Positive electrode lithium supplement material and preparation method thereof, slurry, pole piece, and lithium ion battery

By coating the surface of organic lithium salt lithium replenishment materials with ordered mesoporous carbon to form a core-shell structure, the problems of poor conductivity and high delithiation potential of organic lithium salt lithium replenishment materials are solved, thereby improving the performance of lithium-ion batteries.

CN118572092BActive Publication Date: 2024-11-01JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411038517.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-01
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Organic lithium salt lithium replenishment materials have poor conductivity and high delithiation potential, making it difficult to match the operating voltage of most commercial cathode materials, thus hindering their practical application.

Method used

A micelle solution was formed by mixing triblock copolymer F127 with phenolic resin prepolymer. Ordered mesoporous carbon was then coated onto the surface of the organic lithium salt lithium supplement material through a hydrothermal reaction to form a core-shell structure. This controlled the size and pore distribution of the core and shell layers, thereby reducing the delithiation potential and improving conductivity.

Benefits of technology

It improves the overall conductivity and lithium-ion migration rate of the positive electrode lithium replenishment material, reduces the delithiation potential, and enhances the electrochemical performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118572092B_ABST
    Figure CN118572092B_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode lithium supplement material and a preparation method thereof, slurry, pole piece, and lithium ion battery. The positive electrode lithium supplement material is a core-shell structure including a core and a shell layer, the material of the core includes an organic lithium salt lithium supplement material, and the material of the shell layer includes ordered mesoporous carbon. The above-mentioned positive electrode lithium supplement material uses an organic lithium salt lithium supplement material as a core, and coats the organic lithium salt lithium supplement material with ordered mesoporous carbon as a shell layer. The coating of the ordered mesoporous carbon can improve the overall conductivity of the positive electrode lithium supplement material. After carbon coating, the organic lithium salt lithium supplement material exists in the form of nanoparticles. The dynamics of the nanoparticles are better, which is conducive to the extraction and embedding of lithium ions. In addition, the orderly distributed pore space in the ordered mesoporous carbon has a higher utilization rate than the disordered distribution, and there are more reactive active sites, which reduces the delithiation potential of the organic lithium salt lithium supplement material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochemical energy storage, and in particular to a positive electrode lithium supplement material and a preparation method thereof, a positive electrode slurry, a positive electrode sheet, and a lithium ion battery. Background Art

[0002] As an electrochemical energy storage device, lithium-ion batteries (LIBs) have the advantages of high energy density and long service life, and therefore have attracted widespread attention. In the initial few charge and discharge cycles of lithium-ion batteries, a solid electrolyte interface (SEI) will be formed. This process consumes a large amount of active lithium, causing irreversible capacity loss, reducing the energy density and cycle life of the battery.

[0003] In order to compensate for the irreversible capacity loss of lithium-ion batteries during the initial cycle, pre-lithiation technology can be used. Pre-lithiation technology mainly includes two methods: negative electrode lithium replenishment and positive electrode lithium replenishment. Among them, negative electrode lithium replenishment generally has problems such as complex process, low safety, and high process requirements. Positive electrode lithium replenishment usually adopts electrochemical method, by adding lithium replenishment additives to the positive electrode of lithium-ion battery. During the battery charging process, the lithium replenishment additives decompose to release active lithium, which compensates for the loss of active lithium caused by the growth of negative electrode SEI. Compared with negative electrode lithium replenishment, the positive electrode lithium replenishment process is relatively simple. The positive electrode lithium replenishment additive can be directly added during the homogenization process of the positive electrode slurry, without the need for additional process improvements, and the cost is low.

[0004] Traditional positive electrode lithium supplement additives are mainly inorganic pre-lithiation compounds, in addition to organic lithium salts. Inorganic pre-lithiation compounds are very sensitive to air and water, and are prone to violent reactions with air and water, which can be dangerous. Organic lithium salt lithium supplement materials have good air stability and high theoretical capacity, so they have greater application potential. However, most organic lithium salt lithium supplement materials have poor conductivity, resulting in their actual capacity being far lower than the theoretical capacity, and the delithiation potential of organic lithium salt lithium supplement materials is too high, making it difficult to match the operating voltage of most commercial positive electrode materials, hindering their practical application. Summary of the invention

[0005] Based on this, it is necessary to provide a positive electrode lithium replenishing material and its preparation method, positive electrode slurry, positive electrode plate, and lithium ion battery to solve the problems of poor conductivity and high delithiation potential of organic lithium salt lithium replenishing materials.

[0006] The first aspect of the present invention is to provide a method for preparing a positive electrode lithium supplement material, the scheme is as follows:

[0007] A method for preparing a positive electrode lithium supplement material comprises the following steps:

[0008] The solution of triblock copolymer F127 is mixed with the solution of phenolic resin prepolymer, and reacted at 60°C to 100°C until the reaction solution becomes turbid to obtain a micellar solution;

[0009] Taking an organic lithium salt lithium supplement material and a surfactant and dissolving them in water, adjusting the pH value of the solution to 7-10, adding a hydroxylamine hydrochloride solution, mixing evenly, performing a centrifugal washing treatment, and drying to obtain a pre-treated lithium supplement agent;

[0010] The pretreated lithium supplement agent is mixed with the micelle solution, and subjected to a hydrothermal reaction at 100° C. to 160° C. for 8 h to 36 h to obtain a hydrothermal reaction product;

[0011] The hydrothermal reaction product is calcined to obtain a positive electrode lithium supplement material, wherein the positive electrode lithium supplement material is a core-shell structure including a core and a shell layer, the material of the core layer includes the organic lithium salt lithium supplement material, and the material of the shell layer includes ordered mesoporous carbon.

[0012] In one embodiment, the solution of the phenolic resin prepolymer is prepared by the following method:

[0013] Mix phenol and formaldehyde with a phenol-formaldehyde ratio of 1:(1.5~3), adjust the pH value of the solution to 7~10, and react at 60℃~80℃ for 30min~2h.

[0014] In one embodiment, the organic lithium salt lithium supplement material is prepared by the following method:

[0015] The organic lithium salt, water and ethanol are mixed in a mass ratio of 1: (0-10): (10-20), heated at 60°C-100°C for 6h-48h, filtered and dried to obtain the organic lithium salt lithium supplement material.

[0016] In one embodiment, the calcination treatment is performed at a temperature of 200°C to 600°C and for a time of 3h to 6h.

[0017] In one embodiment, the particle size of the core is 100nm~20μm.

[0018] In one embodiment, the thickness of the shell layer is 2nm~20nm.

[0019] In one embodiment, the pore size of the shell layer is 2nm~50nm.

[0020] In one embodiment, the specific surface area of ​​the shell is 100m 2 / g~600m 2 / g.

[0021] In one embodiment, the organic lithium salt lithium supplement material is selected from Li 2 C 2 O 4 , Li 2 C 3 O 3 , Li 2 C 4 O 4 , Li 2 C 5 O 5 , Li 2 C 6 O 6 , Li 2 C 4 O 6 、[COCON(Li)N(Li)] n and Li 2 At least one of DHBN.

[0022] The second aspect of the present invention is to provide a positive electrode lithium supplement material, which is prepared by the preparation method described in any of the above embodiments.

[0023] The third aspect of the present invention is to provide a positive electrode slurry, the scheme is as follows:

[0024] A positive electrode slurry comprises the positive electrode lithium supplement material described in any one of the above embodiments and a solvent, wherein the positive electrode lithium supplement material is dispersed in the solvent.

[0025] The fourth aspect of the present invention is to provide a positive electrode plate, the scheme is as follows:

[0026] A positive electrode plate comprises a positive electrode current collector and a positive electrode material layer arranged on the positive electrode current collector, wherein the positive electrode material layer comprises the positive electrode lithium supplement material described in any one of the above embodiments.

[0027] A fifth aspect of the present invention is to provide a lithium ion battery, the scheme is as follows:

[0028] A lithium-ion battery comprises a shell, a positive electrode sheet, a negative electrode sheet, a diaphragm and an electrolyte, wherein the positive electrode sheet, the negative electrode sheet, the diaphragm and the electrolyte are arranged in the shell, the positive electrode sheet and the negative electrode sheet are arranged opposite to each other, and the diaphragm is located between the positive electrode sheet and the negative electrode sheet.

[0029] Compared with the traditional solution, the above-mentioned positive electrode lithium supplement material and preparation method thereof, positive electrode slurry, positive electrode sheet, and lithium-ion battery have the following beneficial effects:

[0030] The above-mentioned positive electrode lithium replenishing material has an organic lithium salt lithium replenishing material as the core, and an ordered mesoporous carbon is coated on the organic lithium salt lithium replenishing material as a shell layer. The coating of ordered mesoporous carbon can improve the overall conductivity of the positive electrode lithium replenishing material. After carbon coating, the organic lithium salt lithium replenishing material exists in the form of nanoparticles. The dynamics of nanoparticles are better, which is conducive to the extraction and embedding of lithium ions. In addition, the orderly distributed pore space in the ordered mesoporous carbon has a higher utilization rate than the disordered distribution, and there will be more reaction active sites, which reduces the delithiation potential of the organic lithium salt lithium replenishing material.

[0031] The above preparation method uses a solution of triblock copolymer F127 and a phenolic resin prepolymer to mix and react to obtain a micellar solution, wherein a low molecular weight phenolic resin prepolymer is used as a carbon source for the shell layer, and the triblock copolymer F127 is a soft template to regulate the mesoporous structure; the organic lithium salt lithium supplement material is mixed with a surfactant and hydroxylamine hydrochloride for pretreatment to regulate the core size of the organic lithium salt lithium supplement material. Under alkaline conditions, the OH group of hydroxylamine hydrochloride is deprotonated and combined with the phenolic resin, which is conducive to the polymerization of the phenolic resin; the pretreated lithium supplement agent is then mixed with the micellar solution and subjected to a hydrothermal reaction to achieve an ordered distribution of the pores. The orderly distributed pore space has a higher utilization rate than the disordered distribution, and there are more reactive sites; the shell layer is then carbonized by calcination to form an ordered mesoporous carbon, and an ordered mesoporous carbon-coated core-shell structure of an organic lithium salt lithium supplement material is obtained. The above preparation method can improve the overall conductivity of the positive electrode lithium supplement material and reduce the delithiation potential of the organic lithium supplement agent by coating the ordered mesoporous carbon on the surface of the organic lithium supplement agent.

[0032] The above-mentioned positive electrode slurry, positive electrode plate, and lithium-ion battery contain the positive electrode lithium supplement material described in any of the above-mentioned embodiments, and thus have corresponding technical characteristics and can obtain corresponding beneficial effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] FIG1 is a schematic flow diagram of a method for preparing a positive electrode lithium supplement material according to an embodiment of the present invention;

[0034] FIG. 2 is a TEM image of the positive electrode lithium supplement material prepared in Example 1. DETAILED DESCRIPTION

[0035] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are shown in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. The purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0036] In the description of the present invention, it should be understood that the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number or order of the indicated technical features.

[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0038] The invention provides a positive electrode lithium supplement material.

[0039] The positive electrode lithium supplement material of one embodiment is a core-shell structure, which includes a core and a shell layer, wherein the shell layer is wrapped around the core. The material of the core includes an organic lithium salt lithium supplement material. The material of the shell layer includes ordered mesoporous carbon.

[0040] The above-mentioned positive electrode lithium replenishing material has an organic lithium salt lithium replenishing material as the core, and an ordered mesoporous carbon is coated on the organic lithium salt lithium replenishing material as a shell layer. The coating of ordered mesoporous carbon can improve the overall conductivity of the positive electrode lithium replenishing material. After carbon coating, the organic lithium salt lithium replenishing material exists in the form of nanoparticles. The dynamics of nanoparticles are better, which is conducive to the extraction and embedding of lithium ions. In addition, the orderly distributed pore space in the ordered mesoporous carbon has a higher utilization rate than the disordered distribution, and there will be more reaction active sites, which reduces the delithiation potential of the organic lithium salt lithium replenishing material.

[0041] In some of the examples, in the core-shell structure, the particle size of the core is 100nm~20μm. The particle size of the core is at the micro-nano level, which gives it a large specific surface area, high reactivity, and low delithiation potential. Further, the particle size of the core is 200nm~10μm. Further, the particle size of the core is 200nm~1μm.

[0042] In some specific examples, the particle size of the core is 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1μm, 2μm, 4μm, 6μm, 8μm, 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, etc.

[0043] The coating of the ordered mesoporous carbon shell can improve the overall conductivity of the positive electrode lithium supplement material. If the shell is too thin, the coating effect is poor, and the improvement of conductivity is relatively limited. However, if the shell is too thick, the lithium ion migration channel will become longer and the lithium ion migration rate will be reduced. Taking all factors into consideration, in the core-shell structure, the thickness of the shell is 2nm~20nm. Furthermore, the thickness of the shell is 5nm~15nm to better balance the conductivity and lithium ion migration rate of the positive electrode lithium supplement material. Furthermore, the thickness of the shell is 8nm~12nm to better balance the conductivity and lithium ion migration rate of the positive electrode lithium supplement material.

[0044] In some specific examples, the thickness of the shell layer is 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm, etc.

[0045] The larger the pore size of the shell layer, the more conducive it is to the release of lithium ions. At the same time, in order to maintain a good conductive effect of the shell layer, the pore size of the shell layer is preferably set to 2nm~60nm. Further, the pore size of the shell layer is 20nm~50nm. Further, the pore size of the shell layer is 10nm~50nm.

[0046] In some specific examples, the pore size of the shell is 2nm, 5nm, 8nm, 11nm, 14nm, 17nm, 20nm, 23nm, 26nm, 29nm, 32nm, 35nm, 38nm, 41nm, 44nm, 47nm, 50nm, etc.

[0047] The larger the specific surface area of ​​the shell and the smaller the particle size, the more favorable it is for the delithiation reaction. In some examples, the specific surface area of ​​the shell is 100m 2 / g~600m 2 / g. Furthermore, the specific surface area of ​​the shell layer is 200m 2 / g~600m 2 / g. Furthermore, the specific surface area of ​​the shell is 300m 2 / g~600m 2 / g.

[0048] In some specific examples, the specific surface area of ​​the shell is 100m 2 / g, 125m 2 / g, 150m 2 / g, 175m 2 / g, 200m 2 / g, 225m 2 / g, 250m 2 / g, 275m 2 / g、300m 2 / g, 325m 2 / g, 350m 2 / g, 375m 2 / g, 400m 2 / g, 425m 2 / g, 450m 2 / g, 475m 2 / g、500m 2 / g, 525m 2 / g, 550m 2 / g, 575m 2 / g、600m 2 / g, etc.

[0049] The thermal decomposition temperature of the organic lithium salt lithium supplement material is preferably above 200°C, for example, 200°C to 600°C, to prevent the organic lithium salt lithium supplement material from decomposing when the ordered mesoporous carbon is formed. The thermal decomposition temperature of the organic lithium salt lithium supplement material is more preferably above 250°C. The thermal decomposition temperature of the organic lithium salt lithium supplement material is further preferably above 300°C. The thermal decomposition temperature of the organic lithium salt lithium supplement material is further preferably above 350°C. The thermal decomposition temperature of the organic lithium salt lithium supplement material is further preferably above 400°C.

[0050] Optionally, the organic lithium salt lithium supplement material may be, but is not limited to, Li 2 C 2 O 4 (lithium oxalate), Li 2 C 3 O 5 (lithium acetonate), Li 2 C 4 O 4 (lithium squarate), Li 2 C 5 O 5 (Lithium Pentaquarate), Li 2 C 6 O 6 (lithium kojic acid), Li 2 C 4 O 6 (lithium diketosuccinate), [COCON(Li)N(Li)] n (Polyimide lithium), Li 2 At least one of DHBN (dilithium 3,4-dihydroxybenzonitrile).

[0051] Furthermore, the present invention also provides a method for preparing the positive electrode lithium supplement material of any of the above examples.

[0052] As shown in FIG1 , a method 10 for preparing a positive electrode lithium supplement material according to an embodiment includes the following steps:

[0053] Step S100, mixing a solution of the triblock copolymer F127 with a solution of a phenolic resin prepolymer to obtain a mixed solution, reacting at 60° C. to 100° C. until the reaction solution becomes turbid, thereby obtaining a micellar solution.

[0054] Step S200, dissolving an organic lithium salt lithium supplement material and a surfactant in water, adjusting the pH value of the solution to 7-10, adding a hydroxylamine hydrochloride solution, mixing evenly, performing a centrifugal washing treatment, and drying to obtain a pre-treated lithium supplement agent.

[0055] Step S300, mixing the pretreated lithium supplement agent with the micelle solution, and subjecting the mixture to a hydrothermal reaction at 100° C. to 160° C. for 8 h to 36 h to obtain a hydrothermal reaction product.

[0056] Step S400, burning the hydrothermal reaction product to obtain a positive electrode lithium supplement material.

[0057] The above preparation method uses a solution of triblock copolymer F127 and a phenolic resin prepolymer to mix and react to obtain a micellar solution, wherein a low molecular weight phenolic resin prepolymer is used as a carbon source for the shell layer, and the triblock copolymer F127 is a soft template to regulate the mesoporous structure; the organic lithium salt lithium supplement material is mixed with a surfactant and hydroxylamine hydrochloride for pretreatment to regulate the core size of the organic lithium salt lithium supplement material. Under alkaline conditions, the OH group of hydroxylamine hydrochloride is deprotonated and combined with the phenolic resin, which is conducive to the polymerization of the phenolic resin; the pretreated lithium supplement agent is then mixed with the micellar solution and subjected to a hydrothermal reaction to achieve an ordered distribution of the pores. The orderly distributed pore space has a higher utilization rate than the disordered distribution, and there are more reactive sites; the shell layer is then carbonized by calcination to form an ordered mesoporous carbon, and an ordered mesoporous carbon-coated core-shell structure of an organic lithium salt lithium supplement material is obtained. The above preparation method can improve the overall conductivity of the positive electrode lithium supplement material and reduce the delithiation potential of the organic lithium supplement agent by coating the ordered mesoporous carbon on the surface of the organic lithium supplement agent.

[0058] The above preparation method has simple process, low cost, no obvious destruction or damage to the battery system, and has a wide range of adaptability.

[0059] In some of the examples, in step S100, in the mixed solution, the concentration of the triblock copolymer F127 is 5 g / L-50 g / L, for example, 5 g / L, 10 g / L, 20 g / L, 30 g / L, 40 g / L, 50 g / L, etc.

[0060] In some of the examples, in step S100, in the mixed solution, the concentration of the phenolic resin prepolymer is 50 g / L-500 g / L, for example, 50 g / L, 100 g / L, 200 g / L, 300 g / L, 400 g / L, 500 g / L, etc.

[0061] In some of the examples, in step S100, a mixed solution of the triblock copolymer F127 and the phenolic resin prepolymer is first reacted at 60°C to 100°C for 2h to 6h, diluted with water, and then continued to react for 12h to 56h until the reaction solution becomes turbid.

[0062] In some of these examples, a solution of phenolic resin prepolymer is prepared by:

[0063] Mix phenol and formaldehyde in a phenol-formaldehyde ratio of 1:(1.5-3), adjust the solution pH to 7-10, and react at 60°C-80°C for 30min-2h to obtain a low molecular weight phenolic resin prepolymer.

[0064] Before the reaction in step S200, the organic lithium salt lithium supplement material is preferably recrystallized in a poor solvent to adjust its grain size. The recrystallization step includes: mixing the organic lithium salt with its poor solvent, heating at 60°C to 100°C for 6h to 48h, filtering and drying to obtain a recrystallized organic lithium salt lithium supplement material.

[0065] Poor solvents include water, ethanol, etc. In some examples, the organic lithium salt, water and ethanol are mixed in a mass ratio of 1: (0-10): (10-20). Further, the organic lithium salt, water and ethanol are mixed in a mass ratio of 1: (1-8): (10-20).

[0066] By recrystallizing the organic lithium salt in a poor solvent, the size of the organic lithium salt crystalline particles is smaller than before recrystallization, that is, the core size of the core-shell structure is smaller, the dynamics of the nanoparticles is better, which is conducive to the extraction and embedding of lithium ions. At the same time, it can also have better conductivity after carbon coating.

[0067] In some of the examples, in step S200, the surfactant is one or more of sodium dodecylbenzene sulfonate, sodium secondary alkyl sulfonate, and sodium fatty alcohol ether sulfate. In some of the examples, the surfactant is sodium dodecyl sulfonate.

[0068] In some of the examples, in step S200, the mass ratio of the organic lithium salt lithium supplement material to the surfactant is 1:(6-15), specifically 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, etc.

[0069] In some of the examples, in step S200, the mass ratio of the organic lithium salt lithium supplement material to hydroxylamine hydrochloride is 1:0.05-0.1, specifically 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.1, etc.

[0070] In some of the examples, in step S200, the centrifugal washing process includes successively using ethanol and acetone for centrifugal washing for multiple times, for example, successively using ethanol and acetone for centrifugal washing for three times.

[0071] In some of the examples, the mass ratio of the pretreatment lithium supplement agent to the micelle solution is 1:1.5-3, such as 1:1.5, 1:1.7, 1:1.9, 1:2.1, 1:2.3, 1:2.5, 1:2.7, 1:2.9, 1:3, etc.

[0072] In some examples, in step S400, the temperature of the calcination treatment is 200°C to 600°C, for example, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, etc. The time of the calcination treatment is 3h to 6h, for example, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, etc.

[0073] It should be understood that although the steps in the flowchart shown in FIG1 are shown in sequence as indicated by the arrows, these steps are not necessarily performed in the order indicated by the arrows. Unless otherwise specified herein, there is no strict order restriction for the execution of these steps, and they can be performed in other orders.

[0074] Furthermore, the present invention also provides a positive electrode slurry, which comprises any of the positive electrode lithium supplement materials in the above examples.

[0075] Specifically, the positive electrode slurry of an embodiment includes a positive electrode lithium supplement material and a solvent. The positive electrode lithium supplement material is dispersed and mixed in the solvent.

[0076] The positive electrode slurry may further include a positive electrode active material. The positive electrode active material is dispersed in a solvent. In some examples, the mass fraction of the positive electrode active material in the positive electrode slurry is 5% to 90%. The mass fraction of the positive electrode lithium supplement material in the positive electrode slurry is 5% to 90%. The mass fraction of the solvent in the positive electrode slurry is 5% to 90%.

[0077] Illustratively, the positive electrode active material includes one or more of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, and lithium nickel cobalt manganese oxide.

[0078] It is understood that the positive electrode slurry may further include a positive electrode binder, a positive electrode conductor, etc. The mass fraction of the positive electrode binder in the positive electrode slurry is, for example, 2.0% to 5.0%. The mass fraction of the positive electrode conductor in the positive electrode slurry is, for example, 2.0% to 5.0%.

[0079] For example, the positive electrode binder includes one or more of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, epoxy resin and nylon. For example, the positive electrode conductor includes one or more of graphite, carbon black, acetylene black and Ketjen black.

[0080] Illustratively, the solvent includes one or more of water and N-methylpyrrolidone.

[0081] Furthermore, the present invention also provides a positive electrode plate, which comprises any of the positive electrode lithium supplement materials in the above examples.

[0082] Specifically, the positive electrode sheet of an embodiment includes a positive electrode current collector and a positive electrode material layer disposed on the positive electrode current collector. The positive electrode material layer includes a positive electrode lithium supplement material.

[0083] The positive electrode material layer may further include a positive electrode active material, and the positive electrode lithium supplement material is mixed with the positive electrode active material.

[0084] Illustratively, the positive electrode current collector includes metal foil such as aluminum foil and copper foil.

[0085] The positive electrode material layer may further include a positive electrode binder, a positive electrode conductor, etc. The positive electrode active material, the positive electrode binder and the positive electrode conductor may be the materials listed in the positive electrode slurry above, which will not be described in detail here.

[0086] In some examples, the active material surface density of the positive electrode sheet is 8 mg / cm 2 ~10mg / cm 2 The compaction density of the positive electrode is 1.6 mg / cm 3 ~1.9mg / cm 3 .

[0087] The positive electrode sheet can be prepared by coating the positive electrode slurry on the positive electrode current collector, and then drying to remove the solvent to form a positive electrode material layer on the positive electrode current collector.

[0088] Furthermore, the present invention also provides a lithium-ion battery, which includes the positive electrode sheet of any of the above examples.

[0089] More specifically, the lithium-ion battery includes a housing, a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet, the negative electrode sheet, the separator and the electrolyte are arranged in the housing. The positive electrode sheet and the negative electrode sheet are arranged opposite to each other. The separator is between the positive electrode sheet and the negative electrode sheet.

[0090] The negative electrode plate includes a negative electrode current collector and a negative electrode material layer arranged on the negative electrode current collector.

[0091] Illustratively, the negative electrode current collector includes metal foil such as aluminum foil and copper foil.

[0092] The negative electrode material layer contains a negative electrode active material. Exemplarily, the negative electrode active material includes one or more of natural graphite, artificial graphite, soft carbon, hard carbon, lithium metal, lithium metal alloy and transition metal oxide.

[0093] It is understood that the negative electrode material layer may further include a negative electrode binder, a negative electrode conductor, etc. Exemplarily, the negative electrode binder includes one or more of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, epoxy resin, and nylon. Exemplarily, the negative electrode conductor includes one or more of graphite, carbon black, acetylene black, and Ketjen black.

[0094] The positive electrode sheet and the negative electrode sheet can be prepared by mixing and dispersing the corresponding active material, binder and conductive agent in a solvent to obtain a slurry, then coating the slurry on the corresponding current collector, and then drying to remove the solvent to form a corresponding active material layer on the current collector.

[0095] The diaphragm includes a polymer film material. For example, the material of the polymer film material includes one or more of polyethylene, polypropylene and polyvinylidene fluoride. The diaphragm can be a single-layer diaphragm or a multi-layer diaphragm.

[0096] The electrolyte includes a solvent and a lithium salt dispersed in the solvent. For example, the lithium salt includes LiPF 6 , LiBF 4 、LiClO 4 、LiAsF 6 、LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2 , LiBOB, LiDFOB, LiFSI and LiTFSI. Exemplarily, the solvent includes one or more of ethylene carbonate, fluoroethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl formate, ethyl formate, methyl acetate, ethyl acetate, ethyl propionate, propyl propionate, ethyl butyrate and propyl butyrate.

[0097] It is understood that the electrolyte may further include additives, for example, fluoroethylene carbonate, vinylene carbonate, and chloroethylene carbonate.

[0098] The following specific examples are provided to further illustrate the present invention. The present invention provides the following specific examples for a better understanding of the present invention, but is not limited to the specific implementation methods, and does not limit the content and protection scope of the present invention.

[0099] Example 1

[0100] This embodiment provides a positive electrode lithium supplement material and a preparation method thereof.

[0101] The preparation method of the positive electrode lithium supplement material comprises the following steps:

[0102] Step 1: Organic lithium salt lithium supplement material Li 2 C 2 O 4 Recrystallization treatment.

[0103] 0.3 mol of organic lithium salt Li 2 C 2 O 4 Dissolve in 120 ml of deionized water, add 240 ml of ethanol, stir, and place in an oil bath at 60 °C for 12 h. Filter and dry to obtain recrystallized Li 2 C 2 O 4 .

[0104] Step 2, preparing a solution of phenolic resin prepolymer.

[0105] Take a 38% formaldehyde solution and a 0.1 mol / L sodium hydroxide solution, mix them in a volume ratio of 1:5. Then add 0.006 mol of phenol, the phenol-formaldehyde ratio is about 1:1.5, and react the mixed solution in an oil bath at 60°C for 30 minutes to obtain a low molecular weight phenolic resin prepolymer solution.

[0106] Step 3, preparing micelle solution.

[0107] The solution containing 1.08 g of triblock copolymer F127 was mixed evenly with the solution of phenolic resin prepolymer obtained in step 2, and stirred in an oil bath at 70° C. for 2 h. An appropriate amount of deionized water was added to dilute the reaction solution. After 12 h of reaction, the reaction solution became turbid, and the reaction was terminated to obtain a micellar solution.

[0108] Step 4, preparing a pre-treatment lithium supplement agent.

[0109] Take 0.1mmol recrystallized Li 2 C 2 O 4 , 0.6mmol sodium dodecyl sulfate was dissolved in deionized water, and 15ml of 1mol / L sodium hydroxide solution was added dropwise at 35℃ oil bath to adjust the solution pH to 8.5. After cooling to room temperature, 0.08mmol hydroxylamine hydrochloride solution was added. After mixing evenly, the solution was washed by centrifugation three times with ethanol and acetone respectively, and dried to obtain a pretreated lithium supplement agent.

[0110] Step 5, hydrothermal reaction.

[0111] The pre-treated lithium supplement agent was made into a solution, mixed with 5 ml of the micelle solution, and hydrothermally reacted at 120° C. for 12 h. The reactor was taken out and cooled to room temperature, centrifuged and washed three times, and dried at 80° C. for 12 h to obtain a hydrothermal reaction product.

[0112] Step 6: Burning treatment.

[0113] The hydrothermal reaction product was calcined at 450 °C for 6 h to obtain an ordered mesoporous carbon shell coated with Li 2 C 2 O 4 The core's positive electrode lithium replenishing material.

[0114] FIG2 is a transmission electron microscope (TEM) image of the positive electrode lithium replenishing material prepared in Example 1. As can be seen from FIG2, the positive electrode lithium replenishing material is a core-shell structure. The core of the core-shell structure is the organic lithium replenishing agent Li 2 C 2 O 4 , the shell layer is a mesoporous carbon layer.

[0115] Example 2

[0116] The steps of this embodiment are basically the same as those of embodiment 1, except that the organic lithium salt lithium supplement material is Li 2 C 4 O 4 .

[0117] Example 3

[0118] The steps of this embodiment are basically the same as those of embodiment 1, except that the organic lithium salt lithium supplement material is Li 2 C 4 O 6 .

[0119] Example 4

[0120] The steps of this embodiment are basically the same as those of embodiment 1, except that step 1 is not performed, that is, the organic lithium salt lithium supplement material Li 2 C 2 O 4 Recrystallization was performed.

[0121] Comparative Example 1

[0122] Compared with Example 1, this comparative example only performs step 1, that is, only the organic lithium salt lithium supplement material Li 2 C 2 O 4 Recrystallization was performed, but steps 2 to 6 were not performed.

[0123] The positive electrode lithium supplement materials prepared in the above-mentioned embodiments and comparative examples are respectively used to prepare lithium supplement half-cells. The difference between the lithium supplement half-cells is only that the positive electrode lithium supplement materials are different.

[0124] The preparation method of the lithium supplemented half-cell comprises the following steps:

[0125] Step 1: Prepare the positive electrode.

[0126] Take the positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O 2 , positive electrode lithium supplement material, conductive carbon black and polyvinylidene fluoride, the mass ratio is 94:2.5:1.5:2. Add the positive electrode active material and positive electrode lithium supplement material into N-methylpyrrolidone solvent, add polyvinylidene fluoride, stir and mix evenly, then add conductive carbon black to make positive electrode slurry. Coat the positive electrode slurry on aluminum foil, press and cut into discs with a diameter of 14 mm, and the active material surface density is 6.5 mg / cm 2 , compacted density is 2.1 mg / cm 3 , and vacuum dried at 80 °C for 12 h to obtain the positive electrode sheet, which was then cooled and placed in a glove box for later use.

[0127] Step 2, battery assembly.

[0128] The button cell is assembled in the order of placing the negative electrode shell, lithium sheet, diaphragm, positive electrode sheet, gasket, spring sheet, and positive electrode shell. The diaphragm is a polyethylene diaphragm. The electrolyte uses EC (ethylene carbonate) and EMC (ethyl methyl carbonate) with a mass ratio of 3:7 as solvents, VC (vinyl carbonate) is added as an additive with a mass fraction of 3%, and LiFP is added. 6 As lithium salt, the mass fraction is 12.5%. The amount of electrolyte added is 80 μL.

[0129] After the button cell was assembled, it was packaged with a press and left to stand for 12 hours before the electrochemical performance test was performed. The test results are shown in Table 1.

[0130] Table 1

[0131]

[0132] It can be seen from the experimental data in Table 1 that the electrochemical performance of the button cells using the positive electrode lithium replenishment materials of Examples 1 to 3 is significantly better than that of Comparative Example 1. Compared with the organic lithium salt lithium replenishment material of Comparative Example 1, the positive electrode lithium replenishment materials with a core-shell structure obtained by coating the organic lithium salt lithium replenishment material with ordered mesoporous carbon have all been well utilized. In Example 4, the lithium oxalate was not recrystallized, and the primary particle size of the lithium oxalate was relatively large. Although the mesoporous carbon was subsequently coated, the coating effect was not as good as that of the lithium oxalate after recrystallization, and the gram capacity and electrochemical impedance were relatively poor.

[0133] The positive electrode lithium supplement materials prepared in the above-mentioned embodiments and comparative examples are used to prepare pairs of lithium half-cells, respectively. The difference between the pairs of lithium half-cells is only the difference in the positive electrode lithium supplement materials.

[0134] The preparation method of the lithium half-cell comprises the following steps:

[0135] Step 1: Prepare the positive electrode.

[0136] Take positive electrode lithium supplement material, conductive carbon black and polyvinylidene fluoride, with a mass ratio of 96.5:1.5:2. Add the positive electrode lithium supplement material to N-methylpyrrolidone solvent, add polyvinylidene fluoride, stir and mix evenly, and then add conductive carbon black to make positive electrode slurry. Coat the positive electrode slurry on aluminum foil, press and cut into discs with a diameter of 14 mm, vacuum dry at 80°C for 12 hours to obtain the positive electrode sheet, and place it in a glove box for standby after cooling.

[0137] Step 2, battery assembly.

[0138] The button cell is assembled in the order of placing the negative electrode shell, lithium sheet, diaphragm, positive electrode sheet, gasket, spring sheet, and positive electrode shell. The diaphragm is a polyethylene diaphragm. The electrolyte uses EC (ethylene carbonate) and EMC (ethyl methyl carbonate) with a mass ratio of 3:7 as solvents, VC (vinyl carbonate) is added as an additive with a mass fraction of 3%, and LiFP is added. 6 As lithium salt, the mass fraction is 12.5%. The amount of electrolyte added is 80 μL.

[0139] After the button cells were assembled, they were packaged using a press and left to rest for 12 hours before being tested for electrochemical properties. The test results are shown in Table 2.

[0140] Table 2

[0141]

[0142] It can be seen from the experimental data in Table 2 that, compared with Comparative Example 1, the delithiation potential of the positive electrode lithium supplement materials of Examples 1 to 4 is reduced, and the degree of delithiation is higher, and the capacity is high. The coating effect of the organic lithium supplement without recrystallization is not as good as that of the organic lithium supplement after recrystallization, and the gram capacity and electrochemical impedance are relatively poor.

[0143] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0144] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a positive electrode lithium supplement material, characterized in that: The following steps are involved: The solution of triblock copolymer F127 is mixed with the solution of phenolic resin prepolymer, and reacted at 60°C to 100°C until the reaction solution becomes turbid to obtain a micellar solution; Take an organic lithium salt lithium supplement material and a surfactant and dissolve them in water, adjust the pH value of the solution to 7-10, add a hydroxylamine hydrochloride solution, mix evenly, perform centrifugal washing, and dry to obtain a pre-treated lithium supplement agent, wherein the organic lithium salt lithium supplement material is selected from Li2C2O4, Li2C3O3, Li2C4O4, Li2C5O5, Li2C6O6, Li2C4O6, [COCON(Li)N(Li)] n and at least one of Li2DHBN; The pretreated lithium supplement agent is mixed with the micelle solution, and subjected to a hydrothermal reaction at 100° C. to 160° C. for 8 h to 36 h to obtain a hydrothermal reaction product; The hydrothermal reaction product is calcined to obtain a positive electrode lithium replenishing material. The calcination temperature is 200°C~600°C, and the time is 3h~6h. The positive electrode lithium replenishing material is a core-shell structure including a core and a shell. The material of the core includes the organic lithium salt lithium replenishing material, and the material of the shell includes ordered mesoporous carbon. After carbon coating, the organic lithium salt lithium replenishing material exists in the form of nanoparticles.

2. The preparation method according to claim 1, characterized in that The solution of the phenolic resin prepolymer is prepared by the following method: Mix phenol and formaldehyde with a phenol-formaldehyde ratio of 1:(1.5~3), adjust the pH value of the solution to 7~10, and react at 60℃~80℃ for 30min~2h.

3. The preparation method according to claim 1, characterized in that: The organic lithium salt lithium supplement material is prepared by the following method: The organic lithium salt, water and ethanol are mixed in a mass ratio of 1: (0-10): (10-20), heated at 60°C-100°C for 6h-48h, filtered and dried to obtain the organic lithium salt lithium supplement material.

4. The preparation method according to any one of claims 1 to 3, characterized in that The particle size of the core is 100nm~20μm.

5. The preparation method according to claim 1, characterized in that: The thickness of the shell layer is 2nm~20nm.

6. The preparation method according to claim 1, characterized in that: The pore size of the shell layer is 2nm~50nm.

7. The preparation method according to claim 1, characterized in that: The specific surface area of ​​the shell is 100m 2 / g~600m 2 / g.

8. A positive electrode lithium supplement material, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 7.

9. A positive electrode slurry, characterized in that: The invention comprises the positive electrode lithium supplement material as claimed in claim 8 and a solvent, wherein the positive electrode lithium supplement material is dispersed in the solvent.

10. A positive electrode sheet, characterized in that: It comprises a positive electrode current collector and a positive electrode material layer arranged on the positive electrode current collector, wherein the positive electrode material layer comprises the positive electrode lithium supplement material as claimed in claim 8.

11. A lithium ion battery, characterized in that: It includes a shell, a positive electrode sheet as described in claim 10, a negative electrode sheet, a diaphragm and an electrolyte, wherein the positive electrode sheet, the negative electrode sheet, the diaphragm and the electrolyte are arranged in the shell, the positive electrode sheet and the negative electrode sheet are arranged opposite to each other, and the diaphragm is located between the positive electrode sheet and the negative electrode sheet.