A welding method for high temperature stainless steel 316Ti

By using ER316Ti submerged arc welding wire and SJ601 flux for automatic submerged arc welding, the existing 318 welding materials cannot meet the problem of high-temperature stainless steel 316Ti welding, improve welding efficiency and quality, and enhance the high-temperature stability of the weld and Mechanical properties avoid cracks and pore defects, ensuring product performance under high temperature conditions.

CN118559162BActive Publication Date: 2024-11-19HIMILE MECHANICAL MFG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411034694.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing 318 welding materials cannot meet the automatic submerged arc welding requirements of stainless steel 316Ti for high temperatures. The welding efficiency is low, the working conditions are poor, and the chemical composition does not match the 316Ti, resulting in insufficient weld stability, corrosion resistance and mechanical properties, which are prone to occur. Cracked and air hole defects.

Method used

Automatic submerged arc welding of ER316Ti submerged arc welding wire and SJ601 flux are used for automatic submerged arc welding. ER316Ti welding wire contains 0.35-0.6% Ti, and SJ601 flux contains CaF2, CaO, MgO, SiO2 and other components, combined with specific welding process parameters, such as DCEN power supply electrode , proper welding current and voltage, welding speed is 400-550mm/min.

Benefits of technology

The welding efficiency of high-temperature stainless steel 316Ti has been greatly improved, the welding quality has been improved, the high-temperature stability, corrosion resistance and mechanical properties of the weld have been enhanced, cracks and pore defects are avoided, and the product has excellent performance in high-temperature working conditions after welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118559162B_ABST
    Figure CN118559162B_ABST
Patent Text Reader

Abstract

The present invention provides a welding method for high-temperature stainless steel 316Ti, and relates to the field of high-temperature stainless steel 316Ti welding. In the welding method for high-temperature stainless steel 316Ti, the high-temperature stainless steel 316Ti does not need to be preheated, and an ER316Ti submerged arc welding wire is used, and an SJ601 flux is matched to perform automatic submerged arc welding on the high-temperature stainless steel 316Ti; the ER316Ti submerged arc welding wire contains 0.35-0.6% Ti by mass. The welding method for high-temperature stainless steel 316Ti can overcome the problem that the chemical composition and welding performance of the existing 318 welding materials are not matched with the high-temperature stainless steel 316Ti, and under the condition of realizing automatic fine-wire submerged arc welding, the high-temperature stability, corrosion resistance and mechanical properties of the welding joint are improved, and defects such as cracks and pores are avoided in the weld, and the welding quality is improved while improving the welding efficiency for the high-temperature stainless steel 316Ti.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of high-temperature stainless steel 316Ti welding, in particular to a high-temperature stainless steel 316Ti welding method. Background Art

[0002] With the continuous development of science and technology, there are many high-temperature stainless steel 316Ti containers and other products that need to be welded. Since high-temperature stainless steel 316Ti contains trace elements Ti, the existing standards and the only welding materials recommended on the market are 318 welding materials. Nb in 318 welding materials is used to replace the Ti element in high-temperature stainless steel 316Ti.

[0003] However, the existing 318 welding materials are argon arc welding wires and electrodes, which cannot meet the requirements of automatic submerged arc welding. Only argon arc welding and electrode welding can be performed, and the welding efficiency is extremely low and the welding working conditions are poor. At the same time, the chemical composition and welding performance of the existing 318 welding materials do not match the high-temperature stainless steel 316Ti. The large heat input during welding will burn the Nb element in the 318 welding materials, which not only reduces the high-temperature stability, corrosion resistance and mechanical properties of the weld, but may also cause defects such as cracks and pores in the weld, resulting in poor welding quality, which seriously affects the working performance of the high-temperature stainless steel 316Ti products after welding in high-temperature conditions.

[0004] Therefore, the present invention provides a welding method for high-temperature stainless steel 316Ti, which can overcome the problem that the chemical composition and welding performance of the existing 318 welding materials are not matched with the high-temperature stainless steel 316Ti, and only argon arc welding and electrode welding can be performed. Under the condition of automatic fine-wire submerged arc welding for high-temperature stainless steel 316Ti, the high-temperature stability, corrosion resistance and mechanical properties of the welding joint are effectively improved, and defects such as cracks and pores are effectively avoided in the weld. While improving the welding quality, the welding efficiency for high-temperature stainless steel 316Ti is greatly improved, the welding labor intensity is reduced, and the product competitiveness is further improved, which has important technical significance. Summary of the invention

[0005] In order to solve the technical problems existing in the prior art, the present invention provides a welding method for high-temperature stainless steel 316Ti, which can overcome the problem that the chemical composition and welding performance of the existing 318 welding materials are not matched with the high-temperature stainless steel 316Ti, and only argon arc welding and electrode welding can be performed. Under the condition of automatic fine-wire submerged arc welding for high-temperature stainless steel 316Ti, the high-temperature stability, corrosion resistance and mechanical properties of the welding joint are effectively improved, and defects such as cracks and pores in the weld are effectively avoided. While improving the welding quality, the welding efficiency for high-temperature stainless steel 316Ti is greatly improved, the welding labor intensity is reduced, and the product competitiveness is further improved.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] A welding method for high temperature stainless steel 316Ti, wherein the high temperature stainless steel 316Ti does not need to be preheated, and an ER316Ti submerged arc welding wire is used, and an SJ601 flux is matched to perform automatic submerged arc welding on the high temperature stainless steel 316Ti;

[0008] The ER316Ti submerged arc welding wire contains Ti in an amount of 0.35-0.6% by mass.

[0009] Furthermore, the specific composition and weight percentage content of the ER316Ti submerged arc welding wire are: C≤0.08%, Cr 18-20%, Ni 11-14%, Mo 2-3%, Mn 1-2.5%, Si 0.3-0.65%, P≤0.03%, S≤0.03%, Cu≤0.75%, Ti0.35-0.6%, and the balance is Fe and unavoidable impurities.

[0010] Preferably, the diameter of the ER316Ti submerged arc welding wire is 1.6 mm or 2.0 mm.

[0011] Furthermore, the SJ601 flux contains the following components in weight percentage: S≤0.035%, P≤0.0004%, CaF2+CaO+MgO+MnO≥50%, SiO2≤20%, CaF2≥15%; other components in the SJ601 flux are not particularly limited and may be Al2O3 or coating.

[0012] Preferably, the particle size specification of the SJ601 flux is 10-60 mesh.

[0013] Preferably, in the automatic submerged arc welding, the groove form of the high temperature stainless steel 316Ti is one of the following: X-shaped symmetrical double-sided groove, V-shaped single-sided groove.

[0014] More preferably, the inclination angle of the X-shaped symmetrical double-sided groove is 50-60°.

[0015] More preferably, the inclination angle of the V-shaped single-sided groove is 40-50°.

[0016] Furthermore, in the automatic submerged arc welding, the control power polarity is DCEN, the base welding current is 180-260A, the base welding voltage is 23-28V, the filling cover current is 240-350A, and the filling cover voltage is 28-31V.

[0017] Furthermore, in the automatic submerged arc welding, the automatic welding speed is controlled to be 400-550 mm / min.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1) The welding method of high-temperature stainless steel 316Ti of the present invention breaks the conventional welding method that 316Ti can only be welded by manual argon arc welding, and the welding rod welding material can only be 318 welding materials; a specific ER316Ti submerged arc welding wire with a diameter of 1.6mm / 2.0mm is used, matched with SJ601 flux, and through a specific welding method and welding process parameter combination, it can overcome the problem that the chemical composition and welding performance of the existing 318 welding material do not match the high-temperature stainless steel 316Ti, and only argon arc welding and welding rod welding can be performed, and automatic fine wire submerged arc welding of high-temperature stainless steel 316Ti is effectively realized, and no preheating is required before welding, which greatly improves the welding efficiency of high-temperature stainless steel 316Ti, reduces the welding labor intensity, and further improves the product competitiveness.

[0020] 2) The welding method of high temperature stainless steel 316Ti of the present invention effectively avoids the burning of trace elements in large heat input by adopting a specific ER316Ti submerged arc welding wire. In the automatic fine wire submerged arc welding of high temperature stainless steel 316Ti, the high temperature stability, corrosion resistance and mechanical properties of the welded joint are effectively improved, and defects such as cracks and pores are effectively avoided in the weld, thereby further improving the welding quality and ensuring the working performance of the high temperature stainless steel 316Ti products in high temperature conditions after welding.

[0021] 3) After the automatic fine-wire submerged arc welding is performed using the welding method of the high-temperature stainless steel 316Ti of the present invention, the welds are 100% qualified by non-destructive testing (100% RT); the tensile strength exceeds 570Mpa, the yield strength exceeds 360MPa, and the impact performance at -196℃ can reach 75J / cm 2 ; The 180° bending test showed no defects and passed the test; the chemical composition and content of the weld met the requirements of 316Ti material (ASTM A240 316Ti); the intergranular corrosion test was conducted according to the test E method in ASTM A262, copper-copper sulfate-16% sulfuric acid, boiling for 24 hours, with no defects and passed the test. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of the welding joint form and welding groove of Example 1. DETAILED DESCRIPTION

[0023] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0024] Example 1

[0025] This embodiment provides a welding method for high temperature stainless steel 316Ti, specifically:

[0026] like Figure 1 As shown in the figure, a 15mm thick high temperature stainless steel 316Ti plate is welded, the groove form is an X-shaped symmetrical double-sided groove (groove inclination angle 60°), and the blunt edge 2mm is paired without leaving a gap; the high temperature stainless steel 316Ti plate does not need to be preheated, and an ER316Ti submerged arc welding wire with a specific composition and content of 2.0mm in diameter is used, matched with SJ601 flux, to perform automatic submerged arc welding on the high temperature stainless steel 316Ti plate.

[0027] During the automatic submerged arc welding process, the control power polarity is DCEN, the base welding current is 240A, the base welding voltage is 28V, the filling and covering current is 320A, the filling and covering voltage is 30V, and the welding speed is 450mm / min.

[0028] The specific composition and weight percentage of the ER316Ti submerged arc welding wire are as follows:

[0029]

[0030] The particle size specification of the SJ601 flux is 20 mesh; the SJ601 flux contains the following components in weight percentage:

[0031]

[0032] The welding method of high temperature stainless steel 316Ti described above in this embodiment was used to perform automatic submerged arc welding, and two sets of parallel tests were set for welding the same test plate. The test data results were as follows: 100% non-destructive testing (100% RT) of the welds was qualified; the chemical composition of the welds met the requirements of 316Ti material; the tensile performance test, 180° bending performance test, impact performance test, and intergranular corrosion test all met the standard requirements.

[0033] The specific composition and weight percentage of the weld (cladding metal) are as follows:

[0034]

[0035] The mechanical properties and intergranular corrosion test results of the weld (cladding metal) are shown below:

[0036]

[0037] Example 2

[0038] The welding method of high temperature stainless steel 316Ti of Example 1 is adopted, and the ER316Ti submerged arc welding wire, SJ601 flux and the same welding process parameters are maintained with the same composition and content, and automatic submerged arc welding is performed on high temperature stainless steel 316Ti plates with different groove forms and different thicknesses in the following schemes 1 to 5.

[0039] The specific groove forms and thickness specifications of Schemes 1 to 5 are as follows:

[0040] Solution 1: X-symmetric double-sided 50° groove, plate thickness 10mm;

[0041] Option 2: X-symmetric double-sided 60° groove, plate thickness 15mm;

[0042] Option 3: V-shaped single-sided 50° groove, plate thickness 10mm;

[0043] Option 4: V-shaped single-sided 55° groove, plate thickness 15mm;

[0044] Option 5: X-symmetrical double-sided 60° groove, plate thickness 20mm.

[0045] After welding, the welds of Schemes 1 to 5 were subjected to 100% nondestructive testing, tensile test, 180° bending test, impact test, and intergranular corrosion test, and the chemical composition and content of each weld were tested to see if they met the requirements of 316Ti material. The specific results are shown below:

[0046]

[0047] It can be seen from Examples 1-2 that the welding method of the high temperature stainless steel 316Ti of the present invention is adopted. After automatic submerged arc welding, the 100% non-destructive testing (100% RT) of each weld is qualified, the tensile strength is ≥515Mpa, the yield strength is ≥205Mpa; the 180° bending test is defect-free and the test is qualified; the -196°C impact performance is ≥27J / cm 2 ; The chemical composition and content of each weld meet the requirements of 316Ti material (ASTM A240 316Ti); the intergranular corrosion test is in accordance with the test E method in ASTM A262, copper-copper sulfate-16% sulfuric acid, boiling for 24 hours, no defects, and the test is qualified. The welding method of high-temperature stainless steel 316Ti can overcome the problem that the chemical composition and welding performance of the existing 318 welding materials are not matched with high-temperature stainless steel 316Ti, and only argon arc welding and electrode welding can be performed, and automatic fine wire submerged arc welding for high-temperature stainless steel 316Ti is effectively realized, and no preheating is required before welding, which greatly improves the welding efficiency of high-temperature stainless steel 316Ti and reduces the labor intensity of welding.

[0048] Example 3

[0049] This embodiment provides a welding method for high temperature stainless steel 316Ti, specifically:

[0050] The high-temperature stainless steel 316Ti plate with a thickness of 15mm is welded. The groove form is an X-shaped symmetrical double-sided groove (groove inclination angle 60°), and the blunt edge 2mm is paired without leaving a gap; the high-temperature stainless steel 316Ti plate does not need to be preheated. A specific ER316Ti submerged arc welding wire with a diameter of 2.0mm is used, matched with SJ601 flux, to perform automatic submerged arc welding on the high-temperature stainless steel 316Ti plate.

[0051] During the automatic submerged arc welding process, the control power polarity is DCEN, the base welding current is 200A, the base welding voltage is 25V, the filling cover current is 280A, the filling cover voltage is 30V, and the welding speed is 500mm / min.

[0052] The specific composition and weight percentage of the ER316Ti submerged arc welding wire are as follows:

[0053]

[0054] The specifications of the SJ601 flux and the contents of its components are the same as those in Example 1.

[0055] The welding method of high temperature stainless steel 316Ti described above in this embodiment was used to perform automatic submerged arc welding, and two sets of parallel tests were set for welding the same test plate. The test data results were as follows: 100% non-destructive testing (100% RT) of the welds was qualified; the chemical composition of the welds met the requirements of 316Ti material; the tensile performance test, 180° bending performance test, impact performance test, and intergranular corrosion test all met the standard requirements.

[0056] The specific composition and weight percentage of the weld (cladding metal) are as follows:

[0057]

[0058] The mechanical properties and intergranular corrosion test results of the weld (cladding metal) are shown below:

[0059]

[0060] Example 4

[0061] This embodiment provides a welding method for high temperature stainless steel 316Ti, specifically:

[0062] The high-temperature stainless steel 316Ti plate with a thickness of 15mm was welded, and the groove form was an X-shaped symmetrical double-sided groove (groove inclination angle of 60°), and the blunt edge 2mm was paired without leaving a gap; the high-temperature stainless steel 316Ti plate did not need to be preheated, and a specific ER316Ti submerged arc welding wire with a diameter of 2.0mm was used, matched with SJ601 flux, and automatic submerged arc welding was performed on the high-temperature stainless steel 316Ti plate; during the automatic submerged arc welding process, the power supply polarity was controlled to DCEN, the base welding current was 200A, the base welding voltage was 25V, the filling and covering current was 280A, the filling and covering voltage was 30V, and the welding speed was 500mm / min.

[0063] The specific composition and weight percentage of the ER316Ti submerged arc welding wire are as follows:

[0064]

[0065] The specifications of the SJ601 flux and the contents of its components are the same as those in Example 1.

[0066] The welding method of high temperature stainless steel 316Ti described above in this embodiment was used to perform automatic submerged arc welding, and two sets of parallel tests were set for welding the same test plate. The test data results were as follows: 100% non-destructive testing (100% RT) of the welds was qualified; the chemical composition of the welds met the requirements of 316Ti material; the tensile performance test, 180° bending performance test, impact performance test, and intergranular corrosion test all met the standard requirements.

[0067] The specific composition and weight percentage of the weld (cladding metal) are as follows:

[0068]

[0069] The mechanical properties and intergranular corrosion test results of the weld (cladding metal) are shown below:

[0070]

[0071] It can be seen that the welding method of high temperature stainless steel 316Ti of the present invention, by adopting ER316Ti submerged arc welding wire with specific composition and content, matching SJ601 flux, and matching through specific welding methods and welding process parameters, can overcome the problem that the chemical composition and welding performance of the existing 318 welding materials are not matched with high temperature stainless steel 316Ti, and can only be used for argon arc welding and welding rod welding, and effectively realize automatic fine wire submerged arc welding for high temperature stainless steel 316Ti, without preheating before welding, greatly improve the welding efficiency for high temperature stainless steel 316Ti, reduce welding labor intensity, and further improve product competitiveness. At the same time, it effectively avoids the burning of trace elements in large heat input, effectively improves the high temperature stability, corrosion resistance and mechanical properties of the welding joint in the automatic fine wire submerged arc welding for high temperature stainless steel 316Ti, effectively avoids defects such as cracks and pores in the weld, further improves the welding quality, and ensures the working performance of high temperature stainless steel 316Ti products in high temperature conditions after welding. After automatic fine-wire submerged arc welding, the welds are 100% qualified by non-destructive testing (100% RT); the tensile strength exceeds 570Mpa, the yield strength exceeds 360MPa, and the impact performance at -196℃ can reach 75J / cm 2 ; The 180° bending test showed no defects and passed the test; the chemical composition and content of the weld met the requirements of 316Ti material (ASTM A240 316Ti); the intergranular corrosion test was conducted according to the test E method in ASTM A262, copper-copper sulfate-16% sulfuric acid, boiling for 24 hours, with no defects and passed the test.

[0072] Unless otherwise specified, all percentages used in the present invention are by mass.

[0073] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A welding method for high temperature stainless steel 316Ti, characterized in that: High temperature stainless steel 316Ti does not need to be preheated. ER316Ti submerged arc welding wire is used, matched with SJ601 flux, to perform automatic submerged arc welding on high temperature stainless steel 316Ti; The specific composition and weight percentage content of the ER316Ti submerged arc welding wire are: C≤0.08%, Cr 18-20%, Ni11-14%, Mo 2-3%, Mn 1-2.5%, Si 0.3-0.65%, P≤0.03%, S≤0.03%, Cu≤0.75%, Ti 0.35-0.6%, and the balance is Fe and unavoidable impurities; The SJ601 flux contains the following components in weight percentage: S≤0.035%, P≤0.0004%, CaF2+CaO+MgO+MnO≥50%, SiO2≤20%, CaF2≥15%; In the automatic submerged arc welding, the control power polarity is DCEN, the base welding current is 180-260A, the base welding voltage is 23-28V, the filling cover current is 240-350A, and the filling cover voltage is 28-31V.

2. The welding method of high temperature stainless steel 316Ti according to claim 1, characterized in that: The diameter of the ER316Ti submerged arc welding wire is 1.6 mm or 2.0 mm.

3. The welding method of high temperature stainless steel 316Ti according to claim 1, characterized in that: The particle size specification of the SJ601 flux is 10-60 mesh.

4. The welding method of high temperature stainless steel 316Ti according to claim 1, characterized in that: In the automatic submerged arc welding, the groove form of the high temperature stainless steel 316Ti is one of the following: an X-shaped symmetrical double-sided groove and a V-shaped single-sided groove.

5. The welding method of high temperature stainless steel 316Ti according to claim 4, characterized in that: The inclination angle of the X-shaped symmetrical double-sided groove is 50-60°.

6. The welding method of high temperature stainless steel 316Ti according to claim 4, characterized in that: The inclination angle of the V-shaped single-sided groove is 40-50°.

7. The welding method of high temperature stainless steel 316Ti according to claim 1, characterized in that: In the automatic submerged arc welding, the automatic welding speed is controlled to be 400-550 mm / min.