A fixture for eutectic welding of power amplifier chips and a method for processing and using the fixture
By designing positioning pieces and pressure blocks made of high-purity graphite base and ceramic materials, combined with laser-processed fixtures, the problems of difficult pressure application and low precision in eutectic welding of radio frequency power amplifier chips are solved, and efficient and precise welding results are achieved. .
Patent Information
- Application Number
- CN202411019815.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-29
AI Technical Summary
In the existing technology, in the eutectic welding of radio frequency power amplifier chips, it is difficult to apply pressure due to different chip heights, and the production efficiency is low. The small size of the radio frequency chip and the limited contact area on the surface make the pressing process difficult.
A power amplifier chip eutectic welding fixture is designed, which includes a high-purity graphite base, a positioning piece and a pressing block made of ceramic materials. Laser processing is used to manufacture bosses and avoidance grooves of different heights. It is combined with claw springs and copper needles to achieve precise installation. Pressure and positioning.
It realizes the simultaneous application of pressure to chips of different types and thicknesses, ensuring welding integrity, improving production efficiency and accuracy. Ceramic materials do not bond in high-temperature environments, avoiding solder rejection treatment.
Smart Images

Figure CN118553679B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of chip eutectic welding, and in particular to a fixture for eutectic welding of a power amplifier chip and a processing and use method of the fixture. Background Art
[0002] The following problems currently exist in the eutectic welding of multiple chips in a vacuum furnace inside an RF power amplifier tube: First, when multiple chips / devices are eutectic at the same time on the power amplifier tube shell / carrier, it is difficult to apply pressure to all chips / devices at the same time with existing technology due to the different heights of each chip / device. Second, when using a vacuum eutectic furnace for multi-chip eutectic welding, due to the small space, the large variety of devices / chips and the small gaps, the devices / chips are very small and light. The current method of manually placing devices / chips is prone to tipping over or sliding to the bottom of the positioning piece when placing, resulting in the need to remove the positioning piece and all devices / chips and then re-place them, resulting in low production efficiency. Third, the RF chip / monolithic microwave integrated circuit (MMIC) itself is very small in size, and the area on its surface that can be contacted and pressed is very limited, making it difficult to process the pressing block itself and the avoidance area of the pressing block connected to it. Summary of the invention
[0003] Based on the above problems, the present invention provides a fixture for eutectic welding of power amplifier chips and a method for processing and using the fixture.
[0004] A fixture for eutectic welding of a power amplifier chip, comprising: a base, a preformed welding sheet, a positioning sheet, a pressing block and a counterweight block;
[0005] The base is provided with a tube shell positioning groove for placing chip devices and power amplifier tube shells, and the inner chamber of the power amplifier tube shell is sequentially provided with a preformed solder sheet, a positioning sheet, a pressing block and a counterweight block from bottom to top; the positioning sheet is provided with a device positioning groove, and the chip device is placed in the device positioning groove, and the same pressing block is pressed on the upper surface of multiple chip devices, and the counterweight block is located on the upper part of the pressing block;
[0006] The lower surface of the pressing block is provided with bosses of different heights.
[0007] Furthermore, a pressing installation hole is provided on the base, a pressing member is provided through the pressing installation hole, and a pressing end of the pressing member is connected to the positioning piece.
[0008] Furthermore, the pressing member is a claw spring, and a U-shaped copper needle is movably inserted into the claw spring.
[0009] Furthermore, the positioning piece and the pressing block are both made of ceramic materials.
[0010] Furthermore, the base is entirely made of high-purity graphite.
[0011] Furthermore, the above-mentioned bosses include a first-level boss, a second-level boss and a third-level boss. The height of the first-level boss is 0.2 mm, the height of the second-level boss is 0.15 mm, and the height of the third-level boss is 0.05 mm.
[0012] A method for processing a power amplifier chip eutectic welding fixture, using the above fixture, comprises the following steps:
[0013] S1: processing the preformed solder piece according to the size of the power amplifier tube shell in the tube shell positioning groove, so that the side of the preformed solder piece is connected to the inner wall of the power amplifier tube shell;
[0014] S2: Making a ceramic sheet into a positioning sheet; firstly, processing a ceramic sheet with uniform thickness according to the length and width of the inner cavity of the power amplifier tube shell, so that the length and width of the ceramic sheet match the inner cavity of the power amplifier tube shell, and then processing a device positioning groove on the ceramic sheet according to the layout requirements of the chip device, and the length and width of the device positioning groove are adapted to the preset length and width of the chip device; the ceramic sheet is processed by laser cutting;
[0015] S3: Processing the outer dimensions of the pressing block to be the same as those of the positioning sheet, and then processing bosses of different heights in sequence on the pressing block by laser etching according to the device positioning grooves on the positioning sheet and the layout of chip devices of different thicknesses;
[0016] Processing sequence: first form the highest boss, then continue etching some of the highest bosses to form bosses of the next level, and continue laser etching the bosses in descending order until all bosses of different heights are processed;
[0017] S4: Processing an avoidance groove and setting a placement area for a counterweight on the pressing block. The position of the avoidance groove is selected according to the position of the lower pressing piece, and the placement area for the counterweight is located at the center of the pressing block.
[0018] Furthermore, in the above S2, a CAD plan is first made according to the layout requirements of the chip device, and then the CAD plan is imported into the laser processing equipment, the parameters and focal length of the laser processing equipment are adjusted, and then the laser processing equipment cuts the ceramic sheet according to the CAD plan to form a positioning sheet.
[0019] A method for using a eutectic welding fixture for a power amplifier chip, using the above-mentioned fixture, comprises the following steps:
[0020] Step 1: Clean the preformed solder sheet using plasma cleaning or isopropyl alcohol liquid;
[0021] Step 2: Place the power amplifier tube shell inside the tube shell positioning groove of the base, place the cleaned preformed solder sheet inside the power amplifier tube shell, place the positioning sheet on the preformed solder sheet, and install the pressing piece on the pressing installation hole so that the pressing piece presses the positioning sheet on the preformed solder sheet;
[0022] Step 3: Place the chip devices of different thicknesses in the device positioning grooves of the positioning sheet according to the predetermined layout and confirm that they are correct;
[0023] Step 4: placing a pressing block above the chip device, so that each boss on the lower surface of the pressing block is aligned with and connected to the corresponding chip device; the part where the boss and the chip device are connected is the contactable area on the chip device;
[0024] Step 5: placing a counterweight on the upper surface of the pressing block;
[0025] Step 6: Place the eutectic fixture containing the chip device into the furnace chamber of the vacuum eutectic furnace;
[0026] Step 7: Setting a vacuum eutectic welding curve, and performing vacuum eutectic welding according to the set vacuum eutectic welding curve;
[0027] Step 8: Perform microscope inspection and X-ray penetration inspection on the power amplifier chip that has completed vacuum eutectic welding.
[0028] Among them, the vacuum eutectic welding curve in step seven is as follows:
[0029] Before the vacuum eutectic furnace is heated up, the air in the eutectic furnace cavity is replaced by evacuating the cavity and filling the cavity with nitrogen twice, so that the temperature in the cavity is 25°C and the pressure is one standard atmospheric pressure.
[0030] The temperature in the furnace chamber rises from 25°C to 200°C and is kept warm for 2 minutes. During this process, formic acid gas is continuously filled into the furnace chamber at a flow rate of 10-20slm.
[0031] The temperature in the furnace chamber is raised from 200°C to 240°C. During the heating process, vacuum is drawn to discharge the reaction waste gas. When the temperature in the furnace chamber reaches 240°C, it is kept warm for 1 minute. During this warm-keeping period, formic acid gas is again filled into the furnace chamber to flush the furnace chamber.
[0032] The temperature in the furnace chamber rises from 240°C to 310°C, and then starts to evacuate after reaching 270°C. After the temperature in the furnace chamber reaches 310°C, it is kept warm for 30 seconds to achieve vacuum eutectic welding of the power amplifier chip.
[0033] The temperature in the furnace chamber quickly dropped from 310°C to room temperature, and nitrogen was continuously filled in during the cooling process with a nitrogen flow rate of 30-60slm.
[0034] The present invention has the following beneficial effects:
[0035] (1) The base of the fixture of the present invention is made of high-purity graphite, which has excellent thermal conductivity and uniform heat transfer, can quickly transfer heat for eutectic welding, and graphite is easy to process.
[0036] (2) The positioning plate and the pressing block of the clamp of the present invention are both made of ceramic material. Compared with metal sheets of the same thickness, they have higher strength and hardness and can achieve better flatness. Moreover, the ceramic material will not adhere to the welding material even in a high-temperature environment, and is easy to separate from the welding material and does not require solder rejection treatment on the surface.
[0037] (3) The fixture of the present invention can simultaneously apply pressure for eutectic welding of chip devices of different models and thicknesses, thereby ensuring that each chip device can overcome the surface tension of the solder during welding and achieve complete welding.
[0038] (4) The positioning piece and the pressing block of the fixture of the present invention are both processed by laser, which can meet the needs of fine processing and has high processing accuracy.
[0039] (5) The boss on the pressing block of the clamp of the present invention is etched with a non-contact avoidance area according to the sensitive area of the RF chip to avoid contact between the boss and the sensitive area of the RF chip. The processing of the boss is achieved by laser etching, which can realize the processing of micro-sized bosses and avoidance areas. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is a schematic diagram of the overall structure of the clamp of the present invention;
[0041] Figure 2 It is a schematic structural diagram of a base in the clamp of the present invention;
[0042] Figure 3 This is a schematic diagram of the assembly structure of the clamp of the present invention after the base is hidden;
[0043] Figure 4 for Figure 3 Exploded diagram of the assembly structure;
[0044] Figure 5 It is a schematic structural diagram of a positioning piece in the clamp of the present invention;
[0045] Figure 6 It is a schematic diagram of the structure of the pressing block in the clamp of the present invention;
[0046] Figure 7 It is a schematic diagram of assembling the chip device and the pressing block in the fixture of the present invention;
[0047] Figure 8 It is a schematic diagram of the vacuum eutectic welding curve in the present invention.
[0048] In the figure: 1-base; 101-tube shell positioning groove; 102-pressing mounting hole; 103-claw spring; 104-copper needle; 2-power amplifier tube shell; 3-preformed solder sheet; 4-positioning sheet; 401-device positioning groove; 5-chip device; 6-pressing block; 601-first-level boss; 602-second-level boss; 603-third-level boss; 604-avoidance groove; 7-counterweight block. DETAILED DESCRIPTION
[0049] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0050] Embodiment 1
[0051] refer to Figures 1 to 5 The present invention provides a fixture for eutectic welding of a power amplifier chip, comprising: a base 1, a preformed welding sheet 3, a positioning sheet 4, a pressing block 6 and a counterweight block 7.
[0052] The base 1 is made entirely of high-purity graphite, which has the advantages of good thermal conductivity and uniform heat transfer, and can transfer heat quickly and evenly during welding; the base 1 is provided with tube shell positioning grooves 101 for placing chip devices 5 and power amplifier tube shells 2, and the number and length, width and height size parameters of the tube shell positioning grooves 101 are set according to the type and layout of the chip devices 5 to be welded.
[0053] The inner chamber of the power amplifier tube shell 2 is sequentially provided with a preformed solder sheet 3, a positioning sheet 4, a pressing block 6 and a counterweight 7 from bottom to top. A device positioning groove 401 is provided on the positioning sheet 4. The size of the device positioning groove 401 is slightly larger than the chip device 5. The chip device 5 is placed in the device positioning groove 401, and the same pressing block 6 is pressed on the upper surface of multiple chip devices 5. The counterweight 7 is located on the upper part of the pressing block 6. The lower surface of the pressing block 6 is provided with bosses of different heights. When the pressing block 6 is placed, the bosses on the lower surface of the pressing block 6 are embedded in the device positioning groove 401 to play a positioning role. The pressing block 6 will not be deflected, and the pressing block 6 simultaneously applies pressure to the chip devices 5 of different thicknesses to ensure that each chip device 5 is in contact with the preformed solder sheet 3, thereby ensuring that each chip device 5 can achieve complete welding.
[0054] Preferably, the positioning piece 4 and the pressing block 6 are both made of ceramic material. The positioning piece 4 and the pressing block 6 made of ceramic material have high strength and hardness, and are not easily deformed under the action of external force and high temperature, so that they have good flatness, ensuring the accuracy and reliability of welding. In addition, the ceramic material does not react with the welding device material, and does not need to be subjected to surface solder rejection treatment.
[0055] The base 1 is also provided with a pressing installation hole 102 , through which a pressing piece is arranged, and a pressing end of the pressing piece is connected to the positioning piece 4 , so as to press the positioning piece 4 onto the preformed welding piece 3 .
[0056] Optionally, the pressing member is a claw spring 103, which is fixed in the pressing installation hole 102. A U-shaped copper needle 104 is movably inserted on the claw spring 103 to position and press the positioning piece 4. The copper needle 104 is made of pure copper, and its diameter matches the selected claw spring 103. Of course, it can also be made of a metal material such as aluminum that is elastic and resistant to high temperatures. The claw spring 103 is a conventional standard product.
[0057] In order not to affect the subsequent assembly operation, the claw spring 103 and the copper needle 104 are arranged on both sides of the positioning sheet 4, and the copper needle 104 is slightly higher than the top edge of the power amplifier tube shell 2.
[0058] Embodiment 2
[0059] In order to obtain the fixture as described in the first embodiment, this embodiment provides a method for processing a eutectic welding fixture for a power amplifier chip, comprising the following steps:
[0060] S1: processing the preformed solder piece 3 according to the size of the power amplifier tube shell 2 in the tube shell positioning groove 101, so that the side of the preformed solder piece 3 is connected to the inner wall of the power amplifier tube shell 2;
[0061] S2: Making a ceramic sheet into a positioning sheet 4; firstly, processing a ceramic sheet of uniform thickness according to the length and width of the inner chamber of the power amplifier tube shell 2, so that the length and width of the ceramic sheet match the inner chamber of the power amplifier tube shell 2, and the side wall of the positioning sheet 4 is limitedly connected with the inner side wall of the inner chamber of the power amplifier tube shell 2, and then processing a device positioning groove 401 on the ceramic sheet according to the layout requirements of the chip device 5, and the length and width of the device positioning groove 401 are adapted to the preset length and width of the chip device 5; the processing method of the ceramic sheet is laser cutting;
[0062] S3: The outer dimensions of the pressing block 6 are processed to be the same as those of the positioning sheet 4, and the side wall of the pressing block 6 is also limitedly connected with the inner side wall of the inner cavity of the power amplifier tube shell 2, and then according to the device positioning groove 401 on the positioning sheet 4 and the layout of the chip devices 5 of different thicknesses, bosses of different heights are processed in sequence on the pressing block 6 by laser etching;
[0063] Processing sequence: first form the highest boss, then continue etching some of the highest bosses to form bosses of the next level, and continue laser etching the bosses in descending order until all bosses of different heights are processed;
[0064] S4: Process an avoidance groove 604 on the pressing block 6 and set a placement area for the counterweight block 7. The position of the avoidance groove 604 is selected according to the position of the lower pressing piece. The placement area of the counterweight block 7 is located at the center of the pressing block 6. The placement area of the counterweight block 7 can be achieved by laser marking.
[0065] In order to automatically perform the processing of the positioning plate 4, in step S2, a CAD plan is first prepared according to the layout requirements of the chip device 5, and then the CAD plan is imported into the laser processing equipment, the parameters and focal length of the laser processing equipment are adjusted, and then the laser processing equipment cuts the ceramic sheet according to the CAD plan to form the positioning plate 4; in this embodiment, the laser light source is a fiber laser, and the cutting power is about 55%.
[0066] As an example, in the above S3, the thickness of the positioning sheet 4 and the pressing block 6 are both 0.3 mm, the thickness of the chip device 5 includes three types: 0.1 mm, 0.15 mm, and 0.25 mm, and the bosses on the lower surface of the pressing block 6 include a first-level boss 601, a second-level boss 602, and a third-level boss 603. For details, refer to Figure 6 and Figure 7 The height of the first-level boss 601 is 0.2 mm, the height of the second-level boss 602 is 0.15 mm, and the height of the third-level boss 603 is 0.05 mm. The first-level boss 601 is used to connect with the chip device 5 with a thickness of 0.1 mm, the second-level boss 602 is used to connect with the chip device 5 with a thickness of 0.15 mm, and the third-level boss 603 is used to connect with the chip device 5 with a thickness of 0.25 mm.
[0067] Specifically, first, a predetermined area on the pressing block 6 is etched to a depth of 0.2 mm, with a laser power of 30%, an etching rate of 200, and etching for 20 times, so that a boss with a height of 0.2 mm can be obtained, i.e., the first-level boss 601. Then, based on the first-level boss 601, 0.05 mm is etched again, with a laser power of 30%, an etching rate of 200, and etching for 4 times, so that a boss with a height of 0.15 mm can be obtained, i.e., the second-level boss 602. Finally, based on the second-level boss 602, the remaining bosses are etched to a depth of 0.1 mm, with a laser power of 30%, an etching rate of 200, and etching for 10 times, so that a boss with a height of 0.05 mm can be obtained, i.e., the third-level boss 603.
[0068] In this embodiment, the chip device 5 includes a radio frequency power amplifier chip or a monolithic microwave integrated circuit, a single-layer ceramic capacitor, and a ceramic circuit chip. The thickness of the radio frequency power amplifier chip or the monolithic microwave integrated circuit is 0.1 mm, the thickness of the single-layer ceramic capacitor is 0.15 mm, and the thickness of the ceramic circuit chip is 0.25 mm.
[0069] In this embodiment, the positioning sheet 4 is cut by laser, and a device positioning groove 401 with ultra-small pitch can be obtained on the ceramic sheet; the pressing block 6 is processed by laser etching, and bosses of different heights and cavities of different depths can be accurately obtained. Moreover, laser processing is non-contact processing, which generates little stress and can process fine structures.
[0070] Embodiment 3
[0071] In order to use the fixture of the present invention more accurately and thus improve welding efficiency and welding accuracy, this embodiment uses the fixture in Embodiment 1 as an implementation object and provides a method for using the eutectic welding fixture for a power amplifier chip, including the following steps:
[0072] Step 1: Clean the preformed solder sheet 3 using plasma cleaning or isopropyl alcohol liquid;
[0073] Step 2: Place the power amplifier tube shell 2 inside the tube shell positioning groove 101 of the base 1, place the cleaned preformed solder sheet 3 inside the power amplifier tube shell 2, place the positioning sheet 4 on the preformed solder sheet 3, and install the pressing piece on the pressing installation hole 102, so that the pressing piece presses the positioning sheet 4 tightly on the preformed solder sheet 3;
[0074] Step 3: Place the chip devices 5 of different thicknesses in the device positioning grooves 401 of the positioning sheet 4 according to a predetermined layout, and confirm that they are correct;
[0075] Step 4: placing a pressing block 6 above the chip device 5, so that each boss on the lower surface of the pressing block 6 is aligned with and connected to the corresponding chip device 5; the chip device 5 includes an incontactable area such as an air bridge, so when the chip device 5 is pressed by the boss of the pressing block 6, the part where the boss and the chip device 5 are connected is the contactable area on the chip device 5;
[0076] Step 5: Place a counterweight block 7 on the upper surface of the pressing block 6, and use the counterweight block 7 to press the pressing block 6. The mass of the counterweight block 7 is calculated by multiplying the area of the device to be welded by 0.01g / mm 2 Make a selection;
[0077] Step 6: placing the eutectic fixture with the chip device 5 into the furnace chamber of the vacuum eutectic furnace;
[0078] Step 7: Setting a vacuum eutectic welding curve, and performing vacuum eutectic welding according to the set vacuum eutectic welding curve;
[0079] Step 8: Perform microscope inspection and X-ray penetration inspection on the power amplifier chip that has completed vacuum eutectic welding.
[0080] refer to Figure 8 The vacuum eutectic welding curve set in step 7 of this embodiment is as follows:
[0081] Before the vacuum eutectic furnace is heated up, the furnace cavity is flushed with nitrogen through two vacuum pumpings and nitrogen fillings to displace the air in the eutectic furnace cavity, reduce the oxygen content in the furnace, and obtain a furnace environment with a high-purity nitrogen atmosphere. Specifically, the first and second vacuum pumping times are both 50 seconds, and nitrogen is filled in between the two vacuum pumpings, so that the temperature in the furnace cavity is 25°C and the air pressure is a standard atmospheric pressure. The nitrogen filled is high-purity nitrogen with a purity of 99.999%. The filling time is 50 seconds and the flow rate is 7.5slm.
[0082] The temperature in the furnace chamber rises from 25°C to 200°C and is kept warm for 2 minutes. During this process, formic acid gas is continuously filled into the furnace chamber with a formic acid gas flow rate of 10-20slm. Filling with formic acid gas can reduce the oxide layer on the surface of the device to be welded to obtain a welding surface with better weldability, and 200°C is the appropriate temperature for the reduction reaction between formic acid gas and the oxide layer.
[0083] The temperature in the furnace chamber rises from 200°C to 240°C. During the heating process, vacuum is drawn to discharge the waste gas generated by the reduction reaction. When the temperature in the furnace chamber reaches 240°C, it is kept warm for 1 minute. During this insulation period, formic acid gas is filled into the furnace chamber again to flush the furnace chamber so that the waste gas in the furnace chamber can be discharged as much as possible.
[0084] The temperature in the furnace chamber rises from 240°C to 310°C. During the process of heating up to melt the solder, vacuuming begins when the temperature reaches 270°C to exhaust the gas inside the components to be welded and the solder to obtain solder joints that are almost void-free. After the temperature in the furnace chamber reaches 310°C, it is kept warm for 30S to achieve vacuum eutectic welding of the various welding components of the power amplifier chip.
[0085] After welding is completed, the temperature in the furnace chamber drops rapidly from 310°C to room temperature. During the cooling process, nitrogen is continuously filled in with a nitrogen flow rate of 30-60slm.
[0086] The above description is only a preferred embodiment of the present invention, which does not represent all possible forms of the present invention, and the protection scope of the present invention is not limited to such special statements and embodiments. According to the technical enlightenment disclosed by the present invention, various other modifications and improvements that do not deviate from the essence of the present invention are made, and these modifications and improvements are still within the protection scope of the present invention.
Claims
1. A fixture for eutectic welding of power amplifier chips, characterized in that: include: A base (1), a preformed welding sheet (3), a positioning sheet (4), a pressing block (6) and a counterweight block (7); The base (1) is provided with a tube shell positioning groove (101) for placing a chip device (5) and a power amplifier tube shell (2); the inner chamber of the power amplifier tube shell (2) is provided with a preformed solder sheet (3), a positioning sheet (4), a pressing block (6) and a counterweight block (7) from bottom to top; the positioning sheet (4) is provided with a device positioning groove (401); the chip device (5) is placed in the device positioning groove (401), and the same pressing block (6) is pressed on the upper surface of a plurality of the chip devices (5); the counterweight block (7) is located on the upper part of the pressing block (6); The lower surface of the pressing block (6) is provided with bosses of different heights; The base (1) is provided with a pressing installation hole (102), a pressing piece is arranged through the pressing installation hole (102), and a pressing end of the pressing piece is connected to the positioning piece (4).
2. The fixture for eutectic welding of power amplifier chips according to claim 1, characterized in that: The pressing member is a claw spring (103), and a U-shaped copper needle (104) is movably inserted into the claw spring (103).
3. The fixture for eutectic welding of power amplifier chips according to claim 2, characterized in that: The positioning piece (4) and the pressing block (6) are both made of ceramic material.
4. The fixture for eutectic welding of power amplifier chips according to claim 3, characterized in that: The base (1) is entirely made of high-purity graphite.
5. The fixture for eutectic welding of power amplifier chips according to claim 1, characterized in that: The bosses comprise a first-level boss (601), a second-level boss (602) and a third-level boss (603); the height of the first-level boss (601) is 0.2 mm, the height of the second-level boss (602) is 0.15 mm, and the height of the third-level boss (603) is 0.05 mm.
6. A method for processing a power amplifier chip eutectic welding fixture, using the fixture according to claim 4, comprising the following steps: S1: processing the preformed solder piece (3) according to the size of the power amplifier tube shell (2) in the tube shell positioning groove (101), so that the side edge of the preformed solder piece (3) is connected to the inner wall of the power amplifier tube shell (2); S2: making a ceramic sheet into a positioning sheet (4); firstly, processing a ceramic sheet of uniform thickness according to the length and width of the inner chamber of the power amplifier tube shell (2), so that the length and width of the ceramic sheet match the inner chamber of the power amplifier tube shell (2); then, processing a device positioning groove (401) on the ceramic sheet according to the layout requirements of the chip device (5), and the length and width of the device positioning groove (401) match the length and width of the preset chip device (5); the ceramic sheet is processed by laser cutting; S3: processing the outer dimensions of the pressing block (6) to be the same as those of the positioning sheet (4), and then processing bosses of different heights in sequence on the pressing block (6) by laser etching according to the device positioning groove (401) on the positioning sheet (4) and the layout of chip devices (5) of different thicknesses; Processing sequence: first form the highest boss, then continue etching some of the highest bosses to form bosses of the next level, and continue laser etching the bosses in descending order until all bosses of different heights are processed; S4: machining an avoidance groove (604) on the pressing block (6) and setting a placement area for the counterweight block (7); the position of the avoidance groove (604) is selected according to the position of the lower pressing member, and the placement area for the counterweight block (7) is located at the center of the pressing block (6).
7. The processing method of the power amplifier chip eutectic welding fixture according to claim 6, characterized in that: In step S2, a CAD plan is first produced according to the layout requirements of the chip device (5), and then the CAD plan is imported into the laser processing equipment, the parameters and focal length of the laser processing equipment are adjusted, and then the laser processing equipment cuts the ceramic sheet according to the CAD plan to form a positioning sheet (4).
8. A method for using a eutectic welding fixture for a power amplifier chip, using the fixture according to claim 4, comprising the following steps: Step 1: Clean the preformed solder sheet (3) using plasma cleaning or isopropyl alcohol liquid; Step 2: placing the power amplifier tube shell (2) inside the tube shell positioning groove (101) of the base (1), placing the cleaned preformed solder sheet (3) inside the power amplifier tube shell (2), placing the positioning sheet (4) on the preformed solder sheet (3), and installing a pressing piece on the pressing installation hole (102) so that the pressing piece presses the positioning sheet (4) tightly onto the preformed solder sheet (3); Step 3: placing chip devices (5) of different thicknesses in the device positioning grooves (401) of the positioning sheet (4) according to a predetermined layout, and confirming that they are correct; Step 4: placing a pressing block (6) above the chip device (5) so that each boss on the lower surface of the pressing block (6) is aligned with and connected to the corresponding chip device (5); the portion where the boss and the chip device (5) are connected is a contactable area on the chip device (5); Step 5: placing a counterweight (7) on the upper surface of the pressing block (6); Step 6: placing the eutectic fixture containing the chip device (5) into the furnace chamber of the vacuum eutectic furnace; Step 7: Setting a vacuum eutectic welding curve, and performing vacuum eutectic welding according to the set vacuum eutectic welding curve; Step 8: Perform microscope inspection and X-ray penetration inspection on the power amplifier chip that has completed vacuum eutectic welding.
9. The method for using the eutectic welding fixture for power amplifier chips according to claim 8, characterized in that: Vacuum eutectic welding curve in step 7: Before the vacuum eutectic furnace is heated up, the air in the eutectic furnace cavity is replaced by evacuating the cavity and filling the cavity with nitrogen twice, so that the temperature in the cavity is 25°C and the pressure is one standard atmospheric pressure. The temperature in the furnace chamber rises from 25°C to 200°C and is kept warm for 2 minutes. During this process, formic acid gas is continuously filled into the furnace chamber at a flow rate of 10-20slm. The temperature in the furnace chamber is raised from 200°C to 240°C. During the heating process, vacuum is drawn to discharge the reaction waste gas. When the temperature in the furnace chamber reaches 240°C, it is kept warm for 1 minute. During this warm-keeping period, formic acid gas is again filled into the furnace chamber to flush the furnace chamber. The temperature in the furnace chamber rises from 240°C to 310°C, and then starts to evacuate after reaching 270°C. After the temperature in the furnace chamber reaches 310°C, it is kept warm for 30 seconds to achieve vacuum eutectic welding of the power amplifier chip. The temperature in the furnace chamber quickly dropped from 310°C to room temperature, and nitrogen was continuously filled in during the cooling process with a nitrogen flow rate of 30-60slm.
Citation Information
Patent Citations
Welding positioning tool
CN116252087A
Chip eutectic soldering pressing block, positioning piece processing method and chip eutectic soldering method
CN118231273A