Pearlescent colorful flashing glazed tile with concave and convex effects and preparation method thereof
By adopting a concave and concave effect design in pearlescent color glaze tiles, combined with the optimized base glaze and pearlescent color glaze formula, the problems of weak flash point effect and uneven distribution in the existing technology are solved, and the problem of Strong and uniform pearlescent color flash effect and good high temperature resistance.
Patent Information
- Application Number
- CN202411034526.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The existing pearlescent color glaze glaze tiles have poor glaze effect and are unevenly distributed, and the bottom glaze layer covers limited effect, which affects the decorative performance of the pearlescent color glaze layer.
The preparation method of pearl glaze glaze tiles with concave and concave effects is adopted. Through the cooperation of the first base glaze layer, mold texture layer and pearl glaze glaze layer, the formula of base glaze and pearl glaze glaze is optimized, and the use of The dry particle positioning fuse and zirconia crystal form a depression effect, and the mutual repulsion of mold ink and base glaze form a concave and convex effect.
It realizes a strong and uniform pearlescent flash effect on the surface of the glazed tiles, improves the high temperature resistance and application range of pearlescent flash fuses, and enhances the decorative and practicality of the glazed surface.
Smart Images

Figure CN118561628B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building ceramics, in particular to a pearlescent colorful flashing glazed tile with concave and convex effects and a preparation method thereof. Background Art
[0002] In the vast world of the ceramic market, consumers' demands are becoming increasingly diversified and personalized. They not only pursue the practicality and durability of ceramic products, but also have high expectations for their artistic value and visual beauty. This change in market demand has prompted the ceramic industry to continuously innovate technology and develop products to meet the growing aesthetic and practical needs.
[0003] In the production process of ceramic tiles, the mixing of glazes is also extremely important. The same body will produce different glaze effects due to different glazes. The different touch and visual perception of the glaze will also affect the choice of consumers. Pearlescent Magic Flash frit is a special frit. When the glaze with pearlescent magic flash frit is applied to the surface of the body and fired at high temperature, the surface of the tile can present a pearlescent magic flash effect, which not only meets the market demand for the appearance of ceramic tile products, but also provides new ideas and directions for technological innovation and product upgrades in the ceramic industry, avoiding the homogenization of ceramic tile products and increasing the added value of ceramic tile products.
[0004] Due to the selection of raw materials and differences in the preparation process, the existing pearlescent magic color flash frits have technical problems such as weak pearlescent magic color effect and uneven distribution of flash points in the produced ceramic tile glaze. At the same time, in order to control the production cost of ceramic tiles, the whiteness of the green body layer in the existing glazed tiles is generally low. In order to prevent the green body layer with low whiteness from affecting the expression of the decorative function of the glaze layer, a bottom glaze layer covering the green body layer is generally added on the top of the green body layer. However, in the prior art, the bottom glaze layer has limited coverage of the green body layer, and since the green body surface color of the green body layer is generally darker, it is easy to affect the presentation of the flash effect of the pearlescent magic color flash glaze layer located on the top of the glazed tile. In addition, the surface of the existing bottom glaze layer is generally relatively flat, and the bottom glaze layer with a relatively flat surface is not conducive to the presentation of the flash effect of the pearlescent magic color flash glaze layer. That is, the existing bottom glaze layer is not conducive to the presentation of the flash effect of the pearlescent magic color flash glaze layer due to its limited covering effect and poor matching with the pearlescent magic color flash glaze layer. Summary of the invention
[0005] The purpose of the present invention is to propose a pearlescent fantasy glitter glazed tile with concave and convex effects and a preparation method thereof. Through the mutual cooperation of the first base glaze layer, the mold texture layer and the pearlescent fantasy glitter glaze layer, it is beneficial to present a strong and uniform pearlescent fantasy glitter effect on the surface of the glazed tile, so as to effectively solve the technical problems of the existing pearlescent fantasy glitter glaze, such as the weak pearlescent fantasy glitter effect and uneven distribution of the glitter points, and overcome the shortcomings of the prior art.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] The method for preparing pearlescent colorful glittering glazed tiles with concave and convex effects comprises the following steps:
[0008] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank layer after drying;
[0009] B. inkjet printing is performed on the surface of the green body layer according to a preset pattern using mold ink to obtain a mold texture layer;
[0010] C. Applying a base glaze to the surface of the mold texture layer to obtain a first base glaze layer; the base glaze comprises the following raw materials, calculated by weight: 4-8 parts of kaolin, 5-15 parts of quartz, 3-8 parts of alumina, 20-30 parts of nepheline, 25-35 parts of potassium feldspar, 3-8 parts of wollastonite, 3-8 parts of dry particle positioning frit and 15-21 parts of zirconium silicate; the dry particle positioning frit comprises the following raw materials, calculated by weight: 8-15 parts of quartz, 5-12 parts of alumina, 10-15 parts of zircon powder, 5-10 parts of lead carbonate and 49-87 parts of flux I;
[0011] D. Applying a pearlescent colorful glitter glaze to the surface of the first base glaze layer to obtain a pearlescent colorful glitter glaze layer; the pearlescent colorful glitter glaze comprises the following raw materials, calculated by weight: 4-8 parts of kaolin, 92-96 parts of pearlescent colorful glitter frit, 0.2-0.5 parts of sodium carboxymethyl cellulose, 0.2-0.4 parts of sodium tripolyphosphate and 35-45 parts of water; the pearlescent colorful glitter frit comprises the following raw materials, calculated by weight: 8-20 parts of perlite, 25-35 parts of quartz, 8-15 parts of alumina, 10-18 parts of fused magnesia, 3-8 parts of potassium fluorosilicate, 8-15 parts of potassium nitrate, 5-10 parts of phase separator, 5-10 parts of cerium oxide and 6-16 parts of flux II;
[0012] E. After drying, the tiles are put into kiln for firing to obtain pearlescent colorful glazed tiles with double concave and convex effects.
[0013] Furthermore, the method further comprises step F, and step F is located between step A and step B;
[0014] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank layer after drying;
[0015] F. Applying a base glaze on the surface of the green body layer to obtain a second base glaze layer; wherein the amount of the base glaze applied is 45-55 g / cm 3 , specific gravity is 1.85~1.90;
[0016] B. Using mold ink, inkjet printing is performed on the surface of the second base glaze layer according to a preset pattern to obtain a mold texture layer.
[0017] Furthermore, in step C, calculated by mass percentage, the content of zirconium oxide in the zirconium silicate is 60-65%, and the content of zirconium oxide in the zircon powder is 70-85%.
[0018] Furthermore, in step C, the particle size distribution of the dry particle positioning frit is as follows: the residue on a 100-mesh sieve is 0.1-0.5%, the residue on a 120-mesh sieve is 40-50%, and the residue on a 140-mesh sieve is 70-80%.
[0019] Furthermore, in step C, the firing curve of the dry particle positioning frit is:
[0020] It takes 1.5 to 3 hours to heat from room temperature to 500°C;
[0021] It takes 0.5 to 1.5 hours to raise the temperature from 500°C to 1100°C;
[0022] It takes 0.4 to 1 h to heat from 1100°C to 1530°C;
[0023] 1530℃, keep warm for 0.5~1.2h.
[0024] Furthermore, in step C, the base glaze is applied by spraying, and according to the mass percentage, the base glaze passes through a 250-mesh sieve, the sieve residue is 0.5-0.7%, and the spraying amount is 55-60 g / cm 3 , specific gravity is 1.52~1.60;
[0025] In step D, according to the mass percentage, the residue of the pearlescent colorful glaze after passing through a 325-mesh sieve is 0.3-0.5%, and the glazing amount is 23-27 g / cm 3 , specific gravity is 1.28~1.32.
[0026] Furthermore, in step D, the method for preparing the pearlescent colorful sparkling frit comprises the following steps:
[0027] D1. After cerium oxide and perlite are uniformly mixed according to the ratio, water is added to mix to obtain a mixture I; the mixture I is sent to a pelletizer, and after drying, granules I are obtained;
[0028] D2. After quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are uniformly mixed according to the proportion, water is added to mix to obtain a mixture II; the mixture II is fed into a pelletizing machine, and after drying, granules II are obtained;
[0029] D3. After the particles I and II are evenly mixed, a phase separation agent and a flux in a prescribed amount are added, mixed and fired at a high temperature. After water quenching, cooling and drying, a pearlescent colorful sparkling melt is obtained.
[0030] Furthermore, in step D, the mesh size of the cerium oxide is 300-325 meshes, the mesh size of the perlite is 300-325 meshes, and the mesh size of the fused magnesia is 380-400 meshes.
[0031] Further, in step C, calculated by weight, the base glaze includes the following raw materials: 6 parts of kaolin, 10 parts of quartz, 5 parts of alumina, 25 parts of nepheline, 27 parts of potassium feldspar, 5 parts of wollastonite, 5 parts of dry particle positioning frit and 20 parts of zirconium silicate.
[0032] The pearlescent colorful glittering glazed tile with concave and convex effects is prepared by using the preparation method of the pearlescent colorful glittering glazed tile with concave and convex effects.
[0033] The technical solution provided by the present invention may include the following beneficial effects:
[0034] 1. The essence of the pearlescent iridescent frit of the present technical solution is cerium oxide wrapped in fluorphlogopite glass, and the refractive index of the cerium oxide crystal is 2.44, the refractive index of the fluorphlogopite is 1.6, and the refractive index of the glass phase generated by the glass in the frit is 1.54, so that the glaze surface formed by the glaze added with the pearlescent iridescent frit has three crystals with different refractive indices. Since the cerium oxide crystal has a face-centered cubic crystal structure, its crystal plane parallel to the glaze surface has a low interfacial energy, so it shows strong anisotropy during the growth process and has good mirror reflection characteristics for visible light, thus forming a strong mirror reflection. When the incident light shines on the glaze surface formed by the glaze added with the pearlescent iridescent frit, the glaze surface can simultaneously undergo refraction, reflection and interference. And because the fluorphlogopite is translucent and the cerium oxide is white, the glaze surface forms a strong and uniform pearlescent iridescent effect.
[0035] 2. The technical solution adds a first base glaze layer between the body layer and the pearlescent iridescent glaze layer, and introduces dry particle positioning frit that is beneficial to the formation of a recessed effect in the first base glaze layer into the base glaze formula. The high zirconium system of the dry particle positioning frit enables the dry particle positioning frit to use zirconium oxide crystals as the main crystal phase. At the same time, zirconium silicate is introduced into the base glaze formula of the technical solution, which can also enable the base glaze to generate zirconium oxide crystals after firing. The high-temperature viscosity of zirconium oxide crystals is large, and their high-temperature fluidity is relatively low, so that the base glaze is not easy to melt flat after being fired in the kiln, and still maintains its original state and original thickness, which is beneficial to the first base glaze layer to form a surface with micro-corrugations, that is, the first base glaze layer has a concave effect. The concave effect causes the pearlescent fantasy glaze layer to have a thickness deviation, that is, the thickness of the pearlescent fantasy glaze layer at the protrusions of the first base glaze layer is relatively thin, and the thickness of the first base glaze layer is relatively thick at the concave parts. The above-mentioned thickness deviation is beneficial to promoting the pearlescent particles of cerium oxide-wrapped fluorphlogopite with different refractive indices in the inner and outer layers to produce stronger reflection, refraction and interference under light conditions, thereby presenting a stronger pearlescent fantasy glitter effect.
[0036] 3. Through the combination of the concave effect formed by the glaze formula itself and the concave-convex effect formed by the mutual repulsion between the base glaze and the mold ink, the pearlescent colorful glaze layer produces a greater thickness deviation, which greatly promotes the pearlescent particles of cerium oxide wrapped in fluorphlogopite with different refractive indices in the inner and outer layers to produce stronger reflection, refraction and interference under light conditions, thereby presenting an extremely strong pearlescent colorful glitter effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a glaze effect diagram of the glazed tile prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0038] The technical solution provides a method for preparing a pearlescent colorful glazed tile with concave and convex effects, comprising the following steps:
[0039] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank layer after drying;
[0040] B. inkjet printing is performed on the surface of the green body layer according to a preset pattern using mold ink to obtain a mold texture layer;
[0041] C. Applying a base glaze to the surface of the mold texture layer to obtain a first base glaze layer; the base glaze comprises the following raw materials, calculated by weight: 4-8 parts of kaolin, 5-15 parts of quartz, 3-8 parts of alumina, 20-30 parts of nepheline, 25-35 parts of potassium feldspar, 3-8 parts of wollastonite, 3-8 parts of dry particle positioning frit and 15-21 parts of zirconium silicate; the dry particle positioning frit comprises the following raw materials, calculated by weight: 8-15 parts of quartz, 5-12 parts of alumina, 10-15 parts of zircon powder, 5-10 parts of lead carbonate and 49-87 parts of flux I;
[0042] D. Applying a pearlescent colorful glitter glaze to the surface of the first base glaze layer to obtain a pearlescent colorful glitter glaze layer; the pearlescent colorful glitter glaze comprises the following raw materials, calculated by weight: 4-8 parts of kaolin, 92-96 parts of pearlescent colorful glitter frit, 0.2-0.5 parts of sodium carboxymethyl cellulose, 0.2-0.4 parts of sodium tripolyphosphate and 35-45 parts of water; the pearlescent colorful glitter frit comprises the following raw materials, calculated by weight: 8-20 parts of perlite, 25-35 parts of quartz, 8-15 parts of alumina, 10-18 parts of fused magnesia, 3-8 parts of potassium fluorosilicate, 8-15 parts of potassium nitrate, 5-10 parts of phase separator, 5-10 parts of cerium oxide and 6-16 parts of flux II;
[0043] E. After drying, the tiles are put into kiln for firing to obtain pearlescent colorful glazed tiles with double concave and convex effects.
[0044] In order to solve the technical problems in the prior art that the pearlescent fantasy glitter glazed tiles have weak pearlescent fantasy glitter effect and uneven distribution of the flash points, this technical solution proposes a method for preparing pearlescent fantasy glitter glazed tiles with concave and convex effects, including five steps: A (preparing the body layer), B (applying the base glaze), C (printing the mold ink), D (applying the pearlescent fantasy glitter glaze) and E (firing in the kiln), and by optimizing the base glaze formula and the pearlescent glitter glaze formula, the base glaze layer, the mold texture layer and the pearlescent fantasy glitter glaze layer cooperate with each other, which is conducive to presenting a strong and uniform pearlescent fantasy glitter effect on the surface of the glazed tile to meet the use requirements. It should be noted that the body layer in this solution is formed by pressing and drying the conventional ceramic blank in the ceramic field, and the mold texture layer is printed by the conventional mold ink in the ceramic field. The ceramic blank and the mold ink are not further described here.
[0045] Specifically, firstly, the prior art generally uses high-refractive-index oxides (such as iron oxide) to wrap the surface of low-refractive-index mica minerals to form a pearlescent color effect. However, due to the dark color of iron oxide, it is easy to turn red, which can easily cover the original pattern of the ceramic and affect its decorative effect. In addition, the high-temperature decomposition of mica minerals can easily cause the pearlescent color flash frit to no longer have a pearlescent color effect, so that the pearlescent color flash frit can only be used in the field of artistic ceramics and is difficult to be used in the field of architectural ceramics. Therefore, the pearlescent color flash glaze of this technical solution cannot be designed based on the above principle.
[0046] Therefore, in order to solve the defects in the above-mentioned prior art, the technical scheme uses perlite as a layered structure carrier, uses quartz to increase the silicon element, fused magnesia to provide magnesium, potassium fluorosilicate to provide potassium and fluorine elements, alumina to provide aluminum element and potassium nitrate to provide potassium element, so that quartz, fused magnesia, potassium fluorosilicate, alumina and potassium nitrate react with each other to generate fluorophlogopite with a layered structure, and cerium oxide is wrapped around the outside of the fluorophlogopite to form pearlescent particles of cerium oxide wrapped fluorophlogopite, that is, the essence of the pearlescent fantasy flash frit is cerium oxide wrapped fluorophlogopite glass, and the refractive index of cerium oxide crystals is 2.44, and the refractive index of fluorophlogopite is 1.6. At the same time, the refractive index of the glass phase generated by the glass in the frit is 1.54, so that the glaze surface formed by the glaze added with the pearlescent fantasy flash frit has three crystals with different refractive indices. Since cerium oxide crystals have a face-centered cubic crystal structure, the crystal planes parallel to the glaze surface have low interfacial energy, so they show strong anisotropy during the growth process and have good specular reflection characteristics for visible light, thus forming strong specular reflection. When the incident light irradiates the glaze surface formed by the glaze with the pearlescent fantasy flash frit added, the glaze surface can simultaneously undergo three phenomena: refraction, reflection and interference. Moreover, since fluorphlogopite is translucent and cerium oxide is white, the glaze surface forms a strong and uniform pearl fantasy flash effect. In addition, compared with mica minerals, fluorphlogopite has good high temperature resistance. In addition, since the essence of the pearlescent fantasy flash frit is fluorphlogopite glass wrapped with cerium oxide, that is, fluorphlogopite is wrapped with cerium oxide with extremely excellent high temperature resistance to form a high temperature resistant protective layer, the high temperature resistance of fluorphlogopite is further ensured, so that the pearlescent fantasy flash frit can also be used under high temperature firing, which increases its application range. In addition, the cerium oxide in the present technical solution is white, and compared with the darker iron oxide, it is not easy to cover the original pattern of the ceramic, thereby ensuring its decorative effect.
[0047] It should be noted that fused magnesia is a general term for the products of magnesia raw materials such as magnesia that are molten after high-temperature treatment. Calculated by mass percentage, the chemical composition of fused magnesia includes MgO ≥ 98%, SiO2 ≤ 0.6% and CaO ≤ 1.2%.
[0048] In order to further enhance the pearlescent fantasy sparkle effect of the pearlescent fantasy sparkle frit, the technical solution further adds a phase separation agent to the frit formula. The phase separation agent is easily separated from the glass phase network structure during the heat treatment process, resulting in phase separation. The phase separation can promote the enrichment of cerium oxide in the frit, making it easier for cerium oxide crystals to precipitate and be wrapped around the outside of the layered fluorophlogopite, which not only helps to increase the precipitation amount of pearlescent particles of cerium oxide wrapped in fluorophlogopite, forming a strong and uniform pearlescent fantasy sparkle effect, but also helps to enhance the hardness of the frit.
[0049] Furthermore, since the increase in fluorine content will hinder the weakening of hydroxyl groups and lattices at high temperatures, thereby delaying the dehydration and decomposition of fluorophlogopite, that is, the fluorine element in fluorophlogopite plays an important role in stabilizing the lattice structure, significantly improving the thermal stability of fluorophlogopite, and within a certain range, the higher the fluorine content, the greater the degree to which the decomposition temperature of fluorophlogopite can be increased. Therefore, in the present technical solution, the addition amount of potassium fluorosilicate is limited to 3 to 8 parts to ensure the formation of fluorophlogopite and improve its high temperature resistance at a lower cost.
[0050] In addition, it should be noted that the frit of the present technical solution utilizes the reaction of quartz, alumina and flux to generate a silicate network structure, thereby forming a glass phase, which is beneficial to improving the hardness and wear resistance of the frit. However, due to the high melting points of quartz and alumina, and the large amount of both added, when no flux is added or the amount of flux added is too little, it is easy to cause the frit to fail to be completely calcined during the firing process, affecting the precipitation amount of pearlescent particles of cerium oxide-wrapped fluorphlogopite, and further affecting the pearlescent and colorful sparkling effect of the frit. Therefore, in the present technical solution, the amount of flux added is limited to 6 to 16 parts, which is beneficial to ensure the pearlescent and colorful sparkling effect of the frit.
[0051] Therefore, the pearlescent fantasy flash frit in the present technical scheme is achieved through the mutual coordination of perlite, quartz, alumina, fused magnesia, potassium nitrate, phase separation agent, cerium oxide and flux II, so that the pearlescent fantasy flash frit can not only form a strong and uniform pearlescent fantasy flash effect without affecting the decorative effect of the inkjet printing layer, but also effectively maintain its pearlescent fantasy flash effect under high-temperature firing, so that it can be applied to the field of building ceramics, expanding its scope of use.
[0052] Furthermore, the raw materials of the pearlescent fantasy glaze of the technical solution also include kaolin, sodium carboxymethyl cellulose, sodium tripolyphosphate and water. Among them, kaolin can effectively improve the suspension and water retention of the glaze slurry, so that the glaze slurry does not produce precipitation during the glazing process; sodium carboxymethyl cellulose is beneficial to improving the fluidity of the glaze slurry, making it convenient for glazing operation, and at the same time sodium carboxymethyl cellulose can improve the bonding performance of the body glaze and prevent deglazing; sodium tripolyphosphate is beneficial to increase the fluidity of the pearlescent fantasy glaze while reducing the water content of the pearlescent fantasy glaze, and improve the fluidity and stability of the pearlescent fantasy glaze; water as a solvent helps to dissolve and mix the various components evenly to ensure the effect of the pearlescent fantasy glaze. That is, the raw materials in the pearlescent fantasy glaze in the technical solution cooperate with each other to ensure its performance.
[0053] Secondly, in order to best present the glittering effect of the pearlescent fantasy glaze on the surface of the glazed tile, the technical solution adds a first base glaze layer between the body layer and the pearlescent fantasy glaze layer, and introduces dry particle positioning frit that is beneficial to the formation of a recessed effect in the first base glaze layer into the base glaze formula. The high zirconium system of the dry particle positioning frit enables the dry particle positioning frit to use zirconium oxide crystals as the main crystal phase; at the same time, zirconium silicate is introduced into the base glaze formula of the technical solution, which can also enable the base glaze to generate zirconium oxide crystals after firing. The high-temperature viscosity of zirconium oxide crystals is large, and they have low high-temperature fluidity, so that the base glaze is not easy to melt flat after being fired in the kiln, and it still maintains its original state and original thickness, which is conducive to the first base glaze layer to form a surface with micro-ripples, that is, the first base glaze layer has a concave effect, and the concave effect causes the pearlescent fantasy glaze layer to have a thickness deviation, that is, the thickness of the pearlescent fantasy glaze layer is relatively thin at the protrusions of the first base glaze layer, and the thickness of the first base glaze layer is relatively thick at the concave parts. The above thickness deviation is conducive to promoting the pearlescent particles of cerium oxide wrapped in fluorphlogopite with different refractive indices in the inner and outer layers to produce stronger reflection, refraction and interference under the condition of light, thereby presenting a stronger pearlescent fantasy glitter effect. In addition, the refractive index of zirconium oxide crystals is 2.14, and it can also produce reflection, refraction and interference with the pearlescent particles of cerium oxide wrapped in fluorphlogopite under the condition of light, which is conducive to further enhancing the pearlescent fantasy glitter effect. In addition, the zirconium oxide generated after firing in the base glaze formula is beneficial to improving the whiteness of the first base glaze layer, achieving the purpose of covering the body layer, thereby avoiding the poor covering effect of the base glaze layer in the prior art, affecting the pearlescent fantasy and sparkling effect.
[0054] Furthermore, although the present technical solution adds a first bottom glaze layer, and uses the micro-corrugated surface of the first glaze layer to form a concave effect, the concave effect formed by the micro-corrugated surface is limited. In order to further enhance the concave-convex effect of the glaze layer, the present technical solution sets a mold texture layer between the body layer and the first bottom glaze layer, and uses the mutual repulsion between the mold ink and the bottom glaze to form a mold texture with a concave-convex effect, thereby enhancing the concave-convex effect of the glaze layer.
[0055] Therefore, in this technical solution, the concave effect formed by the glaze formula itself and the concave-convex effect formed by the mutual repulsion between the base glaze and the mold ink are coordinated to make the pearlescent fantasy glaze layer produce a larger thickness deviation, which greatly promotes the pearlescent particles of cerium oxide-wrapped fluorphlogopite with different refractive indices in the inner and outer layers to produce stronger reflection, refraction and interference under light conditions, thereby presenting an extremely strong pearlescent fantasy glitter effect.
[0056] It should be noted that the dry particle positioning frit of the present technical solution contains a large amount of flux I, so that the dry particle positioning frit can reduce the firing temperature of the base glaze while increasing the pearlescent and colorful flashing effect, avoiding the base glaze from being fired raw and affecting its performance. In addition, the base glaze formula also contains potassium feldspar and wollastonite with fluxing effect, which cooperate with the fluxing effect of the dry particle positioning frit, which is more conducive to promoting the low-temperature firing of the base glaze.
[0057] Furthermore, the present technical solution also specially adds nepheline to the raw material formula of the base glaze. Compared with conventional potassium and sodium feldspar, nepheline has a smaller expansion coefficient. The introduction of a large amount of nepheline can adjust the expansion coefficient of the base glaze, so that the expansion coefficients of the first base glaze layer and the body layer match each other, thereby avoiding cracking of the glazed tiles after firing in the kiln, and ensuring the hardness and anti-fouling properties of the glazed tiles.
[0058] Therefore, the technical scheme optimizes the base glaze formula and the pearlescent glaze formula, utilizes the strong and uniform pearlescent effect of the pearlescent glaze formula, the whitening effect of the base glaze formula on the body layer, and the concave effect formed by the base glaze formula itself cooperates with the concave and convex effect formed by the mutual repulsion between the base glaze and the mold ink. On the premise of ensuring complete covering of the body layer and avoiding the influence of the depth of the body layer on the pearlescent fantasy glitter effect, it is beneficial to present a strong and uniform pearlescent fantasy glitter effect on the surface of the glazed tile.
[0059] Preferably, in step C, the flux I comprises potassium feldspar, sodium feldspar, calcined talc, barium carbonate, wollastonite and zinc oxide;
[0060] Calculated by weight, the dry particle positioning frit glaze includes the following raw materials: 8 to 15 parts of quartz, 5 to 12 parts of aluminum oxide, 10 to 15 parts of zircon powder, 30 to 40 parts of potassium feldspar, 8 to 15 parts of sodium feldspar, 2 to 5 parts of calcined talc, 1 to 4 parts of barium carbonate, 5 to 15 parts of wollastonite, 3 to 8 parts of zinc oxide, and 5 to 10 parts of lead carbonate.
[0061] Potassium feldspar, sodium feldspar, burnt talc, wollastonite and zinc oxide all have the effect of reducing the firing temperature and promoting sintering. In addition, barium carbonate can increase the transparency and glossiness of the frit, and zinc oxide can be used as a nucleus former to reduce the crystallization activation energy and crystallization peak temperature, which is beneficial to the crystallization of oxidation. Therefore, in a preferred embodiment of the present technical solution, flux I includes potassium feldspar, sodium feldspar, burnt talc, barium carbonate, wollastonite and zinc oxide, and the addition amount of the above raw materials in the dry particle positioning frit glaze is limited to ensure the high temperature viscosity and transparency of the dry particle positioning layer.
[0062] Preferably, calculated by weight, the dry particle positioning frit glaze includes the following raw materials: 10 parts of quartz, 8 parts of aluminum oxide, 12 parts of zircon powder, 35 parts of potassium feldspar, 10 parts of sodium feldspar, 3 parts of calcined talc, 2 parts of barium carbonate, 8 parts of wollastonite, 6 parts of zinc oxide and 6 parts of lead carbonate.
[0063] Preferably, in step D, the flux II comprises zinc oxide and lithium carbonate, and the mixing ratio of the zinc oxide to the lithium carbonate is (0.8-1.2):1 calculated by mass ratio;
[0064] The phase separation agent is calcium phosphate;
[0065] Calculated by mass percentage, the chemical composition of the pearlescent colorful sparkling frit includes SiO2 47-48%, Al2O3 19-22%, Fe2O3 0.2-0.5%, CaO 5-6%, MgO 10-12%, K2O 7-8.5%, ZnO 4.4-4.5%, Na2O 0.02-0.03%, CeO 6-8% and P2O5 3.5-4.5%.
[0066] Both zinc oxide and lithium carbonate have good effects of reducing the firing temperature and promoting sintering. Therefore, in a preferred embodiment of the present technical solution, flux II includes zinc oxide and lithium carbonate, and the mixing ratio of zinc oxide and lithium carbonate is limited to promote high-temperature calcination of the frit, thereby ensuring its pearlescent and colorful flashing effect. In addition, in addition to its fluxing effect, zinc oxide can, on the one hand, act as a nucleus former, reduce the crystallization activation energy and crystallization peak temperature, and is beneficial to the crystallization of cerium oxide, thereby further enhancing the pearlescent and colorful flashing effect; on the other hand, it can also improve the anti-fouling performance.
[0067] Calcium phosphate can produce phosphorus pentoxide when calcined. Due to its high coordination number and strong cationic field, phosphorus pentoxide is easily separated from the glass phase network structure during heat treatment, resulting in phase separation. Phase separation promotes the enrichment of cerium oxide in the pearlescent colorful flash frit, making it easier for cerium oxide crystals to precipitate, which is more conducive to improving the pearlescent colorful flash effect of the pearlescent colorful flash frit. In addition, calcium phosphate can also produce calcium oxide when calcined. Calcium oxide can also play a fluxing effect, which is conducive to reducing the calcination temperature of the frit, allowing the frit to be calcined completely, and ensuring the pearlescent colorful flash effect of the pearlescent colorful flash frit.
[0068] In another preferred embodiment of the present technical solution, a pearlescent colorful sparkling frit is selected, whose chemical composition includes SiO2 47-48%, Al2O3 19-22%, Fe2O3 0.2-0.5%, CaO 5-6%, MgO 10-12%, K2O 7-8.5%, ZnO 4.4-4.5%, Na2O 0.02-0.03%, CeO 6-8% and P2O5 3.5-4.5%, calculated by mass percentage, wherein the SiO2 content is as high as 47-48%, which is a high-silicon frit, and is beneficial to ensuring the hardness and wear resistance of the frit.
[0069] Further description, step F is also included, and step F is located between step A and step B;
[0070] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank layer after drying;
[0071] F. Applying a base glaze on the surface of the green body layer to obtain a second base glaze layer; wherein the amount of the base glaze applied is 45-55 g / cm 3 , specific gravity is 1.85~1.90;
[0072] B. Using mold ink, inkjet printing is performed on the surface of the second base glaze layer according to a preset pattern to obtain a mold texture layer.
[0073] In a preferred embodiment of the present technical solution, a second base glaze layer is formed by pouring base glaze on the top of the mold ink. The second base glaze layer cooperates with the first base glaze layer to further cover the body layer, thereby avoiding the limited white-shielding effect of the first base glaze layer affecting the pearlescent fantasy sparkling effect. At the same time, the second base glaze layer can also enhance the concave and convex effect of the glaze layer, further highlighting the pearlescent fantasy sparkling effect.
[0074] In addition, compared with the spraying process, the pouring process is conducive to forming a thicker glaze layer, improving the covering effect of the body layer and the concave-convex effect of the glaze layer. Therefore, in a preferred embodiment of the present technical solution, the second bottom glaze layer adopts the pouring process, and the pouring amount and specific gravity of the bottom glaze are limited to enhance the pearlescent magic color flash effect, which is more in line with the actual use needs and improves the added value of the glazed tile.
[0075] Preferably, the method further comprises step G, and step G is located between step C and step D;
[0076] C. applying a base glaze to the surface of the mold texture layer to obtain a first base glaze layer;
[0077] G. Printing color ink on the surface of the first base glaze layer according to a preset pattern to obtain a color pattern layer;
[0078] D. Applying the pearlescent colorful glaze on the surface of the color pattern layer to obtain the pearlescent colorful glaze layer.
[0079] In a preferred embodiment of the present technical solution, in order to enhance the decorative effect of the pearlescent iridescent glazed tiles, a color pattern layer may be added between the first base glaze layer and the pearlescent iridescent glaze layer, so that the color of the color pattern layer can be presented on the glaze surface of the glazed tiles through the pearlescent iridescent glaze layer, so as to better meet the viewing needs of consumers.
[0080] Further, in step C, calculated by mass percentage, the content of zirconium oxide in the zirconium silicate is 60-65%, and the content of zirconium oxide in the zircon powder is 70-85%.
[0081] The present technical scheme preferably uses zirconium silicate with a zirconium oxide content of 60-65% as the formula raw material for the base glaze, and zircon powder with a zirconium oxide content of 70-85% as the formula raw material for the dry particle positioning frit, which is more conducive to promoting the formation of zirconium oxide crystals in the glaze layer and more conducive to improving the pearlescent fantasy and sparkling effect.
[0082] Further, in step C, the particle size distribution of the dry particle positioning frit is as follows: the residue on a 100-mesh sieve is 0.1-0.5%, the residue on a 120-mesh sieve is 40-50%, and the residue on a 140-mesh sieve is 70-80%.
[0083] In a preferred embodiment of the present technical solution, by optimizing the particle grading of the dry particle positioning frit, the following effects are achieved: first, it is helpful to improve the fluidity of the dry particle positioning frit, thereby improving the convenience and stability of base glaze application; second, it is helpful to increase the firing temperature of the dry particle positioning frit, thereby increasing the firing temperature of the base glaze, lowering the melting boundary of the base glaze, enhancing the three-dimensional concave-convex effect, and helping to highlight the pearlescent fantasy and glittering effect.
[0084] It should be noted that the particle gradation of the dry particle positioning frit refers to the particle gradation formed after the dry particle positioning frit is dried and crushed into powder by a crusher.
[0085] Further explanation, in step C, the firing curve of the dry particle positioning frit is:
[0086] It takes 1.5 to 3 hours to heat from room temperature to 500°C;
[0087] It takes 0.5 to 1.5 hours to raise the temperature from 500°C to 1100°C;
[0088] It takes 0.4 to 1 h to heat from 1100°C to 1530°C;
[0089] 1530℃, keep warm for 0.5~1.2h.
[0090] In a preferred embodiment of the present technical solution, the firing curve of the dry particle positioning frit is optimized to help ensure its relevant performance.
[0091] Further, in step C, the base glaze is applied by spraying, and according to the mass percentage, the base glaze is passed through a 250-mesh sieve, the sieve residue is 0.5-0.7%, and the spraying amount is 55-60 g / cm 3 , specific gravity is 1.52~1.60;
[0092] In step D, according to the mass percentage, the residue of the pearlescent colorful glaze after passing through a 325-mesh sieve is 0.3-0.5%, and the glazing amount is 23-27 g / cm 3 , specific gravity is 1.28~1.32.
[0093] In a preferred embodiment of the present technical solution, the glazing method in step C is limited to spraying, which is beneficial to ensure the covering effect of the green body layer and the concave-convex effect of the first base glaze layer while reducing the amount of base glaze and thus reducing production costs, thereby highlighting the pearlescent and colorful sparkling effect of the glaze surface.
[0094] In addition, in order to obtain better pearlescent fantasy glitter effect, this technical solution adjusts the fineness, spraying amount and specific gravity of the base glaze and pearlescent fantasy glitter glaze, so that the base glaze and pearlescent fantasy glitter glaze cooperate with each other to ensure that the glazed tiles have better pearlescent fantasy glitter effect, while improving the quality and stability of the glazed tiles.
[0095] Further, in step D, the method for preparing the pearlescent colorful sparkling frit comprises the following steps:
[0096] D1. After cerium oxide and perlite are uniformly mixed according to the ratio, water is added to mix to obtain a mixture I; the mixture I is sent to a pelletizer, and after drying, granules I are obtained;
[0097] D2. After quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are uniformly mixed according to the proportion, water is added to mix to obtain a mixture II; the mixture II is fed into a pelletizing machine, and after drying, granules II are obtained;
[0098] D3. After the particles I and II are evenly mixed, a phase separation agent and a flux in a prescribed amount are added, mixed and fired at a high temperature. After water quenching, cooling and drying, a pearlescent colorful sparkling melt is obtained.
[0099] The technical solution also proposes a method for preparing a pearlescent colorful sparkling frit, which has simple steps and strong operability, and is conducive to ensuring the relevant properties of soft porcelain during the preparation process.
[0100] Specifically, in the technical scheme, cerium oxide and perlite are first mixed evenly according to a ratio, water is added for mixing to obtain mixture I, mixture I is sent to a ball-forming machine, and granules I are obtained after drying; quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are then mixed evenly according to a ratio, water is added for mixing to obtain mixture II, mixture II is sent to a ball-forming machine, and granules II are obtained after drying, thereby reducing the interface contact area between different raw materials and reducing the mutual penetration between glass phases during the sintering process of the frit, thereby ensuring the precipitation amount of cerium oxide-coated fluorphlogopite pearlescent particles and ensuring the pearlescent and colorful sparkling effect of the frit.
[0101] Preferably, in step C, the temperature curve of the high temperature firing is:
[0102] It takes 1.5 to 3 hours to rise from room temperature to 500°C;
[0103] It takes 1.5 to 2.5 hours to increase the temperature from 500°C to 1100°C;
[0104] From 1100℃ to 1530℃, it takes 0.2~0.4h;
[0105] 1530℃, keep warm for 0.1~0.2h;
[0106] It takes 0.05 to 0.2 hours to reduce the temperature from 1500°C to 1400°C.
[0107] 1400℃, keep warm for 0.2~0.4h.
[0108] In a preferred embodiment of the present technical solution, the temperature curve of the high-temperature firing of the pearlescent colorful sparkling frit is optimized, which is helpful to ensure the pearlescent colorful sparkling effect of the pearlescent colorful sparkling frit.
[0109] Specifically, the pearlescent fantasy sparkle frit is kept at 1530°C for 0.1 to 0.2 h during the high-temperature firing process. If the holding time is too long, the glass content of the frit will increase significantly, destroying the layered structure of perlite and fluorophlogopite, and the pearlescent fantasy sparkle effect will deteriorate. If the holding time is too short, the synthesis amount of fluorophlogopite will be small, and the pearlescent fantasy sparkle effect will also deteriorate.
[0110] More specifically, it takes 0.05 to 0.2 hours for the pearlescent fantasy glitter frit to cool from 1500°C to 1400°C during the high-temperature firing process. If the cooling time is too short, the fluorophlogopite is not completely wrapped, the precipitation amount of cerium oxide-wrapped fluorophlogopite pearlescent particles is reduced, and the pearlescent fantasy glitter effect is deteriorated. If the cooling time is too long, the long-term cooling causes the viscosity of the pearlescent fantasy glitter frit to decrease uniformly, which is not conducive to the wrapping of fluorophlogopite by cerium oxide crystals. The precipitation amount of cerium oxide-wrapped fluorophlogopite pearlescent particles is also reduced, and the pearlescent fantasy glitter effect is also deteriorated.
[0111] More preferably, in step C, the temperature curve of the high temperature firing is as follows:
[0112] It takes 2h to rise from room temperature to 500℃;
[0113] It takes 2h to increase the temperature from 500℃ to 1100℃;
[0114] From 1100℃ to 1530℃, it takes 0.3h;
[0115] 1530℃, keep warm for 0.16h;
[0116] It takes 0.1h to reduce the temperature from 1500℃ to 1400℃;
[0117] 1400℃, keep warm for 0.3h.
[0118] In a more preferred embodiment of the present technical solution, the temperature curve of the high-temperature firing of the frit is further optimized so that the temperature curve of the high-temperature firing is optimized, which is beneficial to ensure that the pearlescent colorful flash effect of the frit is optimal.
[0119] Further, in step D, the mesh size of the cerium oxide is 300-325 meshes, the mesh size of the perlite is 300-325 meshes, and the mesh size of the fused magnesia is 380-400 meshes.
[0120] When the mesh size of cerium oxide is too large, it is easy to increase the roughness of the pearlescent particles of cerium oxide-wrapped fluorphlogopite, thereby affecting the uniformity of the pearlescent colorful flash effect. When the mesh size of cerium oxide is too small, it is easy to increase the difficulty of grinding, reduce production efficiency, and increase production costs. Therefore, in a preferred embodiment of the present technical solution, the mesh size of cerium oxide is limited to ensure the uniformity of the pearlescent colorful flash effect at a lower cost. At the same time, by limiting the mesh size of perlite and fused magnesia, it is beneficial to improve the intensity and uniformity of the pearlescent colorful flash effect.
[0121] Further description, in step C, calculated by weight, the base glaze includes the following raw materials: 6 parts of kaolin, 10 parts of quartz, 5 parts of alumina, 25 parts of nepheline, 27 parts of potassium feldspar, 5 parts of wollastonite, 5 parts of dry particle positioning frit and 20 parts of zirconium silicate.
[0122] In a preferred embodiment of the present technical solution, by optimizing the base glaze formula, it is helpful to enhance the concave-convex effect of the glaze layer while covering the body layer as much as possible, so as to achieve the best pearlescent and colorful sparkling effect of the glaze surface.
[0123] The pearlescent colorful glittering glazed tile with concave and convex effects is prepared by using the preparation method of the pearlescent colorful glittering glazed tile with concave and convex effects.
[0124] This plan also proposes pearlescent iridescent glazed tiles with concave and convex effects. In addition to having a strong and uniform pearlescent iridescent effect, the glazed tiles also have good hardness and anti-fouling properties, combining both decorativeness and practicality, which is more conducive to meeting the usage needs of consumers.
[0125] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0126] Example 1
[0127] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank layer after drying;
[0128] B. Using mold ink to perform inkjet printing on the surface of the green body layer according to a preset pattern to obtain a mold texture layer;
[0129] C. Spray the base glaze on the surface of the mold texture layer to obtain the first base glaze layer; wherein, according to the mass percentage, the base glaze is passed through a 250-mesh sieve, the sieve residue is 0.5%, and the spraying amount of the base glaze is 58g / cm 3 , with a specific gravity of 1.55; calculated by weight, the base glaze includes the following raw materials: 6 parts of kaolin, 10 parts of quartz, 5 parts of alumina, 25 parts of nepheline, 35 parts of potassium feldspar, 5 parts of wollastonite, 5 parts of dry particle positioning frit and 20 parts of zirconium silicate with a zirconium oxide content of 60-65%; calculated by weight, the dry particle positioning frit includes the following raw materials: 10 parts of quartz, 8 parts of alumina, 12 parts of zircon powder with a zirconium oxide content of 70%, 35 parts of potassium feldspar, 10 parts of sodium feldspar, 3 parts of calcined talc, 2 parts of barium carbonate, 8 parts of wollastonite, 6 parts of zinc oxide and 6 parts of lead carbonate; the particle grading of the dry particle positioning frit is: the sieve residue of 100 mesh is 0.1%, the sieve residue of 120 mesh is 40%, and the sieve residue of 140 mesh is 80%;
[0130] D. Applying the pearlescent colorful glaze to the surface of the first base glaze layer to obtain a pearlescent colorful glaze layer; wherein, according to the mass percentage, the pearlescent colorful glaze has a 0.3% residue after passing through a 325-mesh sieve, and the glaze application amount is 25 g / cm 3, with a specific gravity of 1.3; calculated by weight, the pearlescent iridescent glaze includes the following raw materials: 5 parts of kaolin, 95 parts of pearlescent iridescent frit, 0.2 parts of sodium carboxymethyl cellulose, 0.3 parts of sodium tripolyphosphate and 40 parts of water; calculated by weight, the pearlescent iridescent frit includes the following raw materials: 10 parts of perlite with a mesh number of 300, 32 parts of quartz, 10 parts of alumina, 15 parts of fused magnesia with a mesh number of 400, 5 parts of potassium fluorosilicate, 10 parts of potassium nitrate, 8 parts of calcium phosphate, 6 parts of cerium oxide with a mesh number of 325, 4 parts of zinc oxide and 5 parts of lithium carbonate;
[0131] E. After drying, the tiles are put into kiln for firing to obtain pearlescent colorful glazed tiles with double concave and convex effects.
[0132] Example 2
[0133] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank layer after drying;
[0134] B. Using mold ink to perform inkjet printing on the surface of the green body layer according to a preset pattern to obtain a mold texture layer;
[0135] C. Spray the base glaze on the surface of the mold texture layer to obtain the first base glaze layer; wherein, the base glaze is sieved through a 250-mesh sieve, the sieve residue is 0.5-0.7%, and the spraying amount of the base glaze is 58g / cm 3 , with a specific gravity of 1.55; calculated by weight, the base glaze includes the following raw materials: 6 parts of kaolin, 6 parts of quartz, 8 parts of alumina, 30 parts of nepheline, 25 parts of potassium feldspar, 8 parts of wollastonite, 3 parts of dry particle positioning frit and 15 parts of zirconium silicate with a zirconium oxide content of 60-65%; calculated by weight, the dry particle positioning frit includes the following raw materials: 8 parts of quartz, 12 parts of alumina, 13 parts of zircon powder with a zirconium oxide content of 75%, 38 parts of potassium feldspar, 15 parts of sodium feldspar, 5 parts of calcined talc, 4 parts of barium carbonate, 8 parts of wollastonite, 6 parts of zinc oxide and 7 parts of lead carbonate; the particle grading of the dry particle positioning frit is: the residue on the 100-mesh sieve is 0.5%, the residue on the 120-mesh sieve is 50%, and the residue on the 140-mesh sieve is 70% of the dry particle positioning frit;
[0136] D. Applying the pearlescent colorful glaze to the surface of the first base glaze layer to obtain the pearlescent colorful glaze layer; wherein, according to the mass percentage, the pearlescent colorful glaze layer has a 0.5% residue after passing through a 325-mesh sieve, and the glaze application amount is 23 g / cm 3, with a specific gravity of 1.28; calculated by weight, the pearlescent iridescent glaze includes the following raw materials: 4 parts of kaolin, 96 parts of pearlescent iridescent frit, 0.5 parts of sodium carboxymethyl cellulose, 0.2 parts of sodium tripolyphosphate and 45 parts of water; calculated by weight, the pearlescent iridescent frit includes the following raw materials: 20 parts of perlite with a mesh number of 325, 25 parts of quartz, 8 parts of alumina, 18 parts of fused magnesia with a mesh number of 380, 8 parts of potassium fluorosilicate, 8 parts of potassium nitrate, 10 parts of calcium phosphate, 10 parts of cerium oxide with a mesh number of 325, 6 parts of zinc oxide and 5 parts of lithium carbonate;
[0137] E. After drying, the tiles are put into kiln for firing to obtain pearlescent colorful glazed tiles with double concave and convex effects.
[0138] Example 3
[0139] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank layer after drying;
[0140] F. Apply the base glaze on the surface of the body layer to obtain a second base glaze layer; wherein the base glaze is applied in an amount of 55 g / cm 3 , specific gravity is 1.90;
[0141] B. Using mold ink to perform inkjet printing on the surface of the second base glaze layer according to a preset pattern to obtain a mold texture layer;
[0142] C. Spray the base glaze on the surface of the mold texture layer to obtain a first base glaze layer; wherein, according to the mass percentage, the base glaze is passed through a 250-mesh sieve, the sieve residue is 0.5%, and the spraying amount of the base glaze is 55g / cm 3 , specific gravity is 1.60; calculated by weight, the base glaze of step F and step C includes the following raw materials: kaolin: 8 parts, quartz: 15 parts, alumina: 3 parts, nepheline: 20 parts, potassium feldspar: 35 parts, wollastonite: 7 parts, dry particle positioning frit: 5 parts and zirconium silicate: 21 parts with zirconium oxide content of 60-65%; calculated by weight, the dry particle positioning frit includes the following raw materials: quartz: 15 parts, alumina: 8 parts, zircon powder: 15 parts with zircon oxide content of 85%, potassium feldspar: 30 parts, sodium feldspar: 8 parts, talc: 2 parts, barium carbonate: 1 part, wollastonite: 15 parts, zinc oxide: 8 parts and lead carbonate: 10 parts; the particle grading of the dry particle positioning frit is 0.5% on the 100 mesh sieve, 50% on the 120 mesh sieve and 70% on the 140 mesh sieve;
[0143] D. Applying the pearlescent colorful glaze to the surface of the first base glaze layer to obtain a pearlescent colorful glaze layer; wherein, according to the mass percentage, the pearlescent colorful glaze has a 0.4% residue after passing through a 325-mesh sieve, and the glaze application amount is 27 g / cm 3, with a specific gravity of 1.28; calculated by weight, the pearlescent iridescent glaze includes the following raw materials: 4 to 8 parts of kaolin, 92 parts of pearlescent iridescent frit, 0.3 parts of sodium carboxymethyl cellulose, 0.4 parts of sodium tripolyphosphate and 3545 parts of water; calculated by weight, the pearlescent iridescent frit includes the following raw materials: 20 parts of perlite with a mesh number of 325, 25 parts of quartz, 8 parts of alumina, 18 parts of fused magnesia with a mesh number of 380, 8 parts of potassium fluorosilicate, 8 parts of potassium nitrate, 10 parts of calcium phosphate, 10 parts of cerium oxide with a mesh number of 325, 6 parts of zinc oxide and 5 parts of lithium carbonate;
[0144] E. After drying, the tiles are put into kiln for firing to obtain pearlescent colorful glazed tiles with double concave and convex effects.
[0145] Comparative Example 1
[0146] The preparation method and raw materials of Comparative Example 1 are the same as those of Example 1, except that the first base glaze layer is not provided in Comparative Example 1.
[0147] Comparative Example 2
[0148] The preparation method and raw materials of Comparative Example 2 are the same as those of Example 1, except that no mold ink layer is provided in Comparative Example 2.
[0149] The glazed tiles prepared in Examples 1-3 and Comparative Examples 1-2 were respectively subjected to conventional hardness, glossiness and antifouling grade tests in the field of architectural ceramics. The results are shown in Table 1 below:
[0150]
[0151] It can be seen from the performance test results in Table 1 that the glazed tiles obtained by the present technical solution not only have a strong and uniform pearlescent fantasy flash effect, but also have good hardness and anti-fouling properties, and are both decorative and practical, which is more conducive to meeting the use needs of consumers.
[0152] In Comparative Example 1, since the first base glaze layer is not provided, the glazed tiles obtained by Comparative Example 1 have a weak pearlescent colorful glitter effect and a darker glaze color.
[0153] In Comparative Example 2, since the mold ink layer is not set, it is not conducive to the glaze layer to form a deeper concave-convex effect. Although the first base glaze layer is set in Comparative Example 1, the pearlescent fantasy color glitter effect of the obtained glazed tiles is slightly weaker and the pearlescent fantasy color glitter effect is average.
[0154] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.
Claims
1. A method for preparing pearlescent colorful glazed tiles with concave and convex effects, characterized in that: The following steps are involved: A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank layer after drying; B. inkjet printing is performed on the surface of the green body layer according to a preset pattern using mold ink to obtain a mold texture layer; C. Applying a base glaze to the surface of the mold texture layer to obtain a first base glaze layer; the base glaze comprises the following raw materials, calculated by weight: 4-8 parts of kaolin, 5-15 parts of quartz, 3-8 parts of alumina, 20-30 parts of nepheline, 25-35 parts of potassium feldspar, 3-8 parts of wollastonite, 3-8 parts of dry particle positioning frit and 15-21 parts of zirconium silicate; the dry particle positioning frit comprises the following raw materials, calculated by weight: 8-15 parts of quartz, 5-12 parts of alumina, 10-15 parts of zircon powder, 5-10 parts of lead carbonate and 49-87 parts of flux I; D. Applying a pearlescent colorful glitter glaze to the surface of the first base glaze layer to obtain a pearlescent colorful glitter glaze layer; the pearlescent colorful glitter glaze comprises the following raw materials, calculated by weight: 4-8 parts of kaolin, 92-96 parts of pearlescent colorful glitter frit, 0.2-0.5 parts of sodium carboxymethyl cellulose, 0.2-0.4 parts of sodium tripolyphosphate and 35-45 parts of water; the pearlescent colorful glitter frit comprises the following raw materials, calculated by weight: 8-20 parts of perlite, 25-35 parts of quartz, 8-15 parts of alumina, 10-18 parts of fused magnesia, 3-8 parts of potassium fluorosilicate, 8-15 parts of potassium nitrate, 5-10 parts of a phase separator, 5-10 parts of cerium oxide and 6-16 parts of flux II; the essence of the pearlescent colorful glitter frit is cerium oxide wrapped in fluorphlogopite glass; E. After drying, the tiles are put into kiln for firing to obtain pearlescent colorful glazed tiles with double concave and convex effects.
2. The method for preparing the pearlescent colorful glazed tile with concave and convex effects according to claim 1, characterized in that: The method further comprises step F, wherein step F is located between step A and step B; A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank layer after drying; F. Applying a base glaze on the surface of the green body layer to obtain a second base glaze layer; wherein the amount of the base glaze applied is 45-55 g / cm 3 , specific gravity is 1.85~1.90; B. Using mold ink, inkjet printing is performed on the surface of the second base glaze layer according to a preset pattern to obtain a mold texture layer.
3. The method for preparing the pearlescent colorful glazed tile with concave and convex effects according to claim 1, characterized in that: In step C, calculated by mass percentage, the content of zirconium oxide in the zirconium silicate is 60-65%, and the content of zirconium oxide in the zircon powder is 70-85%.
4. The method for preparing the pearlescent colorful glazed tile with concave and convex effects according to claim 1, characterized in that: In step C, the particle size distribution of the dry particle positioning frit is as follows: the residue on a 100-mesh sieve is 0.1-0.5%, the residue on a 120-mesh sieve is 40-50%, and the residue on a 140-mesh sieve is 70-80%.
5. The method for preparing the pearlescent colorful glazed tile with concave and convex effects according to claim 1, characterized in that: In step C, the firing curve of the dry particle positioning frit is: It takes 1.5 to 3 hours to heat from room temperature to 500°C; It takes 0.5 to 1.5 hours to raise the temperature from 500°C to 1100°C; It takes 0.4 to 1 h to heat from 1100°C to 1530°C; 1530℃, keep warm for 0.5~1.2h.
6. The method for preparing the pearlescent colorful glazed tile with concave and convex effects according to claim 1, characterized in that: In step C, the base glaze is applied by spraying, and according to the mass percentage, the base glaze is passed through a 250-mesh sieve, the sieve residue is 0.5-0.7%, and the spraying amount is 55-60 g / cm 3 , specific gravity is 1.52~1.60; In step D, according to the mass percentage, the residue of the pearlescent colorful glaze after passing through a 325-mesh sieve is 0.3-0.5%, and the glazing amount is 23-27 g / cm 3 , specific gravity is 1.28~1.
32.
7. The method for preparing the pearlescent colorful glazed tile with concave and convex effects according to claim 1, characterized in that: In step D, the method for preparing the pearlescent colorful sparkling frit comprises the following steps: D1. After cerium oxide and perlite are uniformly mixed according to the ratio, water is added to mix to obtain a mixture I; the mixture I is sent to a pelletizer, and after drying, granules I are obtained; D2. After quartz, alumina, fused magnesia, potassium fluorosilicate and potassium nitrate are uniformly mixed according to the proportion, water is added to mix to obtain a mixture II; the mixture II is fed into a pelletizing machine, and after drying, granules II are obtained; D3. After the particles I and II are evenly mixed, a phase separation agent and a flux in a prescribed amount are added, mixed and fired at a high temperature. After water quenching, cooling and drying, a pearlescent colorful sparkling melt is obtained.
8. The method for preparing the pearlescent colorful glazed tile with concave and convex effects according to claim 1, characterized in that: In step D, the mesh number of the cerium oxide is 300-325 meshes, the mesh number of the perlite is 300-325 meshes, and the mesh number of the fused magnesia is 380-400 meshes.
9. The method for preparing the pearlescent colorful glazed tile with concave and convex effects according to claim 1, characterized in that: In step C, the base glaze includes the following raw materials, calculated by weight: 6 parts of kaolin, 10 parts of quartz, 5 parts of alumina, 25 parts of nepheline, 27 parts of potassium feldspar, 5 parts of wollastonite, 5 parts of dry particle positioning frit and 20 parts of zirconium silicate.
10. Pearlescent colorful glazed tiles with concave and convex effects, characterized in that: The pearlescent colorful glazed tile with concave and convex effects is prepared using the preparation method of any one of claims 1 to 9.