A medium pressure formed foil

Through hole reaming treatment, multi-stage medium voltage electrochemical and metal organic framework modification, combined with the sealing treatment of silicone surfactant, the problem of insufficient electrostatic capacity when chemical foils improve hydration resistance is solved, and high static electricity is achieved The unity of capacity and hydration resistance and reduces the cost of decomposition and energy consumption.

CN118571653BActive Publication Date: 2024-11-19NANTONG NANHUI ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410453823.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-24
Publication Date
2024-11-19
Estimated Expiration
2044-01-24

AI Technical Summary

Technical Problem

When the existing medium and high-pressure foils improve hydration resistance, it is difficult to obtain both electrostatic capacity, and the traditional phosphoric acid passivation method consumes high energy and is unfriendly in the environment, which affects the performance of foils.

Method used

Using pore reaming treatment, multi-stage medium-voltage electrochemical formation and modification of metal organic framework, the silicone surfactant sealing and surface optimization are formed to form a high-pore oxide film and a tightly bonded metal organic framework to improve the electrostatic capacity and water resistance. sex.

Benefits of technology

The electrostatic capacity and hydration resistance of the chemical foil are significantly improved, the chemical foil is reduced, the energy consumption is reduced, the electrostatic capacity and hydration resistance is achieved, and the specific capacity, thermal stability and mechanical properties of the chemical foil are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118571653B_ABST
    Figure CN118571653B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrode foil preparation, and provides a medium-pressure chemical foil. The medium-pressure chemical foil is based on a medium-pressure chemical foil forming method, wherein a corroded foil is first placed in hot water for hydration treatment, and then a pore expander is used to expand the pores of a porous oxide film on the surface of the corroded foil, and then multi-stage medium-voltage electrochemical formation is performed, and then the foil is immersed in a reaction matrix solution of an aluminum-based metal organic framework for surface modification, so that the metal organic framework is in situ grown on the crystalline oxide film on the surface of the medium-pressure chemical foil precursor, and then the foil is immersed in an organic silicon surfactant for pore sealing and surface optimization, and finally heat treatment and repair formation are performed to finally obtain the medium-pressure chemical foil. The invention improves the electrostatic capacity and hydration resistance of the medium-pressure chemical foil, realizes the unity of the two, and is cost-saving and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of application number 2024100952802, application date January 24, 2024, and invention name “A method for forming a medium-pressure chemical foil”. Technical Field

[0002] The invention relates to the technical field of electrode foil preparation, in particular to a medium-pressure chemically formed foil. Background Art

[0003] Medium and high voltage formed foil for aluminum electrolytic capacitors is a special electronic material and one of the basic industries. Due to the late start of my country, it has been included in the national key development and support industries. Formed foil is an important component of aluminum electrolytic capacitors. Formed foil is a product of specially made high-purity aluminum foil after electrochemical or chemical corrosion, and then electrochemically formed on the surface to form an oxide film (aluminum oxide). According to the voltage, the formed aluminum foil can be divided into four types: ultra-low voltage, low voltage, medium-high voltage and high voltage. Among them, high-pressure formed aluminum foil has high purity, high cubic texture and thin surface oxide film, and has excellent quality, but the cost is high, which limits its application; while the process of ultra-low voltage and low voltage formed foil is relatively complicated, and the operation steps are cumbersome. Therefore, the current research focus of formed foil falls on medium and high voltage formed foil.

[0004] The preparation of chemical foil usually involves placing aluminum foil in high-temperature pure water for hydration treatment to form a porous hydrated oxide film on its surface to increase the electrostatic capacity of the chemical foil; then undergoing multi-stage chemical formation, the hydrated film is gradually converted into a crystalline oxide film; after high-temperature calcination, most of the oxide film is converted into γ′-Al2O3, and after multiple chemical formation and repair treatments, a repaired oxide film is formed. However, at high temperatures, the aluminum foil oxide film, especially the anode foil oxide film, will hydrate with water, thereby generating aluminum hydroxide on the surface of the anode foil, resulting in a decrease in the withstand voltage of the anode foil and an increase in the leakage current. The traditional solution is to perform phosphoric acid passivation on the aluminum foil oxide film to dissolve a portion of the aluminum oxide film and improve the hydration resistance of the chemical foil, as described in the prior art patents CN101235529B, CN100480427C and CN101246779B. However, this method still has certain limitations, namely, the pore size of the hydrated oxide film is small, and it is difficult for the passivating agent to fully enter the pores during the passivation treatment to play a passivating role, so that its water resistance needs to be further enhanced. In order to improve this problem, the prior art generally increases the passivation temperature or the concentration of the passivating agent (i.e., the concentration of phosphoric acid), which not only increases the energy consumption of the formation process, but also the large-scale use of phosphoric acid is likely to burden the environment and is not environmentally friendly. In addition, such treatment will also lose a part of the electrostatic capacitance, making it impossible to have both electrostatic capacitance and hydration resistance.

[0005] With the progress of modern science and technology and industry, people have higher and higher requirements for miniaturization and portability of electronic and electrical products. Therefore, electrostatic capacitance has become the key to the development of electrolytic capacitors. The above-mentioned formation method that sacrifices part of the electrostatic capacitance in order to improve the hydration resistance of medium and high voltage formed foil obviously needs to be further optimized. Therefore, how to achieve the unity of improving electrostatic capacitance and hydration resistance has become a hot topic in current research.

[0006] To this end, based on the existing technology, the present invention creatively combines pore expansion treatment, multi-stage medium-voltage electrochemical formation and metal organic framework modification, and then uses silicone surfactants to seal the holes and optimize the surface, thereby providing a method for forming a medium-voltage chemical foil, aiming to improve the electrostatic capacitance and hydration resistance of the medium-voltage chemical foil and achieve the unity of the two. Summary of the invention

[0007] The object of the present invention is to provide a medium-pressure chemically formed foil with high electrostatic capacitance, good hydration resistance, cost saving and environmental friendliness, so as to solve the problems raised in the above-mentioned background technology.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A medium pressure chemical foil, the medium pressure chemical foil is based on a medium pressure chemical foil forming method, the medium pressure chemical foil forming method comprises the following steps:

[0010] Step S1: placing the corroded foil in pure water above 96° C. for hydration treatment for 5-8 minutes, so that a porous oxide film is formed on the surface of the corroded foil;

[0011] Step S2: immersing the corrosion foil after the hydration treatment in step S1 in a pore expanding agent, and calcining after the pore expanding treatment to obtain the corrosion foil containing the large-pore oxide film;

[0012] Step S3: subjecting the etched foil with the large-pore oxide film obtained in step S2 to at least three levels of medium-voltage electrochemical formation, so that the porous oxide film on the surface of the etched foil is densified to form a dense crystalline oxide film, thereby obtaining a medium-voltage electrochemical foil precursor;

[0013] Step S4: immersing the medium-pressure chemical foil precursor obtained in step S3 into the reaction matrix solution of the aluminum-based metal organic framework, stirring evenly to obtain a reaction mixed solution, raising the temperature of the reaction mixed solution to 80-110° C. and reacting for 20-50 minutes, so that the metal organic framework is in situ grown on the crystalline oxide film on the surface of the medium-pressure chemical foil precursor, and obtaining a metal organic framework-modified medium-pressure chemical foil;

[0014] Step S5: soaking the metal organic framework modified medium pressure chemical foil obtained in step S4 in an organic silicon surfactant for 10-20 minutes to obtain a soaked medium pressure chemical foil;

[0015] Step S6: heat-treating the infiltrated medium-pressure chemical foil obtained in step S5 at 450-550° C. for 2-3 minutes to obtain a medium-pressure chemical foil semi-finished product;

[0016] Step S7: placing the medium-pressure chemically formed foil semi-finished product obtained in step S6 in a repair chemically formed liquid for repair chemically formed, and finally obtaining the medium-pressure chemically formed foil.

[0017] Preferably, the pore expanding agent in step S2 is an ammonium chloride solution, and the concentration of the ammonium chloride solution is 1.5-6.5 mol / L.

[0018] Preferably, the time of the hole expansion treatment in step S2 is 20-40 minutes, the temperature of the calcination is 400-600° C., and the time of the calcination is 2-5 hours.

[0019] Preferably, the medium voltage electrification to form a three-stage formation in step S3 includes the following steps:

[0020] Step S31: Place the etched foil with large-aperture oxide film obtained in step S2 in a 2-5% by mass aqueous solution of ammonium dihydrogen phosphate at 75-80°C and a current density of 20-30 mA / cm 2 , the voltage is 70-100V, and the primary formation is carried out for 3-6min;

[0021] Step S32: After washing and drying the corroded foil after the primary formation in step S31, place it in a 0.1-3% by mass aqueous solution of ammonium dihydrogen phosphate at 80-85°C and a current density of 20-30 mA / cm 2 , under the condition of voltage of 80-150V, the secondary formation is carried out, and the formation time is 5-8min;

[0022] Step S33: After washing and drying the corroded foil after the secondary formation in step S32, place it in an aqueous solution of 6-9% by mass boric acid and 0.4-0.6% by mass borate at 80-85°C and a current density of 20-40 mA / cm 2 , under the condition of voltage of 180-210V, three-stage formation is carried out, and the formation time is 6-10min.

[0023] Preferably, the medium voltage electrification in step S3 is a four-stage formation, the four-stage formation includes a three-stage formation, and the four-stage formation further includes step S34: washing and drying the corroded foil after the three-stage formation in S33, placing it in an aqueous solution of 6-9% by mass boric acid and 0.4-0.6% borate, at 80-90°C and a current density of 20-45 mA / cm 2 , under the condition of voltage of 220-250V, four-stage formation is carried out, and the formation time is 5-8min.

[0024] Preferably, the composition of the repairing chemical solution in step S7 is the same as the solution composition in the three-stage chemical step, and the temperature of the repairing chemical solution is 85-90°C, and the current density of the repairing chemical solution is 20-50 mA / cm 2 The voltage of the repair formation is 200-220V, and the time of the repair formation is 3-6min.

[0025] Preferably, the aluminum-based metal organic framework in step S4 uses terephthalic acid as an organic ligand, and the reaction matrix solution of the aluminum-based metal organic framework is prepared by adding terephthalic acid and a soluble aluminum salt into DMF at the same time, stirring and dissolving them, and reacting them.

[0026] Preferably, the molar ratio of the soluble aluminum salt to the organic ligand in step S4 is 1:(1-4).

[0027] Preferably, in step S5, the concentration of the organosilicon surfactant is 0.5-2.3 mL / L, and the temperature of the organosilicon surfactant is controlled at 25-35°C.

[0028] Preferably, the organosilicon surfactant is an anionic organosilicon surfactant or a non-ionic organosilicon surfactant.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention creatively combines pore expansion treatment, multi-stage medium voltage electrification and metal organic framework modification, significantly increasing the pore size of the porous oxide film on the surface of the electroforming foil, which is not only conducive to improving the electrostatic capacitance, but also conducive to the diffusion of the metal organic framework into the crystalline oxide film after the multi-stage medium voltage electrification, thereby playing a passivation role through the close combination of the metal organic framework and the crystalline oxide film substrate, thereby improving the water resistance of the electroforming foil and achieving the unity of electrostatic capacitance and hydration resistance. In addition, the temperature, current and voltage conditions controlled by the multi-stage medium voltage electrification are not high, which reduces energy consumption and formation costs, and the formation time of each step is short, which improves the formation efficiency.

[0031] The present invention creatively adopts an organosilicon surfactant to seal holes and optimize the surface. On the basis of surface modification of the medium-pressure chemical foil by an aluminum-based metal organic skeleton, the crystalline oxide film on the surface of the medium-pressure chemical foil is infiltrated to further seal the crystalline oxide film, inhibit its hydration, and also prevent the porous aluminum-based metal organic skeleton from being contaminated. Silicon atoms in organosilicon are the main components of organosilicon, and they are connected together by covalent bonds to form a stable three-dimensional network structure, thereby having higher electronic conductivity, specific capacity and good electrical properties, and further improving the specific capacity of the chemical foil. In addition, the basic structural unit of organosilicon is composed of silicon-oxygen links, and the bond energy is relatively strong, so it has good thermal stability, chemical stability and mechanical properties, and strong corrosion resistance and wear resistance, thereby enhancing the function of the chemical foil. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A schematic diagram of a process of medium-pressure foil formation according to the present invention;

[0033] Figure 2 It is a schematic diagram of the process of medium voltage electrification in the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] See also Figure 1-2 , the present invention provides:

[0036] Embodiment 1

[0037] A medium pressure chemical foil, the medium pressure chemical foil is based on a medium pressure chemical foil forming method, the medium pressure chemical foil forming method comprises the following steps:

[0038] Step S1: placing the corroded foil in pure water at 97° C. for hydration treatment for 5 minutes, so that a porous oxide film is formed on the surface of the corroded foil.

[0039] Step S2: Immerse the corrosion foil after hydration treatment in step S1 in 1.5 mol / L ammonium chloride solution, expand the pores for 20 minutes, and then bake at 400° C. for 5 hours to obtain a corrosion foil containing a large-pore oxide film.

[0040] Step S3: The etched foil with large-pore oxide film obtained in step S2 is subjected to three-stage medium-voltage electrochemical formation to densify the porous oxide film on the surface of the etched foil and form a dense crystalline oxide film to obtain a medium-voltage electrochemical foil precursor. The specific steps include the following steps (please refer to Figure 2 ):

[0041] Step S31: Place the etched foil with large-aperture oxide film obtained in step S2 in a 2% by mass aqueous solution of ammonium dihydrogen phosphate at 75°C and a current density of 20 mA / cm 2 , the voltage is 70V, and the primary formation is carried out for 3min;

[0042] Step S32: After washing and drying the corroded foil after the primary formation in step S31, place it in a 0.1% by mass aqueous solution of ammonium dihydrogen phosphate at 80°C and a current density of 20 mA / cm 2 , the voltage is 80V, and the secondary formation is carried out for 5min;

[0043] Step S33: After washing and drying the corroded foil after the secondary formation in step S32, the foil is placed in an aqueous solution of 6% by mass boric acid and 0.4% by mass borate at 80°C and a current density of 20 mA / cm 2 Under the conditions of 180V voltage, three-stage formation is carried out, and the formation time is 6min.

[0044] Step S4: using terephthalic acid as an organic ligand, adding terephthalic acid and a soluble aluminum salt into DMF at the same time (the molar ratio of the soluble aluminum salt to the organic ligand is 1:1, stirring to dissolve it, and obtaining a reaction matrix solution of an aluminum-based metal organic framework, immersing the medium-pressure chemical foil precursor obtained in step S3 into the reaction matrix solution of the aluminum-based metal organic framework, stirring evenly to obtain a reaction mixed solution, raising the temperature of the reaction mixed solution to 80° C. and reacting for 50 minutes, so that the metal organic framework is in situ grown on the crystalline oxide film on the surface of the medium-pressure chemical foil precursor, and obtaining a metal organic framework-modified medium-pressure chemical foil.

[0045] Step S5: The metal organic framework modified medium pressure chemical foil obtained in step S4 is immersed in an organic silicon surfactant (anionic organic silicon surfactant) for 10 minutes to obtain an immersed medium pressure chemical foil. The concentration of the organic silicon surfactant in this step is 0.5 mL / L, and the temperature is controlled at 25°C.

[0046] Step S6: heat-treating the infiltrated medium-pressure chemical foil obtained in step S5 at 450° C. for 3 minutes to obtain a medium-pressure chemical foil semi-finished product.

[0047] Step S7: Place the medium-pressure chemically formed foil semi-finished product obtained in step S6 in a repair chemical solution (which has the same composition as the solution in the three-stage chemical step) for repair chemical formation. The repair chemical formation temperature is 85°C and the current density is 20 mA / cm 2 , the voltage is 200V, the repair forming time is 3min, and finally the medium voltage forming foil is obtained. Specific embodiment 2

[0049] A medium pressure chemical foil is provided, wherein the medium pressure chemical foil is based on a medium pressure chemical foil forming method, and the medium pressure chemical foil forming method comprises the following steps:

[0050] Step S1: placing the corroded foil in pure water at 99° C. for hydration treatment for 8 minutes, so that a porous oxide film is formed on the surface of the corroded foil.

[0051] Step S2: The corrosion foil after hydration treatment in step S1 is immersed in 6.5 mol / L ammonium chloride solution, and after pore expansion treatment for 40 minutes, it is baked at 600° C. for 2 hours to obtain a corrosion foil containing a large-pore oxide film.

[0052] Step S3: The etched foil with large-aperture oxide film obtained in step S2 is subjected to four-stage medium-voltage electrochemical formation to densify the porous oxide film on the surface of the etched foil and form a dense crystalline oxide film to obtain a medium-voltage electrochemical foil precursor. The specific steps include the following steps (see Figure 2 ):

[0053] Step S31: Place the etched foil with large-aperture oxide film obtained in step S2 in a 5% by mass aqueous solution of ammonium dihydrogen phosphate at 80°C and a current density of 30 mA / cm 2 , the voltage is 100V, and the primary formation is carried out for 6min;

[0054] Step S32: After washing and drying the corroded foil after the primary formation in step S31, place it in a 3% by mass aqueous solution of ammonium dihydrogen phosphate at 85°C and a current density of 30 mA / cm 2 , the voltage is 150V, and the secondary formation is carried out for 8 minutes;

[0055] Step S33: After washing and drying the corroded foil after the secondary formation in step S32, the foil is placed in an aqueous solution of 9% by mass boric acid and 0.6% by mass borate at 85°C and a current density of 40 mA / cm 2 Under the conditions of 210V voltage, three-stage formation is carried out, and the formation time is 10min.

[0056] Step S34: After washing and drying the corroded foil after the three-stage formation in S33, the foil is placed in an aqueous solution of 9% by mass boric acid and 0.6% by mass borate at 80°C and a current density of 20 mA / cm 2 Under the conditions of 220V voltage, four-stage formation is carried out and the formation time is 5min.

[0057] Step S4: using terephthalic acid as an organic ligand, adding terephthalic acid and a soluble aluminum salt into DMF at the same time (the molar ratio of the soluble aluminum salt to the organic ligand is 1:4), stirring to dissolve, and obtaining a reaction matrix solution of an aluminum-based metal organic framework, immersing the medium-pressure chemical foil precursor obtained in step S3 into the reaction matrix solution of the aluminum-based metal organic framework, stirring evenly to obtain a reaction mixed solution, raising the temperature of the reaction mixed solution to 110° C. and reacting for 50 minutes, so that the metal organic framework is in situ grown on the crystalline oxide film on the surface of the medium-pressure chemical foil precursor, and obtaining a metal organic framework-modified medium-pressure chemical foil.

[0058] Step S5: The metal organic framework modified medium pressure chemical foil obtained in step S4 is immersed in an organic silicon surfactant (non-ionic organic silicon surfactant) for 20 minutes to obtain an immersed medium pressure chemical foil. The concentration of the organic silicon surfactant in this step is 2.3 mL / L, and the temperature is controlled at 35°C.

[0059] Step S6: heat-treating the infiltrated medium-pressure chemical foil obtained in step S5 at 550° C. for 2 minutes to obtain a medium-pressure chemical foil semi-finished product.

[0060] Step S7: Place the medium-pressure chemically formed foil semi-finished product obtained in step S6 in a repair chemical solution (which has the same composition as the solution in the three-stage chemical step) for repair chemical formation. The repair chemical formation temperature is 90°C and the current density is 50 mA / cm 2 , the voltage is 220V, the repair forming time is 6min, and finally the medium voltage formed foil is obtained. Specific embodiment 3

[0062] A medium pressure chemical foil is provided, wherein the medium pressure chemical foil is based on a medium pressure chemical foil forming method, and the medium pressure chemical foil forming method comprises the following steps:

[0063] Step S1: placing the corroded foil in pure water at 98° C. for hydration treatment for 6 minutes, so that a porous oxide film is formed on the surface of the corroded foil.

[0064] Step S2: Immerse the corrosion foil after hydration treatment in step S1 in 2.5 mol / L ammonium chloride solution, expand the pores for 30 minutes, and then bake at 500° C. for 3 hours to obtain a corrosion foil containing a large-pore oxide film.

[0065] Step S3: The etched foil with large-aperture oxide film obtained in step S2 is subjected to four-stage medium-voltage electrochemical formation to densify the porous oxide film on the surface of the etched foil and form a dense crystalline oxide film to obtain a medium-voltage electrochemical foil precursor. The specific steps include the following steps (see Figure 2 ):

[0066] Step S31: Place the etched foil with large-aperture oxide film obtained in step S2 in a 3% by mass aqueous solution of ammonium dihydrogen phosphate at 78°C and a current density of 25 mA / cm 2 , the voltage is 80V, and the primary formation is carried out for 5min;

[0067] Step S32: After washing and drying the corroded foil after the primary formation in step S31, the foil is placed in a 1.2% by mass aqueous solution of ammonium dihydrogen phosphate at 82°C and a current density of 25 mA / cm 2 , the voltage is 100V, and the secondary formation is carried out for 6 minutes;

[0068] Step S33: After washing and drying the corroded foil after the secondary formation in step S32, the foil is placed in an aqueous solution of 8% by mass boric acid and 0.5% by mass borate at 82°C and a current density of 30 mA / cm 2 Under the conditions of 200V voltage, three-stage formation is carried out, and the formation time is 8min.

[0069] Step S34: After washing and drying the corroded foil after the three-stage formation in S33, the foil is placed in an aqueous solution of 8% by mass boric acid and 0.5% by mass borate at 90°C and a current density of 45 mA / cm 2 Under the conditions of 250V voltage, four-stage formation is carried out and the formation time is 8min.

[0070] Step S4: using terephthalic acid as an organic ligand, adding terephthalic acid and a soluble aluminum salt into DMF at the same time (the molar ratio of the soluble aluminum salt to the organic ligand is 1:3), stirring to dissolve, and obtaining a reaction matrix solution of an aluminum-based metal organic framework, immersing the medium-pressure chemical foil precursor obtained in step S3 into the reaction matrix solution of the aluminum-based metal organic framework, stirring evenly to obtain a reaction mixed solution, raising the temperature of the reaction mixed solution to 100° C. and reacting for 35 minutes, so that the metal organic framework is in situ grown on the crystalline oxide film on the surface of the medium-pressure chemical foil precursor, and obtaining a metal organic framework-modified medium-pressure chemical foil.

[0071] Step S5: The metal organic framework modified medium pressure chemical foil obtained in step S4 is soaked in an organosilicon surfactant (anionic organosilicon surfactant) for 15 minutes to obtain an soaked medium pressure chemical foil. The concentration of the organosilicon surfactant in this step is 1.8 mL / L, and the temperature is controlled at 28°C.

[0072] Step S6: heat-treating the infiltrated medium-pressure chemical foil obtained in step S5 at 500° C. for 2 minutes to obtain a medium-pressure chemical foil semi-finished product.

[0073] Step S7: Place the medium-pressure chemically formed foil semi-finished product obtained in step S6 in a repair chemical solution (which has the same solution composition as that in the three-stage chemical step) for repair chemical formation. The repair chemical formation temperature is 88°C and the current density is 40 mA / cm 2 , the voltage is 220V, the repair forming time is 5min, and finally the medium voltage forming foil is obtained.

[0074] The performance of the medium pressure chemical foils prepared in specific examples 1 to 3 was tested, and two groups of comparative examples were added: Comparative example 1: the steps were consistent with specific implementation 1, but no organosilicon surfactant treatment was performed; Comparative example 2: the steps were consistent with specific implementation 1, but no metal organic framework modification and organosilicon surfactant treatment were performed. The results are shown in Table 1:

[0075] Table 1 Performance test results of specific examples 1 to 3 and comparative examples

[0076] Serial number Voltage V <![CDATA[Capacitance μF / cm 2 > <![CDATA[Leakage current μA / cm 2 > Hydration resistance Specific embodiment 1 520 1.865 31 10 Specific embodiment 2 520 1.911 29 11 Specific embodiment 3 520 1.883 28 10 Comparative Example 1 520 1.469 52 15 Comparative Example 2 520 0.708 150 26

[0077] From the above data, it can be seen that the electrostatic capacitance of the medium-pressure formed foil prepared by the present invention has been significantly improved, and the maximum electrostatic capacitance is 1.911μF / cm 2 , which is close to 2.7 times the electrostatic capacitance of the electrochemical foil prepared by the conventional method; the leakage current of the medium-voltage electrochemical foil prepared by the present invention has been significantly improved, and the optimal leakage current is only 28μA / cm 2 , which is much lower than the leakage current of 150μA / cm of the chemically formed foil made by conventional methods. 2 , and the anti-hydration ability is also significantly enhanced. It can be seen that the present invention achieves the simultaneous improvement of electrostatic capacity and anti-hydration ability, and realizes the unity of the two.

[0078] From the above analysis, it can be seen that the present invention combines pore expansion treatment, multi-stage medium voltage electrochemical formation and metal organic framework modification: the selected pore expansion treatment method can effectively avoid the destruction of the pore structure caused by subsequent medium voltage electrochemical formation, so that the macroporous crystalline oxide film formed after the multi-stage medium voltage electrochemical formation is well preserved, thereby improving the specific capacity; on the other hand, the increased pore size is conducive to the diffusion of the metal organic framework into the crystalline oxide film after the multi-stage medium voltage electrochemical formation, so that the crystalline oxide film on the surface of the formed foil is in full contact with the metal organic framework, overcoming the problem of insufficient contact between the smaller pore size and the passivation agent, avoiding the hydrolysis of the crystalline oxide film on the surface of the corrosion foil, thereby exerting a passivation effect through the close combination of the metal organic framework and the crystalline oxide film substrate, thereby improving the water resistance of the formed foil, and achieving the unity of electrostatic capacitance and hydration resistance. The temperature, current and voltage conditions controlled by the selected multi-stage medium voltage electrification are not high, which reduces energy consumption and formation costs (also avoids the use of phosphoric acid, which is environmentally friendly), and the time for each step of formation is relatively short, which improves the formation efficiency. The selected metal organic framework forms an orderly network structure through the coordination of organic bridging ligands and inorganic metal ions, and has the advantages of high specific surface area, large pore size and adjustable pore size. It is in-situ grown on the crystalline oxide film on the surface of the formation foil, and is tightly combined and not easy to fall off, which can not only have a positive effect on the total pore volume of the formation foil, further improve the electrostatic capacity, but also can play a role in passivation of the crystalline oxide film on the surface of the formation foil, prevent its hydrolysis, and improve the water resistance of the formation foil, thus achieving the unity of the two.

[0079] The invention adopts an organic silicon surfactant to seal holes and optimize the surface. On the basis of surface modification of the medium-pressure chemical foil by an aluminum-based metal organic skeleton, the crystalline oxide film on the surface of the medium-pressure chemical foil is infiltrated, and the crystalline oxide film is further sealed to inhibit its hydration, thereby preventing the voltage resistance of the chemical foil from decreasing and the leakage current from increasing, and also preventing the porous aluminum-based metal organic skeleton from being polluted. Silicon atoms in the organic silicon are the main components of the organic silicon, and they are connected together by covalent bonds to form a stable three-dimensional network structure, thereby having higher electronic conductivity, specific capacity and good electrical performance, and further improving the specific capacity of the chemical foil. In addition, the basic structural unit of the organic silicon is composed of silicon-oxygen links, and the bond energy is relatively strong, so it has good thermal stability, chemical stability and mechanical performance, strong corrosion resistance and wear resistance, thereby enhancing the function of the chemical foil.

[0080] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A medium pressure chemical foil, the medium pressure chemical foil is based on a medium pressure chemical foil forming method, the medium pressure chemical foil forming method is characterized by: The following steps are involved: Step S1: placing the corroded foil in pure water above 96° C. for hydration treatment for 5-8 minutes, so that a porous oxide film is formed on the surface of the corroded foil; Step S2: immersing the corrosion foil after the hydration treatment in step S1 in a pore expanding agent, and calcining after the pore expanding treatment to obtain the corrosion foil containing the large-pore oxide film; Step S3: subjecting the etched foil with the large-pore oxide film obtained in step S2 to at least three levels of medium-voltage electrochemical formation, so that the porous oxide film on the surface of the etched foil is densified to form a dense crystalline oxide film, thereby obtaining a medium-voltage electrochemical foil precursor; Step S4: immersing the medium-pressure chemical foil precursor obtained in step S3 into the reaction matrix solution of the aluminum-based metal organic framework, stirring evenly to obtain a reaction mixed solution, raising the temperature of the reaction mixed solution to 80-110° C. and reacting for 20-50 minutes, so that the metal organic framework is in situ grown on the crystalline oxide film on the surface of the medium-pressure chemical foil precursor, and obtaining a metal organic framework-modified medium-pressure chemical foil; Step S5: soaking the metal organic framework modified medium pressure chemical foil obtained in step S4 in an organic silicon surfactant for 10-20 minutes to obtain a soaked medium pressure chemical foil; Step S6: heat-treating the infiltrated medium-pressure chemical foil obtained in step S5 at 450-550° C. for 2-3 minutes to obtain a medium-pressure chemical foil semi-finished product; Step S7: placing the medium-pressure chemically formed foil semi-finished product obtained in step S6 in a repair chemically formed liquid for repair chemically formed, and finally obtaining the medium-pressure chemically formed foil.

2. The medium pressure chemically formed foil according to claim 1, characterized in that: In step S2, the pore expanding agent is an ammonium chloride solution, and the concentration of the ammonium chloride solution is 1.5-6.5 mol / L.

3. The medium pressure chemical foil according to claim 1 or 2, characterized in that: The time of the hole expansion treatment in step S2 is 20-40 minutes, the temperature of the calcination is 400-600° C., and the time of the calcination is 2-5 hours.

4. The medium pressure chemically formed foil according to claim 1, characterized in that: The medium voltage electrification in step S3 is converted into a three-stage formation, comprising the following steps: Step S31: Place the etched foil with large-aperture oxide film obtained in step S2 in a 2-5% by mass aqueous solution of ammonium dihydrogen phosphate at 75-80°C and a current density of 20-30 mA / cm 2 , the voltage is 70-100V, and the primary formation is carried out for 3-6min; Step S32: After washing and drying the corroded foil after the primary formation in step S31, place it in a 0.1-3% by mass aqueous solution of ammonium dihydrogen phosphate at 80-85°C and a current density of 20-30 mA / cm 2 , under the condition of voltage of 80-150V, the secondary formation is carried out, and the formation time is 5-8min; Step S33: After washing and drying the corroded foil after the secondary formation in step S32, place it in an aqueous solution of 6-9% by mass boric acid and 0.4-0.6% by mass borate at 80-85°C and a current density of 20-40 mA / cm 2 , under the condition of voltage of 180-210V, three-stage formation is carried out, and the formation time is 6-10min.

5. The medium pressure chemically formed foil according to claim 4, characterized in that: The medium voltage electrification in step S3 is a four-stage formation, which includes a three-stage formation, and the four-stage formation also includes step S34: washing and drying the corroded foil after the three-stage formation in step S33, placing it in an aqueous solution of 6-9% boric acid and 0.4-0.6% borate by mass, at 80-90°C and a current density of 20-45 mA / cm 2 , under the condition of voltage of 220-250V, four-stage formation is carried out, and the formation time is 5-8min.

6. The medium pressure chemical foil according to claim 4 or 5, characterized in that: The composition of the repairing solution in step S7 is the same as that of the solution in the three-stage formation step, and the temperature of the repairing formation is 85-90°C, and the current density of the repairing formation is 20-50 mA / cm 2 The voltage of the repair formation is 200-220V, and the time of the repair formation is 3-6min.

7. The medium pressure chemically formed foil according to claim 1, characterized in that: In step S4, the aluminum-based metal organic framework uses terephthalic acid as an organic ligand, and the preparation method of the reaction matrix solution of the aluminum-based metal organic framework is to add terephthalic acid and a soluble aluminum salt into DMF at the same time, stir and dissolve them, and then react to obtain the solution.

8. The medium pressure chemically formed foil according to claim 7, characterized in that: The molar ratio of the soluble aluminum salt to the organic ligand in step S4 is 1:(1-4).

9. The medium pressure chemically formed foil according to claim 1, characterized in that: In step S5, the concentration of the organosilicon surfactant is 0.5-2.3 mL / L, and the temperature of the organosilicon surfactant is controlled at 25-35°C.

10. The medium pressure chemically formed foil according to claim 1 or 9, characterized in that: The organosilicon surfactant is an anionic organosilicon surfactant or a nonionic organosilicon surfactant.