resistant coating.

[0034] Bisphenol A type epoxy resin (molecular weight 10000) was dissolved in 10 times its volume of tetrahydrofuran, heated to 60°C and mixed thoroughly. Perfluorooctanoic acid and triethylamine were added dropwise at a rate of 0.1 mL / min. After reacting for 3 hours, the mixture was cooled to room temperature and concentrated. Ethanol was added to precipitate the resin, and after drying, the fluorocarbon chain modified epoxy resin was obtained.

[0035] The above-mentioned fluorocarbon chain modified epoxy resin and an equal mass of particulate filler (silica, particle size 100nm) were mixed in a mixer, then extruded at 90°C, crushed and sieved (6250 mesh) to obtain a coated filler with a particle size of 2μm.

[0036] The above-mentioned coated filler is mixed with 6 times the mass of water-based acrylic emulsion, 1 times the mass of flake filler (mica powder, particle size 5μm), and 3 times the mass of water and dispersed for 60 minutes to obtain a waterproof and wear-resistant coating.

[0037] Bisphenol A type epoxy resin (molecular weight 10000) was dissolved in 10 times its volume of tetrahydrofuran, heated to 60°C and mixed thoroughly. Perfluorooctanoic acid and triethylamine were added dropwise at a rate of 0.1 mL / min. After reacting for 3 hours, the mixture was cooled to room temperature and concentrated. Ethanol was added to precipitate the resin, and after drying, the fluorocarbon chain modified epoxy resin was obtained.

[0038] The above-mentioned fluorocarbon chain modified epoxy resin and an equal mass of particulate filler (silica, particle size 100nm) were mixed in a mixer, then extruded at 90°C, crushed and sieved (6250 mesh) to obtain a coated filler with a particle size of 2μm.

[0039] The above-mentioned coated filler is mixed with 10 times the mass of water-based acrylic emulsion, 1 times the mass of flake filler (mica powder, particle size 5μm), and 3 times the mass of water and dispersed for 60 minutes to obtain a waterproof and wear-resistant coating.

[0040] Bisphenol A type epoxy resin (molecular weight 10000) was dissolved in 10 times its volume of tetrahydrofuran, heated to 60°C and mixed thoroughly. Perfluorooctanoic acid and triethylamine were added dropwise at a rate of 0.1 mL / min. After reacting for 3 hours, the mixture was cooled to room temperature and concentrated. Ethanol was added to precipitate the resin, and after drying, the fluorocarbon chain modified epoxy resin was obtained.

[0041] The above-mentioned fluorocarbon chain modified epoxy resin and an equal mass of particulate filler (silica, particle size 100nm) were mixed in a mixer, then extruded at 90°C, crushed and sieved (6250 mesh) to obtain a coated filler with a particle size of 2μm.

[0042] The above-mentioned coated filler is mixed with 6 times the mass of water-based acrylic emulsion, 0.3 times the mass of flake filler (mica powder, particle size 5μm), and 3 times the mass of water and dispersed for 60 minutes to obtain a waterproof and wear-resistant coating.

[0043] Comparative Example 1 A waterproof and wear-resistant coating is obtained by mixing 6 times the mass of water-based acrylic emulsion, 2 times the mass of flake filler (mica powder, particle size 5μm), and 3 times the mass of water and dispersing for 60 minutes.

[0044] Comparative Example 2 A waterproof and wear-resistant coating is obtained by mixing 6 times the mass of water-based acrylic emulsion, 2 times the mass of particulate filler (silica, particle size 100nm), and 3 times the mass of water and dispersing for 60 minutes.

[0045] Comparative Example 3 A waterproof and wear-resistant coating is obtained by mixing granular filler (silica, particle size 100nm) with 6 times the mass of water-based acrylic emulsion, 1 times the mass of flake filler (mica powder, particle size 5μm) and 3 times the mass of water and dispersing for 60 minutes.

[0046] Comparative Example 4 Bisphenol A type epoxy resin (molecular weight 10000) and an equal mass of particulate filler (silica, particle size 100nm) are mixed in a mixer, then extruded at 90℃, crushed and sieved (6250 mesh) to obtain a coated filler with a particle size of 2μm.

[0047] The above-mentioned coated filler is mixed with 6 times the mass of water-based acrylic emulsion, 1 times the mass of flake filler (mica powder, particle size 5μm), and 3 times the mass of water and dispersed for 60 minutes to obtain a waterproof and wear-resistant coating.

[0048] The impermeability of the coatings in Examples 1-6 and Comparative Examples 1-4 after temperature cycling was tested according to JG / T 25-2017 "Test Method for Temperature Change Resistance of Building Coatings" and GB / T16777-2008 "Test Method for Waterproof Coatings for Buildings". The high and low temperature parameters were 100℃ and -30℃, respectively. The hardness was tested according to GB / T 6739-2006 "Determination of Hardness of Paint Film by Pencil Method" and a scratch test was performed using 450N. The test results are shown in Table 1.

[0049] project Water impermeability after 5 temperature cycles hardness scratches Example 1 0.3MPa, impermeable for 80 minutes 6H No scratches Example 2 0.3MPa, impermeable for 70 minutes 6H No scratches Example 3 0.3MPa, impermeable for 60 minutes 6H No scratches Example 4 0.3MPa, impermeable for 90 minutes 7H No scratches Example 5 0.3MPa, impermeable for 60 minutes 5H No scratches Example 6 0.3MPa, impermeable for 70 minutes 6H No scratches Comparative Example 1 0.3MPa, impermeable for 30 minutes 2H Obvious scratches Comparative Example 2 0.3MPa, impermeable for 20 minutes 3H Minor scratches Comparative Example 3 0.3MPa, impermeable for 40 minutes 4H Minor scratches Comparative Example 4 0.3MPa, impermeable for 40 minutes 6H No scratches According to the data in Table 1, the coatings of Examples 1-6 have improved waterproof and / or abrasion resistance compared to Comparative Examples 1-4. This is because the present method uses fluorocarbon-modified epoxy resin to coat particulate fillers to form coated fillers. The coated fillers can be uniformly mixed in the coating, and the flake fillers are distributed in the gaps between the coated fillers to form an interlaced stacked structure, which can provide enhanced abrasion resistance while preventing moisture from entering. Furthermore, because the surface energy of the fluorocarbon chain is low, it is easy to migrate to the surface of the coated filler, thereby further improving the hydrophobicity of the gaps between the coated fillers and further improving the waterproof performance of the coating. Comparative Example 1 used flake fillers, which can form a flake-like stacked structure, but the waterproof performance and strength of the structure are poor. Comparative Example 2 used particulate fillers, which improved the abrasion resistance of the coating; however, its structure has low density, making it difficult to prevent moisture from entering. Comparative Example 3 used uncoated particulate fillers, which can form an interlaced stacked structure with the flake fillers; however, the particle size difference is large, and there are still pores in the formed structure, allowing moisture to enter the coating through the gaps in the acrylic resin. Comparative Example 4 used unmodified bisphenol A type epoxy resin, which could not improve the hydrophobicity of the gaps, thus exhibiting low hydrophobicity.

[0050] Example 3 used larger-sized flake fillers, which affected the compactness of the interlocking structure, resulting in slightly reduced water resistance and hardness compared to Example 1. Example 4 used a higher proportion of perfluorooctanoic acid (PFOA), enhancing the hydrophobicity and strength of the fluorocarbon-modified epoxy resin. Simultaneously, because the fluorocarbon-modified epoxy resin coated the surface of the particulate filler, it did not adversely affect the coating performance, resulting in improved water resistance and abrasion resistance. Example 5 used lower contents of both particulate and flake fillers, and Example 6 used an even lower proportion of flake fillers, thus leading to poorer water resistance and abrasion resistance in the coating.

[0051] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0052] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A method for preparing a waterproof and wear-resistant coating, characterized in that, Includes the following steps: (1) Preparation of fluorocarbon chain modified epoxy resin; (2) The granular filler is mixed with the fluorocarbon modified epoxy resin and then extruded, crushed and sieved to obtain a coated filler with a particle size of 2-10 μm. (3) The waterproof and wear-resistant coating is obtained by mixing the coating filler with water-based paint emulsion, flake filler and water. Specifically, the coating filler is mixed with 6 times the mass of water-based paint emulsion, 1 times the mass of flake filler and 3 times the mass of water and dispersed for 60 minutes to obtain the waterproof and wear-resistant coating. The particle size of the sheet-like filler is 5-10 μm; The preparation method of the fluorocarbon chain modified epoxy resin includes: dissolving bisphenol A type epoxy resin in 10 times its volume of tetrahydrofuran, heating to 60°C and mixing evenly, adding 0.1 or 0.4 times its volume of perfluorooctanoic acid and 0.0001 times its volume of triethylamine dropwise at a rate of 0.1 mL / min, reacting for 3 hours, cooling to room temperature and concentrating, adding ethanol for precipitation, and drying to obtain the fluorocarbon chain modified epoxy resin; The waterborne coating emulsion comprises at least one of waterborne acrylic emulsion and waterborne epoxy resin emulsion.

2. The method for preparing the waterproof and wear-resistant coating according to claim 1, characterized in that, The granular filler is silicon dioxide.

3. The method for preparing the waterproof and wear-resistant coating according to claim 1, characterized in that, The sheet-like filler is at least one of glass flakes and mica powder.

4. A waterproof and wear-resistant coating, characterized in that, Prepared using the preparation method according to any one of claims 1-3.

Citation Information

Patent Citations

  • Fluorine-containing epoxy resin and preparation method thereof, and double-super-hydrophobic surface preparing from fluorine-containing epoxy resin

    CN103588955A

  • composition

    CN113853409A

  • Decorative material with wear resistance

    JP1999077944A