A high-ductility concrete and its preparation method

By introducing self-made zeolite and foaming components into high-ductility concrete, a microporous structure and fiber bridging mechanism are formed, which solves the problem of insufficient ductility of high-ductility concrete under extreme conditions and achieves higher seismic performance and environmentally friendly resource utilization.

CN118561548BActive Publication Date: 2026-11-17ZHENJIANG JIANKE CONSTR TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410522334.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2026-11-17
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

Existing high-ductility concrete lacks sufficient ductility under extreme conditions, failing to meet engineering requirements, and may cause structural damage, especially in natural disasters such as strong earthquakes.

Method used

By adding homemade zeolite or homemade foaming components to concrete as defect generators, a microporous structure and fiber bridging mechanism are introduced to form a composite reinforcement system, thereby improving the toughness and seismic performance of concrete.

Benefits of technology

It significantly improves the seismic resistance of concrete, fiber bridging prevents crack propagation, microporous structure disperses stress, improves toughness and seismic performance, and at the same time, it environmentally utilizes domestic waste and carbon dioxide resources.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a high-ductility concrete and its preparation method. By adding a defect-generating agent, either a self-made zeolite or a self-made foaming component, to the high-ductility concrete matrix and mixing them uniformly, the defect-generating agent produces defects with a volume fraction of 1%-9% in the high-ductility concrete matrix. This significantly improves flexural strength with a slight sacrifice in compressive strength. The high-ductility concrete of this invention can effectively control crack development, maintain high load-bearing capacity after cracking, and exhibit greater deformation capacity under external forces, thereby improving the seismic and impact resistance of the structure. Due to its excellent durability and damage resistance, high-ductility concrete is suitable for construction projects in various harsh environments, extending the service life of buildings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a high-ductility concrete and its preparation method. Background Technology

[0002] Existing masonry structures and old buildings are widespread throughout my country. Due to limitations of time and technology, these buildings typically suffer from poor earthquake resistance and low safety. With the increasing demands for earthquake-resistant building standards and the growing need for longer building lifespans, the aging problem of these older buildings has become more prominent, no longer meeting current housing safety standards and posing significant safety risks. To address the insufficient safety and poor earthquake resistance of existing buildings, Victor Lee, a Chinese-American scientist, proposed the ECC theory in the 1990s. He explored the use of high-strength fiber-reinforced concrete, significantly improving the flexural strength of concrete and laying a solid theoretical and practical foundation for the future development of high-ductility concrete.

[0003] High-ductility concrete is a novel cement-based composite material. Unlike traditional concrete, it possesses extremely high toughness and is known as "flexible concrete." It is commonly used for the reinforcement and renovation of buildings and historical sites requiring earthquake resistance. The seismic resistance of high-ductility concrete has always been a key focus in scientific research and application. The widespread application of this material is of practical significance to my country's urban renewal strategy. The seismic resistance of high-ductility concrete is primarily influenced by the material's inherent toughness. Unlike ordinary concrete, which fails upon cracking, high-ductility concrete exposes its fibers after cracking. Under the tension of these high-strength fibers, the high-ductility concrete matrix maintains high flexural and tensile strength, ensuring the building does not collapse.

[0004] Although high-ductility concrete has better ductility than traditional concrete, its ductility may still be insufficient to meet engineering requirements under certain extreme conditions, such as large deformation or repeated loading. This could lead to structural damage in natural disasters such as strong earthquakes. Therefore, improving its stability and lifespan in extreme environments is one of the key research focuses. Summary of the Invention

[0005] The main objective of this invention is to provide a high-ductility concrete and its preparation method. By adding defect-producing substances to the concrete, the flexural strength is greatly improved, the ductility of the concrete is further enhanced, and the seismic resistance is significantly improved.

[0006] The objective of this invention can be achieved by adopting the following technical solution:

[0007] A high-ductility concrete, comprising a high-ductility concrete matrix and defect-generating materials;

[0008] The defect-generating products cause defects in the high-ductility concrete matrix to have a volume fraction of 1%-9%;

[0009] The defect product is a self-made zeolite or a self-made foaming component;

[0010] The self-made zeolite is composed of zeolite precursor and carbon dioxide. The zeolite precursor, by weight, includes: 2-3 parts fly ash, 1-2 parts calcium hydroxide, and 8-12 parts water.

[0011] The self-made foaming components, by weight, include: 32-45 parts sodium dodecyl sulfate, 5-15 parts silicone polyether emulsion, 15-25 parts cellulose ether, and 2-5 parts nano silica aerogel.

[0012] The amount of the self-made zeolite added is 1%-9% of the weight of the high-ductility concrete matrix;

[0013] The amount of the self-made foaming component added is 0.1%-0.5% of the weight of the high-ductility concrete matrix.

[0014] Preferably, the high-ductility concrete matrix comprises, by weight, 550-700 parts cement, 320-440 parts quartz sand, 1-3 parts water-reducing agent, 1-3 parts thixotropic agent, 1-2 parts cellulose ether, 1-2 parts starch ether, 0-3 parts defoamer, and 6-12 parts high-strength fiber.

[0015] Preferably, the water-reducing agent is a polycarboxylate water-reducing agent, and the thixotropic agent is an N987 thixotropic agent.

[0016] Preferably, the fly ash is a product of municipal solid waste combustion.

[0017] Preferably, the ratio of fly ash to calcium hydroxide is 2:1.

[0018] A method for preparing high-ductility concrete includes the following steps:

[0019] Step 1: Weigh the raw materials according to the weight proportions specified in claim 2 to obtain a high-ductility concrete matrix;

[0020] Step 2: Weigh the raw materials according to the weight proportions specified in claim 1 to obtain the self-made zeolite or self-made foaming component;

[0021] Step 3: Add the homemade zeolite or homemade foaming component to the high ductility concrete matrix, stir and mix evenly to obtain high ductility concrete.

[0022] Preferably, in step 1, the preparation process of the high-ductility concrete matrix is ​​as follows: weigh cement, quartz sand, water-reducing agent, thixotropic agent, cellulose ether, starch ether, defoamer and high-strength fiber, add them to a mixer and mix them until they are fully mixed and uniform, so as to obtain the high-ductility concrete matrix.

[0023] Preferably, in step 2, the preparation process of the homemade zeolite is as follows:

[0024] 1) Weigh fly ash, calcium hydroxide and water. Mix fly ash and calcium hydroxide evenly and heat the mixture at 600℃-650℃ for 40-80 minutes. After cooling, mix the mixture with water to form an emulsion. Pour the emulsion into a hydrothermal reactor and react at 100-160℃ for 35-60 minutes. Place the reaction product in a centrifuge and centrifuge at 2000 rpm for 4-6 minutes to complete solid-liquid separation and obtain the zeolite precursor.

[0025] 2) Place the zeolite precursor in a carbonization kettle and cure it with carbon dioxide gas for 60-90 minutes to generate calcium carbonate on the surface of the zeolite precursor, thus obtaining the homemade zeolite.

[0026] Preferably, in step 2, the preparation process of the self-made foaming component is as follows: weigh sodium dodecyl sulfate, silicone resin polyether emulsion, cellulose ether and nano silica aerogel, mix them thoroughly and evenly to obtain the self-made foaming component.

[0027] Preferably, the concentration of the carbon dioxide is higher than 50%.

[0028] Compared with the prior art, the beneficial technical effects of the present invention are:

[0029] 1. This invention uses self-made zeolite or self-made foaming components as defect generators added to high-ductility concrete, which introduces a large number of microporous structures into the concrete. These microporous structures act as buffers when the concrete is under stress, reducing stress concentration and increasing energy absorption capacity, thereby improving the seismic performance of the concrete. Simultaneously, the fibers in the high-ductility concrete work together with these microporous structures to form a composite reinforcement system. The fibers act as bridges at the crack tip, preventing crack propagation, while the microporous structures provide additional fracture surfaces, requiring the crack to overcome more resistance during propagation. This synergistic effect enables the high-ductility concrete to generate multiple fine cracks under stress, rather than a few wide cracks, thus more effectively dispersing stress and improving the toughness and seismic performance of the concrete.

[0030] 2. The self-made zeolite used in this invention utilizes fly ash, a byproduct of municipal solid waste incineration, as a raw material, and employs carbon dioxide to strengthen the zeolite. Firstly, this approach significantly reduces environmental pollution because the potential heavy metals and harmful chemicals contained in the fly ash are effectively controlled by converting them into valuable raw materials, thus protecting soil, water, and the atmosphere. Secondly, this resource recycling strategy conserves energy and natural resources, especially in the production of building materials such as cement clinker, where the utilization of fly ash reduces the demand for natural raw materials and energy consumption. Furthermore, this circular economy practice promotes the transition of society towards sustainable development, aligns with global environmental trends, and provides a green and sustainable development model for the future. Simultaneously, using carbon dioxide to strengthen the zeolite not only increases its weight, making it easier for zeolite particles to settle in concrete slurry and fully contact other components such as cement paste, sand, and gravel, achieving uniform dispersion, but also serves as an effective means of carbon capture and utilization, contributing to mitigating climate change.

[0031] 3. The self-made foaming component used in this invention, by combining sodium dodecyl sulfate, silicone polyether emulsion, cellulose ether, and nano-silica aerogel, offers multiple benefits, including environmental advantages, cost advantages, improved concrete performance, and enhanced construction efficiency. First, this self-made foaming agent utilizes readily available raw materials, reducing reliance on commercial foaming agents and lowering environmental pollution. Second, the self-made foaming component effectively improves the thermal insulation and durability of concrete while reducing its weight and increasing its toughness and energy absorption. Furthermore, the self-made foaming component improves the flowability and pumpability of concrete, thereby increasing construction efficiency and reducing construction difficulty. Finally, due to the improved stability of the foam, the consistency of concrete quality and performance is guaranteed. Detailed Implementation

[0032] To make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with embodiments.

[0033] Example 1

[0034] This invention provides a high-ductility concrete and its preparation method. The high-ductility concrete comprises a high-ductility concrete matrix and defect-generating substances. The volume fraction of defects generated by the defect-generating substances in the high-ductility concrete matrix is ​​1%-9%. The defect-generating substances are self-made zeolite or self-made foaming components. The self-made zeolite is composed of zeolite precursor and carbon dioxide. The zeolite precursor, by weight, comprises: 2-3 parts fly ash, 1-2 parts calcium hydroxide, and 8-12 parts water. The self-made foaming components, by weight, comprise... The composition consists of: 32-45 parts sodium dodecyl sulfate, 5-15 parts silicone polyether emulsion, 15-25 parts cellulose ether, and 2-5 parts nano silica aerogel. To ensure the self-made zeolite produces a defect of 1%-9% by volume in the high-ductility concrete matrix, 1%-9% of the weight of the self-made zeolite in the high-ductility concrete matrix needs to be added. Similarly, to ensure the self-made foaming component produces a defect of 1%-9% by volume in the high-ductility concrete matrix, 0.1%-0.5% of the weight of the self-made foaming component in the high-ductility concrete matrix needs to be added.

[0035] The self-made zeolite of this invention uses fly ash and carbon dioxide, substances harmful to the environment, as raw materials, which is beneficial to environmental protection. Moreover, the use of carbon dioxide to strengthen the zeolite increases its self-weight, making it easier for zeolite particles to sink in concrete slurry and fully contact with cement paste, sand, gravel and other components, thereby achieving uniform dispersion and improving the effect of defect prevention.

[0036] The self-made foaming component of this invention incorporates nano-silica aerogel, which can improve the stability of the foam and generate fine and uniformly distributed bubbles. These bubbles can form a good microporous structure during the concrete curing process, thereby improving the homogeneity and durability of the concrete.

[0037] This invention introduces a large number of microporous structures into high-ductility concrete by using self-made zeolite or self-made foaming components as defect generators. Fibers and these microporous structures work together to form a composite reinforcement system. The fibers act as bridges at the crack tips, preventing crack propagation, while the microporous structures provide additional fracture surfaces, forcing cracks to overcome greater resistance during propagation. This synergistic effect enables the high-ductility concrete to generate multiple fine cracks under stress, significantly improving its seismic performance.

[0038] Specifically, the high-ductility concrete matrix, by weight, comprises: 550-700 parts cement, 320-440 parts quartz sand, 1-3 parts water-reducing agent, 1-3 parts thixotropic agent, 1-2 parts cellulose ether, 1-2 parts starch ether, 0-3 parts defoamer, and 6-12 parts high-strength fiber, to form basic high-ductility concrete.

[0039] The fly ash is a product of municipal solid waste combustion. Converting it into valuable raw materials can not only reduce the emission of these pollutants, but also reduce dependence on natural resources.

[0040] In the homemade zeolite, the ratio of fly ash to calcium hydroxide is 2:1.

[0041] The method for preparing high-ductility concrete described in this embodiment includes the following steps:

[0042] Step 1: Weigh the raw materials according to the aforementioned weight proportions to obtain a high-ductility concrete matrix;

[0043] Step 2: Weigh the raw materials according to the aforementioned weight proportions to obtain the homemade zeolite or homemade foaming component;

[0044] Step 3: Add the homemade zeolite or homemade foaming component to the high ductility concrete matrix, stir and mix evenly to obtain high ductility concrete.

[0045] In step 1, the preparation process of the high-ductility concrete matrix is ​​as follows: weigh cement, quartz sand, water-reducing agent, thixotropic agent, cellulose ether, starch ether, defoamer and high-strength fiber, add them to a mixer and mix them until they are fully mixed and uniform, so as to obtain the high-ductility concrete matrix.

[0046] In step 2, the preparation process of the self-made zeolite is as follows:

[0047] 1) Weigh fly ash, calcium hydroxide and water. Mix fly ash and calcium hydroxide evenly and heat the mixture at 600℃-650℃ for 40-80 minutes. After cooling, mix the mixture with water to form an emulsion. Pour the emulsion into a hydrothermal reactor and react at 100-160℃ for 35-60 minutes. Place the reaction product in a centrifuge and centrifuge at 2000 rpm for 4-6 minutes to complete solid-liquid separation and obtain the zeolite precursor.

[0048] 2) Place the zeolite precursor in a carbonization reactor and cure it with carbon dioxide gas for 60-90 minutes. The concentration of carbon dioxide is higher than 50%. Calcium carbonate is generated on the surface of the zeolite precursor to obtain homemade zeolite.

[0049] In step 2, the preparation process of the self-made foaming component is as follows: weigh sodium dodecyl sulfate, silicone polyether emulsion, cellulose ether and nano silica aerogel, mix them thoroughly and evenly to obtain the self-made foaming component.

[0050] Example 2

[0051] This embodiment is a high-ductility concrete. The components of the high-ductility concrete matrix in this embodiment, according to the weight parts, are: 600 parts cement, 400 parts quartz sand, 1.5 parts water-reducing agent, 2 parts thixotropic agent, 1 part cellulose ether, 1 part starch ether, 1.5 parts defoamer, and 7.5 parts high-strength fiber.

[0052] This embodiment investigates the effect of self-made zeolite on the properties of high-ductility concrete matrix. Self-made zeolite is used as a defect generator. 5% of the weight of self-made zeolite is added to the high-ductility concrete matrix to produce a 5% volume fraction of defects in the high-ductility concrete matrix.

[0053] The components of the zeolite precursor in the homemade zeolite, according to the weight percentages, are 3 parts fly ash, 2 parts calcium hydroxide, and 10 parts water.

[0054] The method for preparing high-ductility concrete described in this embodiment is as follows:

[0055] Step 1: Weigh the raw materials according to the aforementioned weight proportions to obtain a high-ductility concrete matrix;

[0056] Step 2: Weigh the raw materials according to the aforementioned weight proportions to obtain homemade zeolite;

[0057] Step 3: Add the homemade zeolite to the high-ductility concrete matrix, stir and mix evenly to obtain high-ductility concrete.

[0058] In step 2, the preparation process of the self-made zeolite is as follows:

[0059] 1) Weigh fly ash, calcium hydroxide and water. Mix fly ash and calcium hydroxide evenly and heat the mixture at 600℃-650℃ for 40-80 minutes. After cooling, mix the mixture with water to form an emulsion. Pour the emulsion into a hydrothermal reactor and react at 100-160℃ for 35-60 minutes. Place the reaction product in a centrifuge and centrifuge at 2000 rpm for 4-6 minutes to complete solid-liquid separation and obtain the zeolite precursor.

[0060] 2) Place the zeolite precursor in a carbonization kettle and cure it with carbon dioxide gas at a concentration of 60% for 60-90 minutes to generate calcium carbonate on the surface of the zeolite precursor, thus obtaining the self-made zeolite.

[0061] Example 3

[0062] This embodiment is a high-ductility concrete. The components of the high-ductility concrete matrix in this embodiment, according to the weight parts, are: 600 parts cement, 400 parts quartz sand, 1.5 parts water-reducing agent, 2 parts thixotropic agent, 1 part cellulose ether, 1 part starch ether, and 7.5 parts high-strength fiber.

[0063] This embodiment investigates the effect of a self-made foaming component on the properties of a high-ductility concrete matrix. The self-made foaming component was used as the defect generator, specifically consisting of 35 parts sodium dodecyl sulfate, 10 parts silicone polyether emulsion, 15 parts cellulose ether, and 2 parts nano-silica aerogel by weight. 0.4% of the self-made foaming component by weight of the high-ductility concrete matrix was added to generate a 5% volume fraction of defects in the high-ductility concrete matrix.

[0064] The method for preparing high-ductility concrete described in this embodiment is as follows:

[0065] Step 1: Weigh the raw materials according to the aforementioned weight proportions to obtain a high-ductility concrete matrix;

[0066] Step 2: Weigh the raw materials according to the aforementioned weight proportions to obtain the self-made foaming component;

[0067] Step 3: Add the self-made foaming component to the high-ductility concrete matrix, stir and mix evenly to obtain high-ductility concrete.

[0068] In step 2, the preparation process of the self-made foaming component is as follows: weigh sodium dodecyl sulfate, silicone polyether emulsion, cellulose ether and nano silica aerogel, mix them thoroughly and evenly to obtain the self-made foaming component.

[0069] Comparative Example 1

[0070] This comparative example examines the influence of existing zeolite on the properties of high-ductility concrete matrix. The zeolite was purchased from a company in Jiangsu Province. The zeolite was mixed evenly with the high-ductility concrete matrix to create a 5% volume fraction defect of zeolite in the high-ductility concrete matrix, thus producing high-ductility concrete. The high-ductility concrete matrix used in this comparative example is the same as that in Example 2, and the production process of the high-ductility concrete in this comparative example is the same as that in Example 2.

[0071] Comparative Example 2

[0072] This comparative example examines the influence of existing foaming components on the properties of high-ductility concrete matrix. The foaming components were purchased from a company in Shandong. The foaming components were mixed evenly with the high-ductility concrete matrix to create a 5% volume fraction defect in the high-ductility concrete matrix, thus producing high-ductility concrete. The high-ductility concrete matrix used in this comparative example is the same as that in Example 3, and the production process of the high-ductility concrete in this comparative example is the same as that in Example 3.

[0073] Comparative Example 3

[0074] This comparative example examines the performance of a high-ductility concrete matrix. The high-ductility concrete matrix used in this comparative example is the same as that in Example 2.

[0075] Comparative Example 4

[0076] This comparative example examines the performance of a high-ductility concrete matrix without the addition of a defoamer. The high-ductility concrete matrix used in this comparative example is the same as that in Example 3.

[0077] Table 1 shows a comparison of the concrete performance in Examples 2, 1, and 3.

[0078] Table 1

[0079] Compressive strength (28d) / MPa Bending strength (28d) / MPa Example 2 64.08 11.76 Comparative Example 1 63.14 10.72 Comparative Example 3 68.08 9.36

[0080] As shown in Table 1, in Example 2, the addition of self-made zeolite to the high-ductility concrete matrix reduced the compressive strength by 4 MPa, a decrease of approximately 5.87%, while increasing the flexural strength by 2.4 MPa, an increase of approximately 25.64%.

[0081] In Comparative Example 1, the addition of commercially available zeolite to a high-ductility concrete matrix reduced the compressive strength by 4.94 MPa, a decrease of approximately 7.26%, while increasing the flexural strength by 1.36 MPa, an increase of approximately 14.53%.

[0082] Table 2 shows a comparison of the concrete performance in Examples 3, 2, and 4.

[0083] Table 2

[0084] Compressive strength (28d) / MPa Bending strength (28d) / MPa Example 3 57.31 14.14 Comparative Example 2 57.24 11.18 Comparative Example 4 65.32 9.33

[0085] In Example 3, the addition of a self-made foaming component to a high-ductility concrete matrix reduced the compressive strength by 8.01 MPa, a decrease of approximately 12.26%, while increasing the flexural strength by 4.81 MPa, an increase of approximately 51.55%.

[0086] In Comparative Example 2, the addition of commercially available foaming components to a high-ductility concrete matrix reduced the compressive strength by 8.08 MPa, a decrease of approximately 12.37%, while increasing the flexural strength by 1.85 MPa, an increase of approximately 19.83%.

[0087] As shown in Tables 1 and 2, introducing defect-generating materials into the high-ductility concrete matrix effectively improves the flexural strength. In particular, when using the self-made zeolite and self-made foaming components described in this application, the compressive strength decreases only slightly, while the flexural strength increases significantly.

[0088] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

Claims

1. A high-ductility concrete, characterized in that: This includes high-ductility concrete matrices and defect-generating materials; The defect-generating products cause defects in the high-ductility concrete matrix to have a volume fraction of 1%-9%. The defect product is a self-made zeolite or a self-made foaming component; The self-made zeolite is composed of zeolite precursor and carbon dioxide. The zeolite precursor, by weight, includes: 2-3 parts fly ash, 1-2 parts calcium hydroxide, and 8-12 parts water. The self-made foaming components, by weight, include: 32-45 parts sodium dodecyl sulfate, 5-15 parts silicone polyether emulsion, 15-25 parts cellulose ether, and 2-5 parts nano silica aerogel. The amount of the self-made zeolite added is 1%-9% of the weight of the high-ductility concrete matrix; The amount of the self-made foaming component added is 0.1%-0.5% of the weight of the high-ductility concrete matrix; The high-ductility concrete matrix, by weight, includes: 550-700 parts cement, 320-440 parts quartz sand, 1-3 parts water-reducing agent, 1-3 parts thixotropic agent, 1-2 parts cellulose ether, 1-2 parts starch ether, 0-3 parts defoamer, and 6-12 parts high-strength fiber. The preparation process of the self-made zeolite is as follows: Weigh fly ash, calcium hydroxide, and water. Mix the fly ash and calcium hydroxide thoroughly and heat the mixture at 600℃-650℃ for 40-80 minutes. After cooling, mix the mixture with water to form an emulsion. Pour the emulsion into a hydrothermal reactor and react at 100-160℃ for 35-60 minutes. Centrifuge the reaction product at 2000 rpm for 4-6 minutes to complete solid-liquid separation and obtain the zeolite precursor. Place the zeolite precursor in a carbonization reactor and cure it with carbon dioxide gas for 60-90 minutes to form calcium carbonate on the surface of the zeolite precursor, thus obtaining the self-made zeolite.

2. The high-ductility concrete according to claim 1, characterized in that: The water-reducing agent is a polycarboxylate water-reducing agent, and the thixotropic agent is an N987 thixotropic agent.

3. The high-ductility concrete according to claim 1, characterized in that: The fly ash is a product of the combustion of municipal solid waste.

4. The high-ductility concrete according to claim 1, characterized in that: The ratio of fly ash to calcium hydroxide is 2:

1.

5. The high-ductility concrete according to claim 1, characterized in that: The concentration of carbon dioxide is higher than 50%.

6. A method for preparing high-ductility concrete as described in any one of claims 1-5, characterized in that: Includes the following steps: Step 1: Weigh the raw materials according to the weight proportions specified in claim 1 to obtain a high-ductility concrete matrix; Step 2: Weigh the raw materials according to the weight proportions specified in claim 1 to obtain the self-made zeolite or self-made foaming component; Step 3: Add the homemade zeolite or homemade foaming component to the high ductility concrete matrix, stir and mix evenly to obtain high ductility concrete.

7. The method for preparing high-ductility concrete according to claim 6, characterized in that: In step 1, the preparation process of the high ductility concrete matrix is ​​as follows: weigh cement, quartz sand, water-reducing agent, thixotropic agent, cellulose ether, starch ether, defoamer and high-strength fiber, add them to a mixer and mix them until they are fully mixed and uniform, so as to obtain the high ductility concrete matrix.

8. The method for preparing high-ductility concrete according to claim 6, characterized in that: In step 2, the preparation process of the self-made foaming component is as follows: weigh sodium dodecyl sulfate, silicone polyether emulsion, cellulose ether and nano silica aerogel, mix them thoroughly and evenly to obtain the self-made foaming component.

Citation Information

Patent Citations

  • Method for synthesis of zeolite from fly ash

    CN104402017A

  • Steel pipe and fiber-reinforced foam concrete composite column and preparation method thereof

    CN108643450A

  • Air-entraining concrete suitable for plateau areas

    CN112851217A