Fiber-reinforced anti-cracking asphalt concrete and preparation method thereof

The modifier is coupled with sisal fiber to form sepiolite-coated composite fiber, which solves the problem of easy cracking of asphalt concrete, improves the crack resistance and pavement stability, and achieves environmentally friendly and economical pavement improvement effects.

CN118580031BActive Publication Date: 2024-10-22NINGBO DONGXING ASPHALT PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411062088.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-22
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing asphalt concrete is prone to cracking, leading to potential traffic safety hazards. Existing anti-cracking measures are costly or unfriendly to the environment, and the strength of plant fibers is insufficient.

Method used

The modifier is prepared from chemical substances such as diallylamine, silane coupling agent KH560, and mercaptoethanol, and is coupled with sisal fiber through the thioether structure to form a sepiolite-coated reinforced composite fiber, which is combined with alginic acid Sodium compound, used to enhance the crack resistance of asphalt concrete.

Benefits of technology

It effectively improves the crack resistance of asphalt concrete, reduces the occurrence of cracks, maintains the bonding strength of asphalt and aggregates, reduces the erosion of water on pavement voids, and improves pavement stability and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a fiber-reinforced anti-cracking asphalt concrete and a preparation method thereof, and belongs to the technical field of asphalt concrete. The asphalt concrete comprises, by weight, 40-45 parts of road asphalt, 700-800 parts of coarse aggregate, 120-160 parts of fine aggregate, 45-60 parts of mineral powder, 1.3-2.5 parts of reinforced composite fiber and 3-4 parts of asphalt oil; the reinforced composite fiber is based on sisal fiber, and an intermediate is prepared by ring-opening of diallylamine and silane coupling agent KH560, and then a modifier is prepared by addition of mercaptoethanol and double bonds grafted on the intermediate, and the methoxysilane structure in the modifier is hydrolyzed and coupled with the sisal fiber to be loaded on the surface of the sisal fiber, and the sulfide structure and central nitrogen element in the modifier molecule form a chelating effect, and a chelating force is generated with the metal ions in the pores after the sepiolite absorbs water, so that the sepiolite is directional loaded on the surface of the modified fiber for compounding, and a composite fiber of sepiolite coated with sisal is formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of asphalt concrete, and in particular, relates to a fiber-reinforced anti-cracking asphalt concrete and a preparation method thereof. Background Art

[0002] Asphalt concrete is a mixture of artificially selected mineral materials with a certain graded composition, crushed stone or crushed gravel, stone chips or sand, mineral powder, etc. and road asphalt. The road surface paved with it is comfortable to drive on, easy to maintain, and has good road performance. It has gradually become the most widely used road surface in highway construction. However, with the increase in vehicle volume and heavy traffic, the disadvantage of asphalt pavement being easy to crack has become increasingly prominent, and serious road cracks affect traffic safety.

[0003] At present, there are two main solutions to the cracking problem of asphalt concrete. First, use high-performance virgin asphalt or modified asphalt to improve the bonding strength with aggregates and resist the damage of rutting to the road surface. Since asphalt accounts for a high proportion of the pavement, the cost of high-quality virgin asphalt and modified products is generally high, and it is not economical to use them as pavement materials; second, compound a certain amount of fiber in the asphalt concrete, which forms a bridging effect between asphalt and aggregate, increases the bonding strength between asphalt and aggregate to improve crack resistance. Among them, mineral fiber is widely used due to its high strength and large modulus, but the production of mineral fiber consumes a lot of energy. High molecular polymer fiber is simple to form, but it is not environmentally friendly. In comparison, plant fiber is widely available and environmentally friendly, but the strength of plant fiber is not high, and the anti-cracking reinforcement of asphalt concrete is insufficient. Summary of the invention

[0004] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a fiber-reinforced anti-cracking asphalt concrete and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A fiber-reinforced anti-cracking asphalt concrete comprises, by weight, 40-45 parts of road asphalt, 700-800 parts of coarse aggregate, 120-160 parts of fine aggregate, 45-60 parts of mineral powder, 1.3-2.5 parts of reinforced composite fiber and 3-4 parts of asphalt oil.

[0007] Preferably, the coarse aggregate is graded crushed stone of 3-15 mm.

[0008] Preferably, the fine aggregate is manufactured sand with a fineness modulus of 2.5-3.5.

[0009] The reinforced composite fiber is prepared by the following method:

[0010] Step A1: Diallylamine, triethylamine and anhydrous tetrahydrofuran were added and mixed, and dry nitrogen was introduced for protection. The temperature was raised to 55-65°C, and stirred at 120-180 rpm. The silane coupling agent KH560 was slowly added, and the reaction was carried out for 2.5-3.5 hours. After the reaction was completed, low-boiling substances were removed by vacuum rotary evaporation to obtain an intermediate;

[0011] Furthermore, the usage ratio of silane coupling agent KH560, diallylamine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 0.102-0.105 mol: 3-4 mL: 25-30 mL, and the epoxy structure of the silane coupling agent KH560 is ring-opened with diallylamine.

[0012] Step A2: The intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone were mixed and uniformly charged, nitrogen was introduced for protection, the temperature was raised to 40-50°C, stirring was applied at 60-90 rpm, and 150-200 W / m 2 UV irradiation, reaction for 4-5 hours, after the reaction is completed, acetone is removed by rotary evaporation to obtain a modifier;

[0013] Furthermore, the usage ratio of the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone is 0.1 mol: 0.2 mol: 25-30 mg: 45-60 mL, and mercaptoethanol is added to the double bond grafted on the intermediate to introduce a thioether structure into the end of the intermediate molecule.

[0014] Step A3: Add the modifier and ethanol solution and mix them evenly, add formic acid to adjust the pH value to 3-4, heat to 35-45°C for hydrolysis for 1-1.5h, then add sisal fiber and mix for 0.5-0.8h, neutralize with ammonia water, stand for 24h, filter and dry to obtain modified fiber;

[0015] Furthermore, the dosage ratio of sisal fiber, modifier and ethanol solution is 100g:12-16g:200-250mL, the volume fraction of ethanol solution is 40%, and the methoxysilane structure in the modifier is hydrolyzed and coupled with the sisal fiber and loaded onto the surface of the sisal fiber.

[0016] Preferably, the sisal fibers have a length of 20-30 mm.

[0017] Step A4: grind sepiolite powder, sodium alginate and water to make pulp, add modified fiber and mix, let stand for 24 hours, filter and dry to obtain reinforced composite fiber;

[0018] Furthermore, the dosage ratio of the modified fiber, sepiolite powder, sodium alginate and water is 100g:35-45g:2-3g:400-500mL. The sepiolite contains a large number of empty pores. After fully absorbing water, the pores contain a large number of metal ions. The sulfide structure and the central nitrogen element in the modifier molecules loaded on the surface of the modified fiber form a chelating effect, which produces a chelating force with the sepiolite, so that the sepiolite is directionally loaded to the surface of the modified fiber for compounding.

[0019] A method for preparing fiber-reinforced anti-cracking asphalt concrete comprises the following steps:

[0020] Step S1: Mix road asphalt and asphalt oil, heat to 145-155°C, stir and mix to make oil.

[0021] Step S2: Mix the coarse aggregate, fine aggregate, mineral powder and reinforced composite fiber, pre-dry to 160-180° C., add oil and mix to obtain fiber-reinforced anti-cracking asphalt concrete.

[0022] Beneficial effects of the present invention:

[0023] The invention discloses a reinforced composite fiber with a composite structure, which is effectively compounded with asphalt concrete to improve the crack resistance. The reinforced composite fiber uses plant-based sisal fiber as a matrix, has a wide source and is environmentally friendly. An intermediate is prepared by ring-opening diallylamine and silane coupling agent KH560, and then a thioether structure is introduced into the molecular end of the intermediate by addition of mercaptoethanol to the double bond grafted on the intermediate to prepare a modifier. The methoxysilane structure in the modifier is hydrolyzed and coupled with the sisal fiber to be loaded onto the surface of the sisal fiber, and the thioether structure in the modifier molecule forms a chelating effect with the central nitrogen element. Sepiolite contains a large number of empty pores, and the pores contain a large number of metal ions after sufficient water absorption. Driven by the chelating force, the sepiolite is directionally loaded. The sisal fiber provides a fibrous template for the sepiolite. In a dry state, the fibrous sepiolite layer is in a high-strength hard state, which effectively strengthens the asphalt concrete. In a wet state, the sepiolite layer fully absorbs water and expands, generating positive stress in the asphalt concrete to resist the micro-deformation caused by rutting, and reducing the cracking problem caused by excessive deformation of the asphalt concrete due to the decrease in strength in a wet state. At the same time, the sepiolite layer absorbs water and expands to form a water-blocking layer, which fixes the absorbed water, reduces the strong dynamic water pressure generated by the infiltrated water in the asphalt concrete due to rutting, and reduces the erosion of the asphalt concrete voids by water, so that the asphalt and aggregate maintain a stable bonding strength and reduce the generation of cracks. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1, preparation of fiber-reinforced anti-cracking asphalt concrete, the specific implementation process is as follows:

[0026] (1) Preparation of reinforced composite fibers

[0027] Step A1: diallylamine, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is raised to 65°C, stirring is applied at 180rpm, and silane coupling agent KH560 is slowly added for 1 hour. After complete addition, constant temperature stirring is continued for reaction, and the total reaction time of the silane coupling agent KH560 is controlled to be 2.5 hours, wherein the amount ratio of silane coupling agent KH560, diallylamine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 0.105 mol: 3 mL: 30 mL. After the reaction is completed, low-boiling substances including excessive diallylamine and tetrahydrofuran are removed by reduced pressure rotary evaporation to obtain an intermediate;

[0028] Step A2: Take the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone, mix them evenly, introduce nitrogen protection, heat to 50°C, stir at 90 rpm, and apply 200 W / m 2 The mixture was irradiated with ultraviolet light and reacted for 4 hours. After the reaction, acetone was removed by rotary evaporation to obtain a modifier, wherein the dosage ratio of the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone was 0.1 mol: 0.2 mol: 30 mg: 60 mL.

[0029] Step A3: prepare a 40% volume fraction ethanol solution, mix the modifier and the ethanol solution, add formic acid to adjust the pH value to 3, heat to 45°C for hydrolysis for 1 hour, then add sisal fiber and mix for 0.5 hour, neutralize with ammonia water, let stand for 24 hours, filter and dry to obtain modified fiber, wherein the sisal fiber is selected from the short-cut fiber products of Guangdong Guangken Oriental Sisal Co., Ltd., the fiber length is 30 mm, and the amount ratio of sisal fiber, modifier and ethanol solution is 100 g:16 g:250 mL.

[0030] Step A4: add sepiolite powder, sodium alginate and water into a grinder, grind and slurry through a 100-mesh sieve, add modified fiber and mix, let stand for 24 hours, filter and dry to obtain reinforced composite fiber; wherein the amount ratio of modified fiber, sepiolite powder, sodium alginate and water is 100g:35g:2g:400mL.

[0031] (2) Preparation of asphalt concrete

[0032] Step S1: Take 40 parts of 70# road asphalt and 3 parts of asphalt oil by weight, mix the two, heat to 145°C, and stir to mix well to obtain oil;

[0033] Step S2: Take 700 parts of coarse aggregate by weight, selected from graded crushed stone of 3-15 mm; 140 parts of fine aggregate, selected from machine-made sand with a fineness modulus of 2.5-3.5; 50 parts of mineral powder, selected from S95 grade limestone mineral powder; 1.3 parts of reinforced composite fiber, which is homemade in this embodiment; stir and mix all the raw materials, pre-bake to 160°C, and then add oil to mix, so as to obtain fiber-reinforced anti-cracking asphalt concrete.

[0034] Example 2, preparation of fiber-reinforced anti-cracking asphalt concrete, the specific implementation process is as follows:

[0035] (1) Preparation of reinforced composite fibers

[0036] Step A1: diallylamine, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is raised to 55°C, stirring is applied at 120rpm, and silane coupling agent KH560 is slowly added for 1.5 hours. After complete addition, constant temperature stirring is continued for reaction, and the total reaction time of the silane coupling agent KH560 is controlled to be 3.5 hours, wherein the amount ratio of silane coupling agent KH560, diallylamine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 0.102 mol: 4 mL: 25 mL. After the reaction is completed, low-boiling substances including excessive diallylamine and tetrahydrofuran are removed by reduced pressure rotary evaporation to obtain an intermediate;

[0037] Step A2: Take the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone, mix them evenly, pass nitrogen gas for protection, heat to 40°C, stir at 60 rpm, and apply 150 W / m 2 The mixture was irradiated with ultraviolet light and reacted for 5 hours. After the reaction, acetone was removed by rotary evaporation to obtain a modifier, wherein the dosage ratio of the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone was 0.1 mol: 0.2 mol: 25 mg: 45 mL.

[0038] Step A3: prepare a 40% volume fraction ethanol solution, mix the modifier and the ethanol solution, add formic acid to adjust the pH value to 4, heat to 35°C for hydrolysis for 1.5 hours, then add sisal fiber and mix for 0.8 hours, neutralize with ammonia water, let stand for 24 hours, filter and dry to obtain modified fiber, wherein the sisal fiber is selected from the short-cut fiber products of Guangdong Guangken Oriental Sisal Co., Ltd., the fiber length is 20 mm, and the amount ratio of sisal fiber, modifier and ethanol solution is 100 g:12 g:200 mL.

[0039] Step A4: add sepiolite powder, sodium alginate and water into a grinder, grind and slurry through a 100-mesh sieve, add modified fiber and mix, let stand for 24 hours, filter and dry to obtain reinforced composite fiber; wherein the amount ratio of modified fiber, sepiolite powder, sodium alginate and water is 100g:45g:3g:500mL.

[0040] (2) Preparation of asphalt concrete

[0041] Step S1: Take 45 parts of 70# road asphalt and 4 parts of asphalt oil by weight, mix the two, heat to 155°C, and stir to mix well to obtain oil;

[0042] Step S2: Take 800 parts of coarse aggregate by weight, selected from graded crushed stone of 3-15 mm; 160 parts of fine aggregate, selected from machine-made sand with a fineness modulus of 2.5-3.5; 45 parts of mineral powder, selected from S95 grade limestone mineral powder; 2.5 parts of reinforced composite fiber, which is homemade in this embodiment; stir and mix all the raw materials, pre-bake to 180°C, and then add oil and mix to obtain fiber-reinforced anti-cracking asphalt concrete.

[0043] Example 3, preparation of fiber-reinforced anti-cracking asphalt concrete, the specific implementation process is as follows:

[0044] (1) Preparation of reinforced composite fibers

[0045] Step A1: diallylamine, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is raised to 60°C, stirring is applied at 180rpm, and silane coupling agent KH560 is slowly added for 1.2 hours. After complete addition, constant temperature stirring is continued for reaction, and the total reaction time of the silane coupling agent KH560 is controlled to be 3 hours, wherein the amount ratio of silane coupling agent KH560, diallylamine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 0.104 mol: 4 mL: 30 mL. After the reaction is completed, low-boiling substances including excessive diallylamine and tetrahydrofuran are removed by vacuum rotary evaporation to obtain an intermediate;

[0046] Step A2: Take the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone, mix them evenly, introduce nitrogen protection, heat to 45°C, stir at 90 rpm, and heat at 180 W / m 2 The reaction was carried out under ultraviolet irradiation for 4.5 hours. After the reaction was completed, the acetone was removed by rotary evaporation to obtain a modifier, wherein the amount ratio of the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone was 0.1 mol: 0.2 mol: 30 mg: 55 mL.

[0047] Step A3: prepare a 40% volume fraction ethanol solution, mix the modifier and the ethanol solution, add formic acid to adjust the pH value to 3-, heat to 40°C for hydrolysis for 1.2h, then add sisal fiber and mix for 0.8h, neutralize with ammonia water, let stand for 24h, filter and dry to obtain modified fiber, wherein the sisal fiber is selected from the short-cut fiber products of Guangdong Guangken Oriental Sisal Co., Ltd., the fiber length is 20-30mm, and the amount ratio of sisal fiber, modifier and ethanol solution is 100g:14g:220mL.

[0048] Step A4: add sepiolite powder, sodium alginate and water into a grinder, grind and slurry through a 100-mesh sieve, add modified fiber and mix, let stand for 24 hours, filter and dry to obtain reinforced composite fiber; wherein the amount ratio of modified fiber, sepiolite powder, sodium alginate and water is 100g:42g:2g:450mL.

[0049] (2) Preparation of asphalt concrete

[0050] Step S1: Take 42 parts of 70# road asphalt and 4 parts of asphalt oil by weight, mix the two, heat to 150°C, stir and mix well, and obtain oil;

[0051] Step S2: Take 760 parts of coarse aggregate by weight, selected from graded crushed stone of 3-15 mm; 120 parts of fine aggregate, selected from machine-made sand with a fineness modulus of 2.5-3.5; 60 parts of mineral powder, selected from S95 grade limestone mineral powder; 2.2 parts of reinforced composite fiber, which is homemade in this embodiment; stir and mix all the raw materials, pre-bake to 170°C, and then add oil to mix, so as to obtain fiber-reinforced anti-cracking asphalt concrete.

[0052] Example 4, preparation of fiber-reinforced anti-cracking asphalt concrete, the specific implementation process is as follows:

[0053] (1) Preparation of reinforced composite fibers

[0054] Step A1: diallylamine, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is raised to 60°C, stirring is applied at 180rpm, and silane coupling agent KH560 is slowly added for 1.5 hours. After complete addition, constant temperature stirring is continued for reaction, and the total reaction time of the silane coupling agent KH560 is controlled to be 2.8 hours, wherein the amount ratio of silane coupling agent KH560, diallylamine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 0.105 mol: 4 mL: 30 mL. After the reaction is completed, low-boiling substances including excessive diallylamine and tetrahydrofuran are removed by vacuum rotary evaporation to obtain an intermediate;

[0055] Step A2: Take the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone, mix them evenly, introduce nitrogen protection, heat to 50°C, stir at 90 rpm, and apply 150 W / m 2 The reaction was carried out under ultraviolet irradiation for 4 hours. After the reaction was completed, the acetone was removed by rotary evaporation to obtain a modifier, wherein the amount ratio of the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone was 0.1 mol: 0.2 mol: 25 mg: 55 mL.

[0056] Step A3: prepare a 40% volume fraction ethanol solution, mix the modifier and the ethanol solution, add formic acid to adjust the pH value to 4, heat to 45°C for hydrolysis for 1.2 hours, then add sisal fiber and mix for 0.8 hours, neutralize with ammonia water, let stand for 24 hours, filter and dry to obtain modified fiber, wherein the sisal fiber is selected from the short-cut fiber products of Guangdong Guangken Oriental Sisal Co., Ltd., the fiber length is 30 mm, and the amount ratio of sisal fiber, modifier and ethanol solution is 100 g:15 g:200 mL.

[0057] Step A4: add sepiolite powder, sodium alginate and water into a grinder, grind and slurry through a 100-mesh sieve, add modified fiber and mix, let stand for 24 hours, filter and dry to obtain reinforced composite fiber; wherein the amount ratio of modified fiber, sepiolite powder, sodium alginate and water is 100g:40g:3g:420mL.

[0058] (2) Preparation of asphalt concrete

[0059] Step S1: Take 45 parts of 70# road asphalt and 4 parts of asphalt oil by weight, mix the two, heat to 150°C, stir and mix, and obtain oil;

[0060] Step S2: Take 720 parts of coarse aggregate by weight, selected from graded crushed stone of 3-15 mm; 150 parts of fine aggregate, selected from machine-made sand with a fineness modulus of 2.5-3.5; 50 parts of mineral powder, selected from S95 grade limestone mineral powder; 2 parts of reinforced composite fiber, which is homemade in this embodiment; stir and mix all the raw materials, pre-bake to 180°C, and then add oil to mix, so as to obtain fiber-reinforced anti-cracking asphalt concrete.

[0061] Comparative Example

[0062] In this comparative example, the reinforced composite fiber in Example 4 is replaced by 1.2 parts of sisal fiber and 0.6 parts of sepiolite powder, and the rest of the implementation process is exactly the same as that in Example 4.

[0063] The asphalt concrete obtained as above was poured into a mold, compacted at 2.0 MPa, and naturally cured for 7 days. Samples were taken according to the JTGE20-2011 standard and Marshall stability test, rutting test and splitting strength test were performed. The specific test results are shown in Table 1:

[0064] Table 1

[0065]

[0066] It can be seen from the data in Table 1 that the Marshall stability, dynamic stability and splitting strength of the asphalt concrete of the embodiment are higher than those of the comparative example, indicating that the reinforcing composite fiber has a better reinforcing effect on the asphalt concrete.

[0067] In order to verify the road crack resistance of the above asphalt concrete, the rutting test was referred to and the tests were carried out in dry and wet states respectively. The test temperature was 23±2℃, the wheel pressure was 1.2MPa, the wheel stroke was 200mm, the wheel speed was 40 times / min, and the test cycle was 100000 times. In the dry state, the air humidity was 65±5%, and the wet state was 1L of water sprayed every 30min of the test. After that, the splitting strength of the sample was tested and compared with the splitting strength in Table 1 and the strength retention rate was calculated. The specific test results are shown in Table 2:

[0068] Table 2

[0069]

[0070] It can be seen from the data in Table 2 that the strength retention rates of the embodiment and the comparative example after simulated rutting in the dry state are similar, while in the wet state, the strength retention rate of the embodiment is above 80%, while that of the comparative example is only 65.58%. Under wet rutting, the crack resistance of the comparative example deteriorates seriously.

[0071] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0072] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A fiber-reinforced anti-cracking asphalt concrete, characterized in that: The composition includes, by weight: 40-45 parts of road asphalt, 700-800 parts of coarse aggregate, 120-160 parts of fine aggregate, 45-60 parts of mineral powder, 1.3-2.5 parts of reinforced composite fiber and 3-4 parts of asphalt oil; The reinforced composite fiber is prepared by the following method: Step A1: Diallylamine, triethylamine and anhydrous tetrahydrofuran were added and mixed, and dry nitrogen was introduced for protection. The temperature was raised to 55-65°C, and the silane coupling agent KH560 was slowly added while stirring. The reaction was continued for 2.5-3.5 hours. After the reaction was completed, low-boiling substances were removed by vacuum rotary evaporation to obtain an intermediate; Step A2: Mix the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone, introduce nitrogen protection, heat to 40-50°C, stir and add 150-200W / m 2 UV irradiation, reaction for 4-5 hours, after the reaction is completed, acetone is removed by rotary evaporation to obtain a modifier; Step A3: Add the modifier and ethanol solution and mix them evenly, add formic acid to adjust the pH value to 3-4, heat to 35-45°C for hydrolysis for 1-1.5h, then add sisal fiber and mix for 0.5-0.8h, neutralize with ammonia water, stand for 24h, filter and dry to obtain modified fiber; Step A4: grind sepiolite powder, sodium alginate and water to make pulp, add modified fiber and mix, let stand for 24 hours, filter and dry to obtain reinforced composite fiber.

2. A fiber-reinforced anti-cracking asphalt concrete according to claim 1, characterized in that: The dosage ratio of silane coupling agent KH560, diallylamine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 0.102-0.105 mol: 3-4 mL: 25-30 mL.

3. The fiber-reinforced anti-cracking asphalt concrete according to claim 2, characterized in that: The usage ratio of the intermediate, mercaptoethanol, dimethylphenylphosphine and anhydrous acetone is 0.1 mol: 0.2 mol: 25-30 mg: 45-60 mL.

4. The fiber-reinforced anti-cracking asphalt concrete according to claim 3, characterized in that: The dosage ratio of sisal fiber, modifier and ethanol solution is 100g:12-16g:200-250mL, and the volume fraction of ethanol solution is 40%.

5. The fiber-reinforced anti-cracking asphalt concrete according to claim 4, characterized in that: The length of sisal fibers is 20-30 mm.

6. The fiber-reinforced anti-cracking asphalt concrete according to claim 5, characterized in that: The dosage ratio of the modified fiber, sepiolite powder, sodium alginate and water is 100g:35-45g:2-3g:400-500mL.

7. The fiber-reinforced anti-cracking asphalt concrete according to claim 1, characterized in that: The coarse aggregate is graded crushed stone of 3-15mm, and the fine aggregate is machine-made sand with a fineness modulus of 2.5-3.

5.

8. A method for preparing a fiber-reinforced anti-cracking asphalt concrete according to any one of claims 1 to 7, characterized in that: The steps include: Step S1: Mix road asphalt and asphalt oil, heat to 145-155°C, stir and mix to make oil. Step S2: coarse aggregate, fine aggregate, mineral powder and reinforced composite fiber are stirred and mixed, pre-dried to 160-180° C., and oil is added and mixed to obtain fiber-reinforced anti-cracking asphalt concrete.