A method for predicting the crack arrest temperature of crack arrest steel based on drop weight tear test

The crack stop temperature prediction model was established through the drop hammer tear test, which solved the problems of long test cycle and high cost of crack stop steel in the existing technology, achieved rapid and accurate crack stop temperature prediction, and improved the safety and R&D of container ships efficiency.

CN118566037BActive Publication Date: 2024-11-15CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411057380.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-15
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The existing crack-resistance toughness test methods of crack-resistance steel have long test cycles, high costs, and complex processes. It is difficult to quickly predict crack-resistance temperature during the crack-resistance steel research and development and trial production stages, which affects the safety and R&D efficiency of container ships.

Method used

Using a method based on the hammer tear test, the crack stop temperature is predicted, the test process is simplified, and the cost is reduced by establishing a correlation model between the crack stop toughness and the hammer tear transition temperature. Specific steps include ladder-temperature double tensile test and drop hammer tear test, establishing a correlation model between Tkca6000 and FATT50 for the prediction of crack stop temperature of new materials.

Benefits of technology

It achieves rapid and accurate prediction of crack stop temperature, reduces test costs and cycles, and is suitable for the research and development and trial production of small-scale crack stop steel, which significantly improves the operational safety of container ships.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118566037B_ABST
    Figure CN118566037B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for predicting the crack arrest temperature of crack arrest steel based on a drop weight tearing test, which belongs to the technical field of fracture and crack arrest of hull structural steel. The present invention firstly carries out a double tensile test on crack arrest steels of different thicknesses and different strength grades to obtain a large number of crack arrest temperatures T k , or obtain the crack arrest temperature T based on the existing crack arrest steel data k ; For each specification and strength grade of crack arrest steel, a series of drop weight tear tests are carried out to obtain the drop weight tear ductile-brittle transition curve and drop weight tear transition temperature FATT 50 ; Further analysis of the characteristic crack arrest temperature T kca6000 and drop weight tear transition temperature FATT 50 The correlation model was established, and then the drop weight tearing transition temperature FATT was used to 50 The invention can realize rapid prediction of crack arrest temperature. The invention can meet the initial evaluation of crack arrest temperature in the research and development and trial production stages of crack arrest steel through a small-scale drop-weight tearing test, and provide important basic input for realizing large-scale application of crack arrest steel and improving the operational safety of ultra-large container ships.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fracture and crack arrest of hull structural steel, and in particular relates to a method for predicting the crack arrest temperature of crack arrest steel based on a drop weight tearing test. Background Art

[0002] With the development of low-carbon economy, container transport ships are becoming increasingly large-scale. Ultra-large container ships with a capacity of more than 24,000 TEU have gradually entered the design, construction and operation stages and will become one of the main ship types in the next few years. Compared with small and medium-sized container ships, the stress state of the hull structure of large container ships is significantly worse. The large size and large opening characteristics of the hull will cause the hull structure to be subjected to the combined action of multiple loads. In addition to meeting the requirements of total longitudinal bending strength and buckling strength, it is also necessary to meet the requirements of large opening (torsion) strength, resulting in high stress levels in the hatch coaming top plate, web plate and upper deck side plate, side top plate and some local areas (hatch corners) in the hull structure. In order to ensure the safety and reliability of the hull structure and prevent the occurrence of brittle fracture damage, high-strength and thick crack arrest steel can usually be used in the high-stress area of ​​the hull. When fatigue fracture occurs in the hull, the crack will stop expanding when it reaches the crack arrest steel, thereby avoiding catastrophic fracture accidents. The large-scale application of crack arrest steel provides an important guarantee for improving the safe and green operation of container ships.

[0003] Crack arrest temperature is the core indicator for evaluating the performance of crack arrest steel, and is also an important reference for the design and service temperature of container ships. During the research and development, trial production and actual ship application of crack arrest steel, multiple rounds of composition and process optimization are required, and each round of iteration requires testing of its crack arrest temperature. ca 6000N / mm 1.5 The corresponding temperature is the characteristic crack arrest temperature, that is, T kca6000 . Its meaning is that when the crack arrest toughness of the material reaches 6000N / mm 1.5 If the characteristic crack arrest temperature is lower than the service temperature of the ship, the hull will not suffer catastrophic fracture from the perspective of crack arrest. According to relevant industry specifications such as the International Classification Society Standard UR W31 and the China Classification Society's Guide to the Application of High-Strength Thick Plates for Ships, the gradient temperature double tensile test is usually used to measure T kca6000 The size of the double tensile specimen is 500mm×500mm×t, where t is the plate thickness. The schematic diagram and fracture of the double tensile specimen are shown in Figure 1-2 The temperature gradient field is achieved by applying heat source and cold source in the crack extension zone of the specimen. kca6000 Generally, four sets of tests are required to obtain T kca6000 (Typical results are shown in Figure 4 ).

[0004] The double tensile test needs to be carried out on a 5,000-ton large tensile testing machine, and a large amount of coolant is consumed when establishing the temperature field. The test cycle is long and the cost is high. The paper "Study on the Equivalence of Double Tensile Test Method and ESSO Test Method" in the Journal of Materials Development and Application discloses the establishment of equivalence between the double tensile test method and the ESSO test method, and evaluates the equivalence of the two test methods by analyzing the test results. However, the ESSO test selected in this method is also a test method with a long test cycle and high cost (a large amount of coolant is consumed). At the same time, the ESSO test is equivalent to the double tensile test in the evaluation of crack arrest performance, but it cannot predict the crack arrest temperature of the sample; therefore, if the commonly used small-scale test can be used to quickly predict the crack arrest temperature in the research and development and trial production stage of crack arrest steel, it will have significant benefits to the research and development progress and cost. Summary of the invention

[0005] In view of this, the present invention aims to overcome the problems of long test cycle, high cost and complicated process of existing crack arrest toughness test methods for crack arrest steel, and provide a method for predicting the crack arrest temperature of crack arrest steel based on drop hammer tear test, which can meet the initial evaluation of crack arrest temperature in the research and development and trial production stages of crack arrest steel through small-scale drop hammer tear test, and provide important basic input for realizing large-scale application of crack arrest steel and improving the operational safety of ultra-large container ships.

[0006] A method for predicting the crack arrest temperature of crack arrest steel based on a drop weight tearing test comprises the following steps:

[0007] S1: Conduct temperature gradient double tensile tests on crack arrest steels of different thicknesses to calculate the crack arrest toughness K ca , the crack arrest temperature T can be obtained through the temperature gradient k , establish the crack arrest toughness K ca and crack arrest temperature T k The correlation model of K is obtained by data fitting. ca 6000N / mm 1.5 The corresponding characteristic crack arrest temperature T kca6000 ;

[0008] S2: Take samples from the same batch of crack arrest steel test plates in step S1, process them into drop weight tearing specimens, carry out drop weight tearing tests at different temperatures, obtain the correlation model between the cross-sectional fiber rate FA and the drop weight tearing temperature T, and obtain the drop weight tearing transition temperature FATT through data fitting 50 ;

[0009] S3: Based on the experimental data obtained from the temperature gradient double tensile test and the drop weight tear test, T kca6000 and FATT 50 The correlation model is T kca6000 =α1+β1*FATT50 Where, T kca6000 , unit is ℃; FATT 50 , unit is °C; α1, β1 are parameters to be determined;

[0010] S4: Perform drop weight tear tests at different temperatures on the crack arrest steel in the subsequent new R&D and trial production process, and use the obtained FATT 50 and T obtained in step S3 kca6000 and FATT 50 The correlation model is used to analyze the crack arrest steel in the new R&D and trial production process. kca6000 predict.

[0011] Furthermore, the crack arrest steel in step S1 is EH40 or EH47 crack arrest steel; the thickness of the crack arrest steel is in the range of 80-100 mm.

[0012] Furthermore, the temperature gradient double tensile test in step S1 includes the following steps:

[0013] S11: Gradient temperature type double tensile test A gradient temperature field was established in the main tensile plate. A cold source was applied to the upper part of the temperature field and a heat source was applied to the lower part, thereby forming a temperature gradient of 0.25℃ / mm to 0.35℃ / mm.

[0014] S12: Cooling the crack initiation plate;

[0015] S13: After the temperature field stabilizes, the main tensile load is applied to the main tensile plate, and then the secondary tensile load is applied to the crack initiation plate. The brittle crack initiates from the notch and enters the main tensile plate. After the test, the crack stops expanding after it reaches a certain length a. The crack arrest temperature T at the crack length a can be obtained according to the temperature gradient. k .

[0016] Furthermore, the crack arrest toughness K ca The calculation formula is:

[0017]

[0018] Where σ is the applied stress in N / mm 2 ; a is the crack length when crack arrest occurs, in mm; W s is the width of the specimen in mm.

[0019] Furthermore, the size of the crack arrest steel sample in the gradient temperature double tensile test is 500 mm×500 mm×t, wherein t is the plate thickness of the crack arrest steel.

[0020] Furthermore, the crack arrest toughness K described in step S1 ca and crack arrest temperature T kThe correlation model is K ca =K0exp(-T0 / T k ); where T k , unit is ℃; K0, T0 are material constants.

[0021] Furthermore, the size of the drop weight tearing specimen in step S2 is 305 mm×76.2 mm×t.

[0022] Further, the drop weight tear test in step S2 includes the following steps:

[0023] S21: A notch with a depth of 5 ± 0.5 mm is pressed in the center of the specimen for the drop weight tear test;

[0024] S22: placing the above samples in liquid media at different temperatures;

[0025] S23: Load the sample processed in step S22 into the testing machine and break it quickly, and measure FA and T when the sample breaks.

[0026] Furthermore, the correlation model between the cross-sectional fiber rate FA and the drop weight tearing temperature T in step S2 is:

[0027] ;

[0028] In the formula, FA is in %; T is in ℃; A1, A2, T 50 is the function parameter, dimensionless, where T 50 FATT 50 The corresponding value.

[0029] Furthermore, the FATT in step S1 50 It is the temperature at which the fiber ratio of the cross section is 50% in the drop weight tear test.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1) The present invention can predict the crack arrest temperature more accurately. Based on the intrinsic connection between the double tensile test and the small-size drop weight tear test in terms of crack initiation, propagation and termination, a correlation model is established, which can predict the crack arrest temperature more accurately, and the error can meet the needs of the material research and development and trial production stages.

[0032] 2) The drop weight tear test specimen is small in size and does not require large-scale rolling, saving a lot of material and processing costs. It is suitable for small-scale crack arrest steel in the research and development or trial production stage.

[0033] 3) The drop weight tear test method is mature and simple, with a short cycle and low cost, saving a lot of research funds. By replacing the double tensile test with the drop weight tear test, the cycle is shortened from several months to several days, and the cost is reduced from hundreds of thousands to thousands of yuan. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a schematic diagram of the double tensile test of the present invention;

[0035] Figure 2 This is a fracture diagram of a double tensile specimen of the present invention;

[0036] Figure 3 is the short distance from the cold end and the crack arrest temperature T of the double stretching in the embodiment of the present invention k Fitting schematic diagram;

[0037] Figure 4 is the crack arrest toughness K in the embodiment of the present invention ca and crack arrest temperature T k Schematic diagram of the correlation model;

[0038] Figure 5 This is a schematic diagram of a drop weight tearing specimen of the present invention;

[0039] Figure 6 This is a fracture diagram of the drop weight tearing specimen of the present invention;

[0040] Figure 7 Schematic diagram of fiber ratio transformation curve of a typical section of drop weight tearing in an embodiment of the present invention;

[0041] Figure 8 is the characteristic crack arrest temperature T in the embodiment of the present invention kca6000 and drop weight tear transition temperature FATT 50 Schematic diagram of the correlation model;

[0042] Fig. 9 This is a diagram showing the prediction effect of characteristic crack arrest temperature in an embodiment of the present invention;

[0043] Reference numerals:

[0044] Main tensile plate 1, temperature field 2, crack initiation plate 3. DETAILED DESCRIPTION

[0045] During the research and development, trial production and actual ship application of crack arrest steel, multiple rounds of composition and process optimization are required. Each round of iteration requires testing of its crack arrest temperature. During the design and development of crack arrest steel, crack arrest temperature measurement is the core indicator for evaluating the design and development effect of crack arrest steel, and is also an important reference for the design and service temperature of container ships. The existing technology usually uses 6000N / mm 1.5 The corresponding temperature is the characteristic crack arrest temperature, that is, when the crack arrest toughness of the material reaches 6000N / mm 1.5When the characteristic crack arrest temperature is lower than the service temperature of the ship, the hull will not suffer catastrophic fracture from the perspective of crack arrest. In order to obtain, four sets of tests are generally required, and the typical results are obtained by interpolation (see Figure 4 ). The double tensile test needs to be carried out on a 5000-ton large tensile testing machine, and a large amount of coolant is required when establishing temperature field 2. The test cycle is long and the cost is high. A large amount of welding materials are required for test tooling assembly. At least 4 test plates of 500mm×500mm×original plate thickness are also required. If the commonly used small-scale test can be used to quickly predict the crack arrest toughness during the research and development and trial production stage of crack arrest steel, it will have significant benefits for research and development progress and cost.

[0046] The Drop Wight Tearing Test was first proposed by Puzak and Perini of the U.S. Naval Research Institute. In September 1963, the Battelle Institute published data that confirmed that there was a good correlation between the drop-weight tearing test results and the service performance of pipeline steel. The fracture morphology was highly consistent with the actual crack propagation morphology in pipelines and pressure vessels. After that, this method was promoted in the evaluation of the crack arrest performance of pipeline steel. This method was listed as a formal test standard (ASTM E436) by the American Society for Materials, and the American Petroleum Institute also formulated a corresponding recommended method (API RP5L3). The drop-weight tearing specimen is small in size and easy to process. A set of series temperature drop-weight tearing tests requires at least 24 specimens, and the weight does not exceed 10kg. It is suitable for small-scale crack arrest steel in the research and development or trial production stage. At the same time, its test method is mature, the equipment is simple, and the relevant standards and specifications are very complete. Many steel mills and research and development institutions have test conditions and low test costs. It has been widely used in hull structural steel.

[0047] The cross-sectional area of ​​the specimen in the drop weight tear test is large (5 to 7 times the area of ​​the impact specimen of the same plate thickness), and the crack propagation distance is long, which is close to the actual fracture situation. The drop weight tear transition temperature FATT is generally used. 50 Evaluation of the fracture and crack arrest temperature of hull steel. If the crack arrest temperature of double tensile test and the drop weight tear transition temperature FATT of drop weight tear test can be established 50 The correlation between the crack arrest temperature of the crack arrest steel can be quickly evaluated through a small-scale drop weight tear test, which has important guiding significance for accelerating the research and development and application of crack arrest steel.

[0048] Specifically, a method for predicting the crack arrest temperature of crack arrest steel based on a drop weight tear test comprises the following steps:

[0049] S1: Conduct temperature gradient double tensile tests on crack arrest steels of different thicknesses to calculate the crack arrest toughness K ca , the crack arrest temperature T can be obtained through the temperature gradient k , establish the crack arrest toughness Kca and crack arrest temperature T k The correlation model of K is obtained by data fitting. ca 6000N / mm 1.5 The corresponding characteristic crack arrest temperature T kca6000 ;

[0050] The crack arrest steel is EH40 or EH47 crack arrest steel with a thickness of 80-100 mm. The temperature gradient double tensile test is carried out, including the following steps:

[0051] S11: a gradient temperature field 2 is established in the main stretching plate 1, a cold source is applied to the upper part of the gradient temperature field 2, and a heat source is applied to the lower part, thereby forming a temperature gradient of 0.25°C / mm to 0.35°C / mm;

[0052] S12: Cooling the crack initiation plate 3;

[0053] S13: After the temperature field 2 is stabilized, the main tensile load is applied to the main tensile plate 1, and then the secondary tensile load is applied to the crack initiation plate 3. The brittle crack is initiated from the notch and enters the main tensile plate 1. After the test, the crack stops expanding after it reaches a certain length a. The crack arrest temperature T at the crack length a can be obtained according to the temperature gradient. k and crack arrest toughness K ca .

[0054] The crack arrest toughness K ca The calculation formula is as follows:

[0055]

[0056] Where σ is the applied stress in N / mm 2 ; a is the crack length when crack arrest occurs, in mm; W s is the width of the specimen in mm.

[0057] Four groups of specimens were prepared for double tensile tests, where the specimen size was 500 mm × 500 mm × t, t being the thickness of the crack arrest steel plate, to obtain at least four groups of effective crack arrest toughness K ca and crack arrest temperature T k The above four sets of data are fitted to obtain the crack arrest toughness K ca and crack arrest temperature T k Correlation Model: K ca =K0exp(-T0 / T k ); where T k is the crack arrest temperature in °C; K0, T0 are material constants, and then K is selected ca 6000N / mm 1.5 , and the corresponding characteristic crack arrest temperature Tkca6000 .

[0058] S2: According to GB / T 8363-2018 "Drop-weight tear test method for steel", samples are taken from the same batch of crack arrest steel test plates in step S1, and they are processed into drop-weight tear test specimens with a sample size of 305 mm × 76.2 mm × t, where t is the thickness of the crack arrest steel plate. Drop-weight tear tests are carried out at different temperatures, and the drop-weight tear test includes the following steps:

[0059] S21: A notch with a depth of 5 ± 0.5 mm is pressed in the center of the specimen for the drop weight tear test;

[0060] S22: placing the above samples in liquid media at different temperatures;

[0061] S23: The sample after the above treatment is loaded into a testing machine and quickly broken, and the cross-sectional fiber rate FA and temperature T of the sample when it is broken are measured.

[0062] According to the above test, the cross-sectional fiber rate FA at different temperatures T is obtained, and a (T, FA) scatter plot is drawn. According to the Boltzmann function, a correlation model between the cross-sectional fiber rate FA and the temperature T is established, and the drop weight tear transition temperature FATT is obtained by data fitting. 50 , where FATT 50 It is the drop weight tear transition temperature when the fiber ratio of the cross section is 50% in the drop weight tear test;

[0063] Among them, the Boltzmann function is as follows:

[0064] ;

[0065] In the formula, FA is in %; T is in ℃; A1, A2, T 50 is the function parameter, dimensionless, where T 50 FATT 50 The corresponding value.

[0066] S3: Based on the experimental data obtained from the temperature gradient double tensile test and the drop weight tear test, the crack arrest temperature T is established. kca6000 and drop weight tear transition temperature FATT 50 The correlation model is T kca6000 =α1+β1*FATT 50 Where, T kca6000 , unit is ℃; FATT 50 , unit is °C; α1, β1 are parameters to be determined;

[0067] The original plate thickness double tensile test and the small-scale drop-weight tear test both belong to the fracture category of hull crack arrest steel. Both reflect the change of material fracture and crack arrest performance with temperature. For ferritic steel such as crack arrest steel, the crack arrest toughness increases with the increase of temperature. Therefore, in the gradient temperature double tensile test, the crack will start from the low temperature area and extend to the high temperature area. As the temperature of the crack tip increases, the material crack arrest toughness increases rapidly. When the material crack arrest toughness is higher than the crack fracture toughness, the crack will stop. At this time, the temperature corresponding to the crack tip is called the crack arrest temperature. For the drop-weight tear test, the cross-sectional fiber rate can usually be used to characterize the toughness level of the material at the time of fracture. When the cross-sectional fiber rate is 100%, the material has high crack arrest toughness. When the cross-sectional fiber rate is 0, it indicates that the material will undergo brittle fracture and has no crack arrest ability. The cross-sectional fiber rate decreases with the decrease of temperature. It can be seen that the large-scale double tensile test and the small-scale drop-weight tear test are both intrinsically related to temperature in terms of material toughness characterization, which provides a theoretical basis for small-scale tests to replace double tensile tests.

[0068] S4: Perform drop weight tear tests at different temperatures on the crack arrest steel in the subsequent new R&D and trial production process, and obtain the drop weight tear transition temperature FATT 50 and the characteristic crack arrest temperature T obtained in step S3 kca6000 and drop weight tear transition temperature FATT 50 The correlation model is used to determine the characteristic crack arrest temperature T of the crack arrest steel in the new R&D and trial production process. kca6000 predict.

[0069] Example

[0070] According to the requirements of the rapid prediction method of crack arrest temperature, the present invention selected 16 groups of crack arrest steels for testing, measured the corresponding crack arrest temperatures and drop weight tear transition temperatures, and constructed a correlation model between the characteristic crack arrest temperature and the drop weight tear transition temperature.

[0071] The specific working process is as follows:

[0072] 1. Select 21 groups of EH40 or EH47 crack arrest steels, and conduct double tensile tests on 4 specimens in each group. The fitting result is 6000N / mm 1.5 The corresponding temperature.

[0073] 2. Samples were taken from the same test plate in the double tensile test to conduct drop weight tear tests at a series of temperatures, ranging from 0°C to -196°C. The ductile-brittle transition curve and FATT of each group of steel were obtained by Boltzmann function fitting. 50 Temperature, typical temperature transition curve see Figure 4 The specifications, crack arrest temperature and transition temperature of each group of crack arrest steel are shown in Table 1:

[0074] Table 1 Specifications, crack arrest temperature and transition temperature of each group of crack arrest steel

[0075]

[0076] Based on the experimental data obtained from the temperature gradient double tensile test and the drop weight tear test, the characteristic crack arrest temperature and the drop weight tear transition temperature FATT were directly calculated by regression analysis. 50 Regression analysis was performed and a regression model with a correlation coefficient greater than 0.9 was obtained. The results are shown in Figure 7 As shown, the prediction model is T kca6000 =FATT 50 -10; where T kca6000 K ca =6000N / mm 1.5 The corresponding characteristic crack arrest temperature is in °C; FATT 50 is the drop weight tear transition temperature, in °C.

[0077] 4. According to the prediction model, the comparison between the predicted and measured values ​​of the crack arrest temperature of each group of steel is obtained, see Fig. 9 As shown. Fig. 9 It can be seen that through FATT 50 The crack arrest temperature can be predicted with a maximum error of no more than 10°C, which has guiding significance for the prediction of crack arrest temperature in the R&D and trial production stages.

[0078] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for predicting the crack arrest temperature of crack arrest steel based on a drop weight tear test, characterized in that: The following steps are involved: S1: For crack arrest steels of different thicknesses, where the crack arrest steel is EH40 or EH47 crack arrest steel with a thickness range of 80-100 mm, a gradient temperature double tensile test is carried out to calculate the crack arrest toughness K ca , the crack arrest temperature T can be obtained through the temperature gradient k , establish K ca and T k The correlation model of K is obtained by data fitting. ca 6000N / mm 1.5 The corresponding characteristic crack arrest temperature T kca6000 ; S2: taking samples from the same batch of crack arrest steel test plates in step S1, processing them into drop weight tearing specimens, and carrying out drop weight tearing tests at different temperatures, including the following steps: S21: A notch with a depth of 5±0.5 mm is pressed in the center of the specimen for the drop weight tear test; S22: placing the above samples in liquid media at different temperatures; S23: Load the sample processed in step S22 into the testing machine and quickly break it, and measure FA and T when the sample breaks; The correlation model between the cross-sectional fiber content FA and the drop weight tearing temperature T was obtained, and the drop weight tearing transition temperature FATT was obtained by data fitting. 50 ; S3: Based on the experimental data obtained from the temperature gradient double tensile test and the drop weight tear test, T kca6000 and FATT 50 The correlation model T kca6000 =α1+β1*FACT 50 ; Where, T kca6000 , unit is ℃; FATT 50 , the unit is ℃; α1, β1 are unknown parameters; the correlation coefficient of the correlation model is greater than 0.9, and the maximum error does not exceed 10℃; S4: Perform drop weight tear tests at different temperatures on the crack arrest steel in the subsequent new R&D and trial production process, and use the obtained FATT 50 and T obtained in step S3 kca6000 and FATT 50 The correlation model is used to analyze the crack arrest steel in the new R&D and trial production process. kca6000 predict.

2. The method according to claim 1, characterized in that The temperature gradient double tensile test in step S1 comprises the following steps: S11: Gradient temperature type double stretching experiment A gradient temperature field (2) is established in the main stretching plate (1), a cold source is applied to the upper part of the temperature field (2), and a heat source is applied to the lower part, thereby forming a temperature gradient of 0.25℃ / mm to 0.35℃ / mm; S12: Cooling the crack initiation plate (3); S13: After the temperature field is stabilized, a primary tensile load is applied to the primary tensile plate (1), and then a secondary tensile load is applied to the crack initiation plate (3). The brittle crack is initiated from the notch and enters the primary tensile plate (1). After the test, the crack stops expanding after it reaches a certain length a. The T at the crack length a can be obtained according to the temperature gradient. k .

3. The method according to claim 2, characterized in that The crack arrest toughness K ca The calculation formula is: , Where σ is the applied stress in N / mm 2 ; a is the crack length at crack arrest, in mm; Ws is the specimen width, in mm.

4. The method according to claim 2, characterized in that: The size of the crack arrest steel sample in the temperature gradient double tensile test is 500 mm×500 mm×t, wherein t is the plate thickness of the crack arrest steel.

5. The method according to claim 1, characterized in that The crack arrest toughness K described in step S1 ca and crack arrest temperature T k The correlation model is K ca =K0exp(-T0 / T k ) Where, T k is the crack arrest temperature, in °C; K0, T0 are material constants.

6. The method according to claim 1, characterized in that The size of the drop weight tearing specimen in step S2 is 305 mm×76.2 mm×t.

7. The method according to claim 1, characterized in that The correlation model between the cross-sectional fiber rate FA and the drop weight tearing temperature T in step S2 is: , In the formula, FA is expressed in % T, unit is ℃; A1, A2, T 50 is the function parameter, dimensionless.

8. The method according to claim 1, characterized in that The drop weight tear transition temperature FATT in step S2 50 It is the temperature corresponding to the cross-sectional fiber ratio of 50% in the drop weight tear test.