A method for preparing unfired dry granules, unfired dry granule ceramic brick and preparation method thereof
By using fire-free dry particles instead of the dry particles of frit and setting them under the inkjet pattern layer, combined with inkjet printing technology, the pattern clarity problem caused by the smooth surface of the dry particles of frit is solved, and the mold convex effect of ceramic tiles is achieved and pattern clarity improvement.
Patent Information
- Application Number
- CN202411019036.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-29
AI Technical Summary
In the existing glue positioning dry particle process, the surface of the frit dry particle is smooth and difficult to adsorb ceramic ink, resulting in poor pattern clarity, especially on dark patterns.
Use non-fired dry particles to replace conventional frit dry particles. Use spray drying technology to prepare non-fired dry particles composed of minerals such as potassium feldspar, sodium feldspar, kaolin, etc., and set them under the inkjet pattern layer to combine inkjet. Printing technology forms ceramic tiles with concave and convex effects and excellent pattern clarity.
The mold concave and convex effect and pattern clarity of ceramic tiles are improved, preventing the influence of dry particles on the pattern and obtaining excellent pattern clarity.
Smart Images

Figure CN118561519B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing unfired dry particles, an unfired dry particle ceramic tile and a preparation method thereof, and belongs to the technical field of ceramic tile production and manufacturing. Background Art
[0002] The glue positioning dry particle process combines digital inkjet printing glue technology with dry particle spreading technology, and utilizes the organic fusion of digital inkjet and glue combined with dry particle spreading technology to produce ceramic products with a certain mold effect and dry particle texture. At present, the glue positioning dry particles usually use frit dry particles. Because the surface of frit dry particles is relatively smooth and difficult to absorb ceramic ink, building ceramic companies currently usually set the frit dry particles above the inkjet pattern layer to avoid the inkjet pattern being printed on the frit dry particles and affecting the clarity of the pattern. The glue positioning dry particle products on the market are generally matte products, so the frit dry particles used are usually matte dry particles with poor transparency. Especially when the dry particles are positioned and applied to dark patterns, the pattern is relatively blurred, which greatly affects the clarity of the brick surface pattern. Summary of the invention
[0003] In response to the problems raised in the background technology, the present invention provides a method for preparing unfired dry particles, an unfired dry particle ceramic tile and a preparation method thereof. By using unfired dry particles to replace conventional frit dry particles, the unfired dry particles can be arranged under the inkjet pattern layer, and an unfired dry particle ceramic tile having both a concave-convex effect and excellent pattern clarity can be obtained.
[0004] In a first aspect, the present invention provides a method for preparing unfired dry granules. The mineral composition of the unfired dry granules includes: by mass percentage, 10-40% potassium feldspar, 25-55% sodium feldspar, 20-30% kaolin, 5-10% quartz powder, and 5-15% calcite; weigh each raw material according to the mineral composition of the unfired dry granules, add water and additives, mix evenly to form a glaze slurry, spray dry the glaze slurry to granulate, and obtain the unfired dry granules.
[0005] Preferably, the chemical composition of the unburned dry particles includes, by mass percentage, SiO2: 55~70%; Al2O3: 18~26%; Fe2O3: 0.1~0.3%; TiO2: 0.1~0.2%; MgO: 0.1~0.5%; CaO: 2~9%; K2O: 1~5%; Na2O: 4~6%; and loss on ignition: 4~10%.
[0006] Preferably, the particle size of the non-fired dry particles is 60-150 meshes.
[0007] In a second aspect, the present invention provides an unfired dry granule ceramic tile. The unfired dry granule ceramic tile comprises: a body layer, a top glaze layer and an unfired dry granule layer with adjustable order, an inkjet pattern layer, and a protective glaze layer; wherein the unfired dry granule layer is formed by the unfired dry granules prepared by the above-mentioned preparation method.
[0008] In the third aspect, the present invention provides a method for preparing glue-positioned dry-granule ceramic tiles. The preparation method comprises: applying a glaze on the surface of the blank; inkjet printing a glue pattern on the surface of the blank after the glaze is applied; applying the unfired dry granules formed by the preparation method on the surface of the blank after the glue pattern is inkjet printed; inkjet printing a common ink pattern on the surface of the blank after the unfired dry granules are applied; applying a protective glaze on the surface of the blank after the common ink pattern is inkjet printed; firing and polishing the blank after the protective glaze is applied to obtain the unfired dry-granule ceramic tiles; or, the preparation method comprises: inkjet printing a glue pattern on the surface of the blank; applying the unfired dry granules formed by the preparation method on the surface of the blank after the glue pattern is inkjet printed; applying a glaze on the surface of the blank after the unfired dry granules are applied; inkjet printing a common ink pattern on the surface of the blank after the glaze is applied; applying a protective glaze on the surface of the blank after the common ink pattern is inkjet printed; firing and polishing the blank after the protective glaze is applied to obtain the unfired dry-granule ceramic tiles.
[0009] Preferably, the chemical composition of the glaze includes, by mass percentage, SiO2: 60~70%, Al2O3: 12~25%, Fe2O3: 0.1~0.5%, TiO2: 0.1~0.5%, CaO: 0.1~0.5%, MgO: 1~5%, K2O: 2~5%, Na2O: 2~5%, ZrO2: 3~10%, and loss on ignition: 1~3%.
[0010] Preferably, the mineral composition of the glaze includes, by mass percentage, 28-35% potassium feldspar, 15-21% sodium feldspar, 12-18% kaolin, 12-18% quartz sand, 8-12% zirconium silicate, 3-5% aluminum oxide, 2-4% calcined talc, and 3-8% calcined kaolin.
[0011] Preferably, the glaze is applied by spraying or pouring; the specific gravity of the glaze is 1.40-1.50 g / cm 3 , glaze application amount is 450~650g / m 2 .
[0012] Preferably, the amount of the unburned dry particles applied is 50-200 g / m 2 .
[0013] Preferably, the chemical composition of the protective glaze includes, by mass percentage, SiO2: 45~55%; Al2O3: 17~24%; MgO: 1~3%; CaO: 2~6%; BaO: 3~8%; ZnO: 2.5~5%; K2O: 1~3%; Na2O: 3.5~5%; loss on ignition: 4~9%.
[0014] Preferably, the mineral composition of the protective glaze includes, by mass percentage, 10-20% potassium feldspar, 35-45% sodium feldspar, 10-20% kaolin, 3-5% zinc oxide, 5-10% calcite, 3-6% talc, 5-10% barium carbonate, 2-4% aluminum oxide, and 3-6% calcined kaolin.
[0015] Preferably, the protective glaze is applied by spraying; the specific gravity of the protective glaze is 1.35-1.40 g / cm 3 , glaze application amount is 250~300 g / m 2 .
[0016] Preferably, the firing temperature is 1180-1200° C., and the firing period is 60-80 minutes.
[0017] Beneficial Effects
[0018] The present invention uses unfired dry particles for the first time, and by using unfired dry particles to replace conventional frit dry particles, ceramic tiles with a mold convex and concave effect are obtained. In addition, the present invention arranges the unfired dry particles in the lower layer of the inkjet pattern layer, which can prevent the dry particles from affecting the pattern clarity, thereby obtaining unfired dry particle ceramic tiles with excellent pattern clarity. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is the optical effect diagram of the unburned dry granules;
[0020] Figure 2 This is a brick surface effect diagram of Example 1;
[0021] Figure 3 This is a brick surface effect diagram of Example 2;
[0022] Figure 4 This is the optical effect picture of the frit dry particles;
[0023] Figure 5 This is the brick surface effect diagram of Example 1;
[0024] Figure 6 This is the brick surface effect diagram of Example 2;
[0025] Figure 7 This is the brick surface effect diagram of Example 3;
[0026] Figure 8This is the brick surface effect diagram of Example 4. DETAILED DESCRIPTION
[0027] The present invention is further described by the following embodiments, and it should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention. The following is an exemplary description of the unfired dry granules, unfired dry granule ceramic tiles and their preparation methods according to the present invention.
[0028] The green body powder is pressed and formed to obtain a green body. The green body powder commonly used in the art can be used. For example, but not limited to, the chemical composition of the green body powder includes: in mass percentage, SiO2: 60-70%, Al2O3: 19-25%, Fe2O3: 0.5-1.5%, TiO2: 0.2-0.5%, CaO: 0.2-0.8%, MgO: 0.3-0.8%, K2O: 2.0-4.0%, Na2O: 1.5-3.5%, and loss on ignition: 4.0-6.0%.
[0029] The pressing machine can be used for pressing. The molding method includes but is not limited to dry pressing.
[0030] The green body is dried. The moisture content of the green body after drying can be controlled within 0.2-0.5wt%. The drying temperature can be 110-130°C. The drying time can be 0.5-1.5 hours.
[0031] Apply glaze on the surface of the blank. The function of the glaze is to cover the base color and defects of the blank and promote the color development of the inkjet pattern.
[0032] In some embodiments, the chemical composition of the glaze includes, by mass percentage, SiO2: 60~70%, Al2O3: 12~25%, Fe2O3: 0.1~0.5%, TiO2: 0.1~0.5%, CaO: 0.1~0.5%, MgO: 1~5%, K2O: 2~5%, Na2O: 2~5%, ZrO2: 3~10%, and loss on ignition: 1~3%.
[0033] As an example, the mineral composition of the glaze includes, by mass percentage, potassium feldspar: 28~35%, sodium feldspar: 15~21%, kaolin 12~18%, quartz sand 12~18%, zirconium silicate 8~12%, aluminum oxide 1~5%, calcined talc 2~4%, and calcined kaolin 3~8%.
[0034] Prepare glaze slurry. The raw material composition of the glaze slurry includes glaze mineral composition, sodium tripolyphosphate, sodium carboxymethyl cellulose and water. In some embodiments, the mass ratio of the glaze mineral composition and water of the glaze slurry is 50~80:20~50. For example, sodium tripolyphosphate accounts for 0.1~0.5% of the total mass of the glaze mineral composition and water. For example, sodium carboxymethyl cellulose accounts for 0.1~0.5% of the total mass of the glaze mineral composition and water. Weigh each raw material according to the raw material composition of the glaze slurry, and ball mill evenly until the glaze slurry passes through a 325 mesh sieve and the residue is ≤0.8wt%. When in use, water can be added to the above-mentioned glaze slurry to adjust the final desired glaze specific gravity.
[0035] The glaze is applied by spraying or pouring. Preferably, the glaze is applied by spraying. In some embodiments, the specific gravity of the glaze is 1.40-1.50 g / cm 3 , glaze application amount is 450~650 g / m 2 .
[0036] The glue pattern is printed on the surface of the body after the glaze is applied. The glue pattern can be printed by double-channel inkjet printing. Preferably, the amount of glue applied is less than 110 g / m 2 .
[0037] After the glue pattern is inkjet printed, the surface of the blank is covered with unfired dry particles, wherein the mineral composition of the unfired dry particles includes, by mass percentage, 10-40% potassium feldspar, 25-55% sodium feldspar, 20-30% kaolin, 5-10% quartz powder, and 5-15% calcite.
[0038] In some embodiments, the chemical composition of the unburned dry particles includes, by mass percentage, SiO2: 55~70%; Al2O3: 18~26%; Fe2O3: 0.1~0.3%; TiO2: 0.1~0.2%; MgO: 0.1~0.5%; CaO: 2~9%; K2O: 1~5%; Na2O: 4~6%; and loss on ignition: 4~10%.
[0039] Prepare the unfired dry granules. Weigh the raw materials according to the mineral composition of the unfired dry granules, add water and additives, mix evenly, prepare glaze slurry, spray dry granulate, and obtain unfired dry granules. The additives include but are not limited to sodium tripolyphosphate and sodium carboxymethyl cellulose.
[0040] In some embodiments, the mass ratio of the unfired dry particle mineral composition and water of the unfired dry particle glaze slurry is 60~70:30~40. For example, sodium tripolyphosphate accounts for 0.2~0.25% of the total mass of the unfired dry particle mineral composition and water. For example, sodium carboxymethyl cellulose accounts for 0.15~0.25% of the total mass of the unfired dry particle mineral composition and water. According to the raw material composition of the unfired dry particle glaze slurry, each raw material is weighed and ball-milled evenly until the glaze slurry passes through a 325-mesh sieve and the residue is ≤0.8wt%, thereby obtaining the unfired dry particle glaze slurry. The glaze slurry is sent to a spray drying tower for granulation. The glaze slurry is atomized by controlling the spray gun pressure, and a large amount of water evaporates at high temperature to obtain spherical dry particles. The particle size of the dry particles can be controlled by adjusting the spray gun pressure. The greater the spray gun pressure, the smaller the particle size of the dry particles. The water content of the dry particles can be controlled by adjusting the temperature of the spray tower. The lower the moisture content of the dry particles, the higher the strength. As an example, the moisture content of the unfired dry particles is controlled below 3wt%. The moisture content of the dry granules is too high, and the dry granules are easy to break, which is not conducive to reuse.
[0041] The present invention prepares the unburned dry granules by spray granulation. In the granulation process, the slurry is sprayed out under high pressure, and the slurry is in the form of spherical droplets. Then, under high temperature conditions, the water in the droplets evaporates quickly to form spherical particles. There are holes in the particles left after the water evaporates, so the surface of the unburned dry granules has certain capillary holes.
[0042] The inventors have also tried other granulation methods. For example, the dry particles are weighed according to the formula components and then ball-milled into a slurry, and then directly dried and crushed into granules. However, the particles obtained by this method have low strength, and after a single use, most of the dry particles become fine powder, which cannot be recycled even if they are recovered.
[0043] After applying the unburned dry granules, a fan is used to remove the unadhered dry granules and recycle them. The application amount of the unburned dry granules can be 50-200 g / m 2 If the amount of unfired dry granules applied is too small, the concave and convex mold effect on the brick surface is not obvious. If the amount of unfired dry granules applied is too large, glaze cracks are likely to occur during the kiln drying process.
[0044] The particle size of the unfired dry granules can be 60~150 mesh. The unfired dry granules are coarse, and the glaze surface presents an abrupt visual effect, resulting in unsightly decoration. The unfired dry granules are fine, and the dry granules are difficult to adhere to the brick surface, and a large number of them are aggregated into agglomerates, the mold effect of the brick surface is poor, and the pattern presentation is not ideal.
[0045] After applying the unfired dry particles, a common ink pattern is printed on the surface of the blank by inkjet printing. The color and texture of the common ink pattern printed by inkjet printing can be adaptively changed according to the needs.
[0046] A protective glaze is applied to the surface of the blank after the inkjet printing of the ordinary ink pattern. The conventional protective glaze in the art can be used.
[0047] In some embodiments, the chemical composition of the protective glaze includes, by mass percentage, SiO2: 45~55%; Al2O3: 17~24%; MgO: 1~3%; CaO: 2~6%; BaO: 3~8%; ZnO: 2.5~5%; K2O: 1~3%; Na2O: 3.5~5%; loss on ignition: 4~9%.
[0048] As an example, the mineral composition of the protective glaze includes, by mass percentage, potassium feldspar: 10~20%, sodium feldspar 35~45%, kaolin 10~20%, zinc oxide 3~5%, calcite 5~10%, talc 3~6%, barium carbonate 5~10%, aluminum oxide 2~4%, and calcined kaolin 3~6%.
[0049] The protective glaze is applied by spraying. The specific gravity of the protective glaze is 1.35-1.40 g / cm 3 , glaze application amount is 250~300 g / m 2 .
[0050] Prepare protective glaze slurry. The raw material composition of the protective glaze slurry includes protective glaze mineral composition, sodium tripolyphosphate, sodium carboxymethyl cellulose and water. In some embodiments, the mass ratio of the protective glaze mineral composition and water of the protective glaze slurry is 65~70:30~35. For example, sodium tripolyphosphate accounts for 0.2~0.25% of the total mass of the protective glaze mineral composition and water. For example, sodium carboxymethyl cellulose accounts for 0.15~0.25% of the total mass of the protective glaze mineral composition and water. Weigh each raw material according to the raw material composition of the protective glaze slurry, and ball mill evenly until the glaze slurry passes through a 325 mesh sieve and the residue is ≤0.5wt%. When in use, water can be added to the above-mentioned protective glaze slurry to adjust the final required specific gravity of the protective glaze.
[0051] The green body with the protective glaze applied is fired. It can be fired in a kiln. The firing temperature can be 1180~1200℃, and the firing cycle can be 60~80 minutes.
[0052] As an alternative technical solution, the order of applying the glaze and the glue-positioned unfired dry particles can be adjusted. For example, a glue pattern is inkjet printed on the surface of the dried green body, the unfired dry particles are applied on the green body surface after the glue pattern is inkjet printed, and then the glaze is applied on the green body surface after the unfired dry particles are applied. Finally, a normal ink pattern is inkjet printed on the green body surface after the glaze is applied, and a protective glaze is applied on the green body surface after the normal ink pattern is inkjet printed, and the green body after the protective glaze is fired and polished to obtain the unfired dry particle ceramic tile.
[0053] The unfired dry granular ceramic tiles can also be edged, graded, waxed, packaged and stored.
[0054] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0055] Example 1
[0056] The method for preparing the unfired dry granular ceramic brick comprises the following steps:
[0057] Step 1. Apply glaze on the surface of the dried body. The chemical composition of the glaze includes: by mass percentage, SiO2: 65.63%, Al2O3: 18.00%, Fe2O3: 0.15%, TiO2: 0.14%, CaO: 0.27%, MgO: 1.09%, K2O: 3.51%, Na2O: 3.04%, ZrO2: 6.37%, loss on ignition: 1.8%. The glaze is applied by spraying. The specific gravity of the glaze is 1.45g / cm 3 , glaze amount 500 g / m 2 .
[0058] Step 2. Inkjet print a glue pattern on the surface of the glazed body.
[0059] Step 3. Apply unburned dry particles on the surface of the blank after the glue pattern is inkjet printed. The mineral composition of the unburned dry particles includes: by mass percentage, 20% potassium feldspar, 40% sodium feldspar, 25% kaolin, 10% quartz powder, and 5% calcite. The chemical composition of the unburned dry particles includes: by mass percentage, SiO2: 65.3%; Al2O3: 19.01%; Fe2O3: 0.15%; TiO2: 0.13%; MgO: 0.24%; CaO: 2.96%; K2O: 2.71%; Na2O: 4.55%; ignition loss: 4.95%. The application amount of the unburned dry particles is 80g / m 2 .
[0060] Step 4. Inkjet printing a common ink pattern on the surface of the green body after applying the unfired dry particles.
[0061] Step 5. Apply protective glaze on the surface of the body after the ordinary ink pattern is inkjet printed. The mineral composition of the protective glaze includes: in mass percentage, potassium feldspar: 15%, sodium feldspar 40%, kaolin 15%, zinc oxide 3%, calcite 6%, calcite 4%, barium carbonate 9%, aluminum oxide 3%, calcined kaolin 5%. The chemical composition of the protective glaze includes: in mass percentage, SiO2: 52.49%; Al2O3: 19.86%; MgO: 1.54%; CaO: 3.46%; BaO: 7.01%; ZnO: 2.98%; K2O: 1.96%; Na2O: 4.36%; loss on ignition: 6.34%. The protective glaze is applied by spraying. The specific gravity of the protective glaze is 1.35 g / cm 3 , glaze application amount is 280 g / m 2 .
[0062] Step 6. The green body with the protective glaze applied is fired and polished to obtain the unfired dry-grain ceramic tile. The firing temperature is 1190° C. and the firing cycle is 70 minutes.
[0063] Figure 1 This is an optical effect picture of unfired dry granules. It can be seen that most of the dry granules are spherical, have not been fired, and have a rough surface.
[0064] Figure 2 This is the brick surface effect diagram of Example 1. Since the surface of the unfired dry particles has certain capillary holes, the ink forming the inkjet pattern is printed on the unfired dry particles, and the ink can quickly penetrate into the capillary holes of the unfired dry particles, which is convenient for the rapid drying of the ink and will not affect the clarity of the inkjet pattern. Therefore, this Example 1 uses unfired dry particles to replace conventional frit dry particles, and the unfired dry particles can be arranged below the inkjet pattern layer to obtain unfired dry particle ceramic tiles with obvious granularity, concave-convex effect and excellent pattern clarity.
[0065] Example 2
[0066] The method for preparing the unfired dry granular ceramic brick comprises the following steps:
[0067] Step 1. Inkjet print glue pattern on the surface of the dried blank.
[0068] Step 2. Apply unburned dry particles on the surface of the blank after the glue pattern is inkjet printed. The mineral composition of the unburned dry particles includes: by mass percentage, 20% potassium feldspar, 40% sodium feldspar, 25% kaolin, 10% quartz powder, and 5% calcite. The chemical composition of the unburned dry particles includes: by mass percentage, SiO2: 65.3%; Al2O3: 19.01%; Fe2O3: 0.15%; TiO2: 0.13%; MgO: 0.24%; CaO: 2.96%; K2O: 2.71%; Na2O: 4.55%; ignition loss: 4.95%. The application amount of the unburned dry particles is 80g / m 2 .
[0069] Step 3. Apply glaze on the surface of the green body after applying the unfired dry particles. The chemical composition of the glaze includes: by mass percentage, SiO2: 65.63%, Al2O3: 18.00%, Fe2O3: 0.15%, TiO2: 0.14%, CaO: 0.27%, MgO: 1.09%, K2O: 3.51%, Na2O: 3.04%, ZrO2: 6.37%, loss on ignition: 1.8%. The glaze is applied by spraying. The specific gravity of the glaze is 1.45g / cm 3 , glaze amount 500 g / m 2 .
[0070] Step 4. Inkjet print a normal ink pattern on the surface of the glazed body.
[0071] Step 5. Apply protective glaze on the surface of the body after the ordinary ink pattern is inkjet printed. The mineral composition of the protective glaze includes: in mass percentage, potassium feldspar: 15%, sodium feldspar 40%, kaolin 15%, zinc oxide 3%, calcite 6%, calcite 4%, barium carbonate 9%, aluminum oxide 3%, calcined kaolin 5%. The chemical composition of the protective glaze includes: in mass percentage, SiO2: 52.49%; Al2O3: 19.86%; MgO: 1.54%; CaO: 3.46%; BaO: 7.01%; ZnO: 2.98%; K2O: 1.96%; Na2O: 4.36%; loss on ignition: 6.34%. The protective glaze is applied by spraying. The specific gravity of the protective glaze is 1.35 g / cm 3 , glaze application amount is 280 g / m 2 .
[0072] Step 6. The green body with the protective glaze applied is fired and polished to obtain the unfired dry-grain ceramic tile. The firing temperature is 1190° C. and the firing cycle is 70 minutes.
[0073] Figure 3This is the brick surface effect diagram of Example 2. Since Example 2 covers the surface glaze on the surface of the unfired dry particle layer, the glaze surface of Example 2 is smoother than that of Example 1, and the granularity is not obvious, which is closer to the traditional mold effect, but its pattern clarity is significantly improved compared with the conventional glue positioning dry particle process.
[0074] Comparative Example 1
[0075] The method for preparing glue-positioned dry-grain ceramic tiles comprises the following steps:
[0076] Step 1. Apply glaze on the surface of the dried body. The composition and glazing parameters of the glaze are the same as those in Example 1.
[0077] Step 2. Inkjet print a normal ink pattern on the surface of the glazed body.
[0078] Step 3. Inkjet glue pattern on the surface of the blank after inkjet printing of ordinary ink pattern.
[0079] Step 4. Apply frit dry particles on the surface of the blank after the inkjet printing of the glue pattern. The frit dry particles are matte frit dry particles commonly used in the industry. The chemical composition of the frit dry particles includes: by mass percentage, Al2O3: 17%, SiO2: 51%, CaO: 9.5%, MgO: 1%, K2O: 3%, Na2O: 3%, BaO: 10%, ZnO: 5.5%.
[0080] Step 5. Apply protective glaze on the surface of the green body after applying the frit dry particles. The composition and glazing parameters of the protective glaze are the same as those in Example 1.
[0081] Step 6. The green body with the protective glaze applied is fired and polished to obtain the glue-positioned dry-grain ceramic tile. The firing temperature is 1190° C. and the firing cycle is 70 minutes.
[0082] Figure 4 This is an optical effect picture of the frit dry particles. It can be seen that the dry particles have been fired and are glassy with a smooth surface.
[0083] Figure 5 This is the brick surface effect diagram of comparative example 1. Since the surface of the frit dry particles is relatively smooth and difficult to absorb ceramic ink, when the ink forming the inkjet pattern is printed on the surface of the conventional frit dry particles, the ink is not only difficult to dry but also agglomerates. Therefore, the prior art must place the frit dry particles above the inkjet pattern layer to avoid affecting the clarity of the pattern. Moreover, the frit dry particles are matte dry particles with poor transparency. When the frit dry particles are positioned and applied on the dark inkjet pattern surface, the pattern is relatively blurred, which greatly affects the clarity of the brick surface pattern.
[0084] Comparative Example 2
[0085] It is basically the same as Example 1, except that the particle size of the non-fired dry particles is about 30 meshes.
[0086] Figure 6 This is the brick surface effect picture of Example 2. It can be seen that the mesh size of the unburned particles is small, the particles are large, and they stand abruptly on the brick surface, which does not match the layout design.
[0087] Comparative Example 3
[0088] It is basically the same as Example 1, except that the particle size of the non-fired dry particles is 250 meshes.
[0089] Figure 7 This is the brick surface effect picture of comparative example 3. It can be seen that the mesh number of the unburned particles is large, the particles are small, the dry particles are difficult to adhere to the brick surface, and a large number of them are agglomerated into agglomerates, the mold effect of the brick surface is poor, and the pattern presentation is not ideal.
[0090] Comparative Example 4
[0091] The same as Example 1, except that the amount of the unburned dry particles applied is 300 g / m 2 .
[0092] Figure 8 This is the brick surface effect diagram of comparative example 4. It can be seen that when the amount of unfired dry particles applied is large, the unfired dry particles shrink more during the drying process, causing drying crack defects on the glaze surface.
Claims
1. A method for preparing non-fired dry granules, characterized in that: The mineral composition of the unfired dry particles includes, by mass percentage, 10-40% potassium feldspar, 25-55% sodium feldspar, 20-30% kaolin, 5-10% quartz powder, and 5-15% calcite; the raw materials are weighed according to the mineral composition of the unfired dry particles, water and additives are added, and the mixture is evenly mixed to form a glaze slurry, and the glaze slurry is spray-dried and granulated to obtain the unfired dry particles; the chemical composition of the unfired dry particles includes, by mass percentage, SiO2: 55-70%; Al2O3: 18-26%; Fe2O3: 0.1-0.3%; TiO2: 0.1-0.2%; MgO: 0.1-0.5%; CaO: 2-9%; K2O: 1-5%; Na2O: 4-6%; loss on ignition: 4-10%; the particle size of the unfired dry particles is 60-150 meshes.
2. Unfired dry granular ceramic bricks, characterized in that: The unfired dry particle ceramic tile comprises: a body layer, a top glaze layer and an unfired dry particle layer with adjustable sequence, an inkjet pattern layer, and a protective glaze layer; wherein the unfired dry particle layer is made of unfired dry particles formed by the preparation method according to claim 1.
3. A method for preparing a non-fired dry granular ceramic tile, characterized in that: The preparation method comprises: applying glaze on the surface of the green body; inkjet printing a glue pattern on the surface of the green body after the glaze is applied; applying the unfired dry particles formed by the preparation method according to claim 1 on the surface of the green body after the glue pattern is inkjet printed; the application amount of the unfired dry particles is 50-200 g / m 2 ; inkjet printing a common ink pattern on the surface of the green body after applying the unfired dry particles; applying a protective glaze on the surface of the green body after the ordinary ink pattern is inkjet printed; firing and polishing the green body after applying the protective glaze to obtain the unfired dry particle ceramic tile; or, The preparation method comprises: inkjet printing a glue pattern on the surface of a blank; applying the unburned dry particles formed by the preparation method according to claim 1 on the surface of the blank after the glue pattern is inkjet printed; the application amount of the unburned dry particles is 50-200 g / m 2 ; applying a glaze on the surface of the green body after applying the unfired dry particles; inkjet printing a common ink pattern on the surface of the green body after applying the glaze; applying a protective glaze on the surface of the green body after inkjet printing the common ink pattern; firing and polishing the green body after applying the protective glaze to obtain the unfired dry particle ceramic tile.
4. The preparation method according to claim 3, characterized in that: The chemical composition of the glaze includes, by mass percentage, SiO2: 60~70%, Al2O3: 12~25%, Fe2O3: 0.1~0.5%, TiO2: 0.1~0.5%, CaO: 0.1~0.5%, MgO: 1~5%, K2O: 2~5%, Na2O: 2~5%, ZrO2: 3~10%, and loss on ignition: 1~3%.
5. The preparation method according to claim 3, characterized in that: The surface glaze is applied by spraying or pouring; the specific gravity of the surface glaze is 1.40-1.50 g / cm 3 , glaze application amount is 450~650g / m 2 .
6. The preparation method according to claim 3, characterized in that: The chemical composition of the protective glaze includes, by mass percentage, SiO2: 45-55%; Al2O3: 17-24%; MgO: 1-3%; CaO: 2-6%; BaO: 3-8%; ZnO: 2.5-5%; K2O: 1-3%; Na2O: 3.5-5%; and loss on ignition: 4-9%.
7. The preparation method according to claim 3, characterized in that The protective glaze is applied by spraying; the specific gravity of the protective glaze is 1.35-1.40 g / cm 3 , glaze application amount is 250~300 g / m 2 .
8. The preparation method according to claim 3, characterized in that: The firing temperature is 1180~1200℃ and the firing cycle is 60~80 minutes.