A corrosion-resistant magnesium alloy and a method for preparing the same

By adding 0.3-0.9% Sr element to the magnesium alloy and controlling the pouring and cooling conditions, the Al4Sr phase is formed, which solves the problem of poor corrosion resistance of the magnesium alloy and improves the hardness and corrosion resistance, especially on the bottom and top surfaces. Corrosion resistant layer.

CN118563149BActive Publication Date: 2024-10-18GUANGZHOU ZHONGSHAN FASTENER CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411060655.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-18
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The corrosion resistance of magnesium alloy materials is poor, especially when the aluminum content is less than 9%, β-Mg17Al12 acts as a corrosion cathode to accelerate the corrosion of magnesium alloys, and Sr higher than 0.9% will cause the crystal nucleus to coarsen and affect the hardness.

Method used

Add 0.3-0.9% Sr element to the magnesium alloy, and control the pouring rate and cooling rate through a semi-solid slurry preparation method to form a high liquid phase region to promote the distribution of Al and Sr and form more Al4Sr phases, thereby Improve the corrosion resistance of magnesium alloys.

Benefits of technology

Through the preparation method, the hardness of the magnesium alloy is not only improved, but also has good corrosion resistance. In particular, the Al4Sr phase on the bottom and top surfaces is significantly enhanced, extending the service life of the magnesium alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563149B_ABST
    Figure CN118563149B_ABST
Patent Text Reader

Abstract

The invention provides a corrosion-resistant magnesium alloy and a preparation method thereof. The preparation method comprises the following steps: adding pure metal into a resistance furnace for smelting according to the composition of an alloy to be prepared to obtain a melt at a temperature of 720-850°C, adding a magnesium intermediate alloy containing Sr and stirring and mixing uniformly so that the mass fraction of Sr in the melt is 0.3-0.9%, transferring the melt into a first container, stirring and cooling the melt to form a semi-solid magnesium alloy slurry, and when the solid content of the semi-solid magnesium alloy slurry is 30-50%, pouring the semi-solid magnesium alloy slurry into a mold, and performing die casting after the pouring is completed to obtain the corrosion-resistant magnesium alloy. The pouring comprises: a first pouring and a second pouring, the first pouring rate is 0.005-0.02 kg / s, the second pouring rate is 0.1-0.2 kg / s, and the mass ratio of the slurry poured for the first time to the slurry poured for the second time is (0.5-3):(92-99.5). As such, the magnesium alloy has improved hardness, and the bottom surface has improved corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semi-solid alloy manufacturing, and in particular to a corrosion-resistant magnesium alloy and a preparation method thereof. Background Art

[0002] In the 1970s, American scientists discovered that applying strong shear force to a metal solution in a semi-solid temperature range can produce a solid-liquid mixed slurry, namely a semi-solid slurry. The semi-solid slurry has a certain viscosity and can flow laminarly in the mold to avoid air entanglement. The temperature of the semi-solid slurry is relatively low, which can extend the life of the mold. The material prepared by the semi-solid slurry has improved mechanical properties. Applying it to magnesium alloy materials can improve the problem of low strength of magnesium alloy materials. However, it cannot improve the corrosion resistance of magnesium alloy materials. The corrosion resistance of magnesium alloys is closely related to their composition. Some elements have a two-sided effect on the corrosion resistance of magnesium alloys. For example, the aluminum content in magnesium alloys has a greater influence on the corrosion resistance of magnesium alloys. When the aluminum content is higher than 9%, the β-Mg 17 Al 12 It can act as a corrosion barrier to prevent the corrosion of magnesium alloys. When the aluminum content is less than 9%, β-Mg 17 Al 12 As a corrosion cathode, it accelerates the corrosion of magnesium alloys. When the mass fraction of Sr in magnesium alloys is 0.3-0.9%, it can promote the grain refinement of magnesium alloys, thereby improving the corrosion resistance of magnesium alloys. When the mass fraction of Sr is 0.5-0.9%, Sr can react with Al to form a highly stable Al4Sr phase, further improving the corrosion resistance of magnesium alloys. When the mass fraction of Sr in magnesium alloys is higher than 0.9%, Sr can react with Al to form more Al4Sr phases, but too much Sr will cause the crystal nucleus to coarsen, affecting the hardness of magnesium alloys.

[0003] Therefore, it is necessary to provide a corrosion-resistant magnesium alloy and a preparation method thereof. Summary of the invention

[0004] Based on this, it is necessary to provide a corrosion-resistant magnesium alloy and a preparation method thereof.

[0005] A first aspect of the present invention provides a method for preparing a corrosion-resistant magnesium alloy, comprising the following steps:

[0006] According to the composition of the alloy to be prepared, pure metal is added to a resistance furnace for melting to obtain a melt with a temperature of 720-850°C, a magnesium intermediate alloy containing Sr is added and stirred and mixed evenly, so that the mass fraction of Sr in the melt is 0.3-0.9%, the melt is transferred to a first container, and the melt is stirred and cooled to form a semi-solid magnesium alloy slurry. When the solid content of the semi-solid magnesium alloy slurry is 30-50%, the semi-solid magnesium alloy slurry is poured into a mold, and after the pouring is completed, die casting is performed to obtain the corrosion-resistant magnesium alloy. The pouring includes: a first pouring and a second pouring, the first pouring rate is 0.005-0.02kg / s, the second pouring rate is 0.1-0.2kg / s, and the mass ratio of the slurry of the first pouring to the slurry of the second pouring is (0.5-3): (92-99.5).

[0007] The present application adds 0.3-0.9% Sr element by mass fraction to the magnesium alloy. The Sr element in the above proportion can promote grain refinement in the preparation process of semi-solid magnesium alloy slurry, and can improve the hardness of the magnesium alloy. By reducing the rate of the first pouring, the liquid phase has a faster flow speed than the solid phase, so that solid-liquid phase separation occurs. The slurry poured for the first time has a higher liquid phase ratio, so that a high liquid phase area is formed at the bottom of the mold, and Al and Sr elements tend to be distributed in the liquid phase, and Mg in the liquid phase decreases with the increase of solid content. In this way, the slurry poured for the first time has a higher concentration of Al and Sr. The high concentration of Al and Sr can form more Al4Sr phases on the bottom surface of the magnesium alloy (i.e., the bottom surface of the mold) during the cooling process, thereby improving the corrosion resistance of the bottom surface of the magnesium alloy material. In this way, the above-mentioned magnesium alloy has improved hardness, and the bottom surface has improved corrosion resistance. Some castings have different performance requirements for different surfaces. For example, the contact surface between the casting and the liquid needs to be a corrosion-resistant surface. Applying the above-mentioned magnesium alloy to the above-mentioned casting and making the bottom surface of the magnesium alloy as the corrosion-resistant surface can further improve the corrosion resistance of the above-mentioned casting.

[0008] Furthermore, it comprises three pourings: after the second pouring is completed, the remaining semi-solid magnesium alloy slurry is passed through a ceramic filter with a pore size of 50-100 μm and then enters the mold, and the mass ratio of the remaining semi-solid magnesium alloy slurry to the second pouring slurry is (1-5): (92-98.5). As the pouring proceeds, the solid content of the slurry in the first container gradually increases. At this time, it is difficult to obtain a slurry with a high liquid content by adjusting the pouring speed. By filtering the slurry through a ceramic filter, a slurry with a lower solid content can be obtained, thereby forming a high liquid phase area at the top of the mold, so that the top of the mold has a higher Al and Sr concentration. The high concentration of Al and Sr can form more Al4Sr phases on the top surface of the magnesium alloy during the cooling process, thereby improving the corrosion resistance of the top surface of the magnesium alloy.

[0009] Furthermore, the cooling rate is 1-5°C / s. Using a higher cooling rate can obtain finer grains, thereby improving corrosion resistance and hardness.

[0010] Furthermore, the first pouring rate is 0.005-0.01 kg / s. The above pouring rate can reduce the solid phase ratio of the slurry poured for the first time.

[0011] Furthermore, the mass ratio of the first pouring slurry to the second pouring slurry is (2-3): (97-99.5). Increasing the mass of the first pouring slurry can increase the thickness of the corrosion-resistant layer on the bottom surface of the magnesium alloy material, thereby further improving the corrosion resistance.

[0012] Furthermore, the mass fraction of Sr in the melt is 0.5%. The above mass fraction of Sr can produce the finest grains and obtain better hardness and corrosion resistance.

[0013] Furthermore, the die casting includes: forming at a strain rate of 1.5-2.5 / s. The faster strain rate can prevent the slurry in the mold from separating into solid and liquid phases during the die casting process.

[0014] Furthermore, the magnesium master alloy is Mg-10Sr.

[0015] Furthermore, the magnesium alloy is AZ31. The Al content of AZ31 is less than 9%, and the corrosion resistance is poor. The preparation method of the present application can improve the corrosion resistance of the above alloy.

[0016] A second aspect of the present invention provides a corrosion-resistant magnesium alloy prepared by the above-mentioned preparation method.

[0017] The above-mentioned corrosion-resistant magnesium alloy not only has excellent hardness, but also has good corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the XRD pattern of the bottom surface of the magnesium alloy of Example 4.

[0019] Figure 2 This is the XRD pattern of the top surface of the magnesium alloy of Example 4. DETAILED DESCRIPTION

[0020] For ease of understanding of the application, the application will be described more fully below. The application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.

[0021] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0023] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0024] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0025] The percentage contents involved in this application, unless otherwise specified, refer to mass percentage for solid-liquid mixing and solid-solid mixing, and refer to volume percentage for liquid-liquid mixing.

[0026] The percentage concentrations mentioned in this application, unless otherwise specified, refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.

[0027] The temperature parameters in this application, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range of instrument control.

[0028] The "particles" mentioned in this application, or materials with a defined particle size distribution, are not necessarily spherical in shape, but may be irregular, primary particles or secondary particles. The particle size of irregular particles is the average of their maximum diameter and minimum diameter.

[0029] Example 1: Various pure metals were weighed according to the ingredients required for preparing 9.7 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C. 0.3 kg of Mg-10Sr was added and stirred to mix evenly. At this time, the mass fraction of Sr in the melt was 0.3%. The melt was transferred to a first container, cooled at a rate of 1°C / s, and the stirring rate was 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured for the first time, the rate of the first pouring was 0.02 kg / s, and the mass of the first pouring was 0.05 kg. Then, a second pouring was performed, the rate of the second pouring was 0.2 kg / s, and the mass of the second pouring was 9.95 kg.

[0030] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of die casting is 2.5 / s. The molds used in the embodiment and the comparative example are both sheet forming molds, and the formed magnesium alloy is a sheet having a top surface and a bottom surface.

[0031] Example 2: Various pure metals were weighed according to the ingredients required for preparing 9.7 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 850°C. 0.3 kg of Mg-10Sr was added and stirred to mix evenly. At this time, the mass fraction of Sr in the melt was 0.3%. The melt was transferred to a first container, cooled at a rate of 5°C / s, and the stirring rate was 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 50%, the semi-solid magnesium alloy slurry was poured for the first time, the rate of the first pouring was 0.005 kg / s, and the mass of the first pouring was 0.05 kg. Then, a second pouring was performed, the rate of the second pouring was 0.1 kg / s, and the mass of the second pouring was 9.95 kg.

[0032] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of die casting is 1.5 / s.

[0033] Example 3: Various pure metals were weighed according to the ingredients required for preparing 9.7 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C. 0.3 kg of Mg-10Sr was added and stirred to mix evenly. At this time, the mass fraction of Sr in the melt was 0.3%. The melt was transferred to a first container, cooled at a rate of 1°C / s, and the stirring rate was 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured for the first time at a rate of 0.02 kg / s and a mass of 0.3 kg. Then, a second pouring was performed at a rate of 0.2 kg / s and a mass of 9.7 kg.

[0034] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of die casting is 2.5 / s.

[0035] Example 4: Various pure metals were weighed according to the ingredients required for preparing 9.7 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C, and 0.3 kg of Mg-30Sr was added and stirred to mix evenly. At this time, the mass fraction of Sr in the melt was 0.9%. The melt was transferred to a first container, cooled at a rate of 1°C / s, and the stirring rate was 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured for the first time, the rate of the first pouring was 0.02 kg / s, and the mass of the first pouring was 0.05 kg, and then the second pouring was performed, the rate of the second pouring was 0.2 kg / s, and the mass of the second pouring was 9.95 kg.

[0036] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of die casting is 2.5 / s.

[0037] Example 5: Various pure metals were weighed according to the ingredients required for preparing 9.5 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C. 0.5 kg of Mg-10Sr was added and stirred to mix evenly. At this time, the mass fraction of Sr in the melt was 0.5%. The melt was transferred to a first container, cooled at a rate of 1°C / s, and the stirring rate was 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured for the first time at a rate of 0.02 kg / s and a mass of 0.05 kg. Then, a second pouring was performed at a rate of 0.2 kg / s and a mass of 9.95 kg.

[0038] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of die casting is 2.5 / s.

[0039] Example 6: Various pure metals were weighed according to the ingredients required for preparing 9.7 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C, and 0.3 kg of Mg-10Sr was added and stirred and mixed evenly. At this time, the mass fraction of Sr in the melt was 0.3%. The melt was transferred to the first container, cooled at a rate of 1°C / s, and the stirring rate was 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured for the first time, the rate of the first pouring was 0.02 kg / s, and the mass of the first pouring was 0.05 kg. Then, a second pouring was performed, the rate of the second pouring was 0.2 kg / s, and the mass of the second pouring was 9.85 kg. Then, a third pouring was performed: the remaining 0.1 kg of slurry was passed through a 50 μm ceramic filter and entered the mold.

[0040] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of die casting is 2.5 / s.

[0041] Example 7: Various pure metals were weighed according to the ingredients required for preparing 9.7 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C, and 0.3 kg of Mg-10Sr was added and stirred and mixed evenly. At this time, the mass fraction of Sr in the melt was 0.3%. The melt was transferred to the first container, cooled at a rate of 1°C / s, and the stirring rate was 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured for the first time, the rate of the first pouring was 0.02 kg / s, and the mass of the first pouring was 0.3 kg. Then, a second pouring was performed, the rate of the second pouring was 0.2 kg / s, and the mass of the second pouring was 9.2 kg. Then, a third pouring was performed: the remaining 0.5 kg of slurry was passed through a 100 μm ceramic filter and entered the mold.

[0042] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of die casting is 2.5 / s.

[0043] Example 8: Various pure metals were weighed according to the ingredients required for preparing 9.7 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C, and 0.3 kg of Mg-10Sr was added and stirred to mix evenly. At this time, the mass fraction of Sr in the melt was 0.3%. The melt was transferred to a first container, cooled at a rate of 1°C / s, and the stirring rate was 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured for the first time, the rate of the first pouring was 0.02 kg / s, and the mass of the first pouring was 0.05 kg, and then the second pouring was performed, the rate of the second pouring was 0.2 kg / s, and the mass of the second pouring was 9.95 kg.

[0044] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of the die casting is 0.8 / s.

[0045] Comparative Example 1: Various pure metals were weighed according to the ingredients required for preparing 9.7 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C. 0.3 kg of Mg-10Sr was added and stirred and mixed evenly. At this time, the mass fraction of Sr in the melt was 0.3%. The melt was transferred to a first container, cooled at a rate of 1°C / s, and the stirring rate was 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured at a pouring rate of 0.2 kg / s, and the pouring mass was 10 kg.

[0046] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of die casting is 2.5 / s.

[0047] Comparative Example 2: Various pure metals were weighed according to the ingredients required for preparing 10 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C. The melt was transferred to a first container, cooled at a rate of 1°C / s, and stirred at a rate of 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured for the first time at a rate of 0.02 kg / s and a mass of 0.05 kg, and then poured for the second time at a rate of 0.2 kg / s and a mass of 9.95 kg.

[0048] After pouring, die casting is performed to obtain a corrosion-resistant magnesium alloy, and the strain rate of die casting is 2.5 / s.

[0049] Comparative Example 3: Various pure metals were weighed according to the ingredients required for preparing 9.7 kg of AZ31 and added to a resistance furnace for smelting to obtain a melt at a temperature of 720°C. 0.3 kg of Mg-40Sr was added and stirred to mix evenly. At this time, the mass fraction of Sr in the melt was 1.2%. The melt was transferred to a first container, cooled at a rate of 1°C / s, with a stirring rate of 100 rpm. After cooling to the semi-solid range of the melt, a semi-solid magnesium alloy slurry was obtained. When the solid content of the semi-solid magnesium alloy slurry was 30%, the semi-solid magnesium alloy slurry was poured at a pouring rate of 0.2 kg / s and a pouring mass of 10 kg.

[0050] Hardness test method: refer to the national standard GB / T 7997-2014 "Vickers hardness test method for cemented carbide" for testing, and record the data in Table 1.

[0051] Corrosion resistance test method: refer to the national standard GB / T10125-2012 "Artificial atmosphere corrosion test salt spray test" to conduct neutral salt spray test, expose in salt spray for 24 hours, and evaluate the corrosion area of ​​the salt spray exposure area. Specifically: sample the magnesium alloys of the above embodiments and comparative examples, take two samples respectively, each sample contains the top surface and the bottom surface of the magnesium alloy, and test the corrosion resistance of the top surface and the bottom surface respectively, and shield the other surfaces during the test.

[0052] Table 1 Test results of hardness and corrosion resistance of Examples 1-8 and Comparative Examples 1-3.

[0053] According to the data in Table 1 and Figure 1-Figure 2It can be seen that Examples 1-8 have stronger hardness than Comparative Examples 2-3. This is because 0.3-0.9% by mass of Sr element is added to the magnesium alloy. The Sr element in the above proportion can promote grain refinement and improve the hardness of the magnesium alloy. Comparative Example 3 uses too high a proportion of Sr element, which in turn leads to coarsening of the grains of the magnesium alloy and reduced performance. The bottom surface of Example 1-8 has stronger corrosion resistance than the bottom surface of Comparative Example 1-3, and the bottom surface of Example 1-6 has stronger corrosion resistance than the top surface of Example 1-6. This is because by reducing the rate of the first pouring, the liquid phase has a faster flow speed than the solid phase, so that solid-liquid phase separation occurs. The slurry poured for the first time has a higher liquid phase ratio, so a high liquid phase area is formed at the bottom of the mold, and Al and Sr elements tend to be distributed in the liquid phase, while Mg in the liquid phase decreases with the increase of solid content. Thus, the slurry poured for the first time has a higher concentration of Al and Sr. The high concentration of Al and Sr can form more Al4Sr phases at the bottom of the magnesium alloy (i.e., the bottom of the mold) during the cooling process, thereby improving the corrosion resistance of the bottom surface of the magnesium alloy material. Figure 1-Figure 2 As shown in the figure, the peak value of Al4Sr on the bottom surface of the magnesium alloy is significantly enhanced, which indicates that more Al4Sr phase is formed in the bottom layer of Example 4. Comparative Example 1 does not have a lower first pouring speed, and cannot form a corrosion-resistant bottom surface. Comparative Example 2 does not add Sr elements, and cannot form Al4Sr phase on the bottom surface; Comparative Example 3 uses too high Sr concentration, which will lead to grain coarsening, resulting in reduced hardness and overall corrosion resistance of the magnesium alloy material.

[0054] Example 2 uses a semi-solid magnesium alloy slurry with a higher solid content, so the first pouring needs to use a lower rate. By using a faster cooling rate, a large number of fine grains can be formed, thereby further improving the corrosion resistance of the material. The first pouring of Example 3 uses a larger mass, which can improve the corrosion resistance of the bottom surface. Example 5 has higher hardness and better corrosion resistance than Example 1 and Example 4, because it uses the preferred mass fraction of Sr. Examples 6-7 add a third pouring, and a corrosion-resistant layer rich in Al4Sr is formed on the top surface of the magnesium alloy material by filtering, which improves the corrosion resistance of the top surface of the magnesium alloy material. The above-mentioned magnesium alloy has better corrosion resistance for making plates, pipes, wheels and other components. Example 8 uses a lower strain rate, which may cause liquid phase separation during the die-casting process, and the solid phase is concentrated in some areas of the mold, destroying the bottom layer rich in Al4Sr.

[0055] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0056] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a corrosion-resistant magnesium alloy, characterized in that: The following steps are involved: According to the composition of the alloy to be prepared, pure metal is added into a resistance furnace for melting, the magnesium alloy is AZ31, a melt with a temperature of 720-850° C. is obtained, a magnesium intermediate alloy containing Sr is added and stirred and mixed evenly, so that the mass fraction of Sr in the melt is 0.3-0.9%, the melt is transferred to a first container, the melt is stirred and cooled to form a semi-solid magnesium alloy slurry, and when the solid content of the semi-solid magnesium alloy slurry is 30-50% by mass, the semi-solid magnesium alloy slurry is The material is poured into the mold, and after the pouring is completed, die casting is performed to obtain the corrosion-resistant magnesium alloy, the pouring includes: a first pouring and a second pouring, the rate of the first pouring is 0.005-0.02kg / s, the rate of the second pouring is 0.1-0.2kg / s, the mass ratio of the slurry of the first pouring to the slurry of the second pouring is (0.5-3): (92-99.5), and the die casting includes: forming at a strain rate of 1.5-2.5 / s.

2. The method for preparing a corrosion-resistant magnesium alloy according to claim 1, characterized in that: The method comprises the following steps: after the second pouring is completed, the remaining semi-solid magnesium alloy slurry is passed through a ceramic filter with a pore size of 50-100 μm and then enters the mold, and the mass ratio of the remaining semi-solid magnesium alloy slurry to the slurry of the second pouring is (1-5): (92-98.5).

3. The method for preparing a corrosion-resistant magnesium alloy according to claim 1, characterized in that: The cooling rate is 1-5°C / s.

4. The method for preparing a corrosion-resistant magnesium alloy according to claim 1, characterized in that: The first pouring rate is 0.005-0.01 kg / s.

5. The method for preparing a corrosion-resistant magnesium alloy according to claim 1, characterized in that: The mass ratio of the slurry poured for the first time to the slurry poured for the second time is (2-3): (97-99.5).

6. The method for preparing a corrosion-resistant magnesium alloy according to claim 1, characterized in that: The mass fraction of Sr in the melt is made to be 0.5%.

7. The method for preparing a corrosion-resistant magnesium alloy according to claim 1, characterized in that: The magnesium master alloy is Mg-10Sr.

8. A corrosion-resistant magnesium alloy, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Alkaline-earth heat insulating magnesium alloy for vehicle use and producing method thereof

    CN101067178A

  • Material forming method for preparing composite product using semi-solid state forming technique

    CN101406941A

  • Method for preparing laminated composite metal material through semi-solid rolling after centrifugal compositing

    CN102489531A

  • Sealing process of hollow fiber membrane

    CN116212643A

  • High-strength and high-thermal-conductivity magnesium alloy and preparation method thereof

    CN116657009A