A modified high-silicon tailings powder and its application in plastics
By mixing high-silicon tailings fine powder with dilute sulfuric acid and modified lignin copolymers, the modified high-silicon tailings fine powder is solved, and the problem of poor mechanical properties and anti-ultraviolet aging performance in PVC and PP is achieved. Improved compatibility and biodegradability.
Patent Information
- Application Number
- CN202411062149.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-05
AI Technical Summary
In the prior art, there are few researches on the modification of high-silicon tailings micro powder, which leads to poor mechanical properties and anti-ultraviolet aging performance in PVC and PP plastics.
Modified high-silicon tailings powder is prepared by mixing the fine powder of high-silicon tailings with dilute sulfuric acid, adding surfactant and modified lignin copolymer, and grinding and vacuum drying to improve its compatibility with PVC and PP and anti-UV aging properties.
The mechanical properties and UV aging resistance of modified high-silicon tailings micro powder in PVC and PP are significantly improved, and the biodegradation ability of plastics is enhanced and white pollution is reduced.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-silicon tailings micropowder, and in particular to modified high-silicon tailings micropowder and application thereof in plastics. Background Art
[0002] High-silicon tailings powder refers to the powder obtained from the cyanide removal of gold concentrate tailings and the enrichment of ferrosulfur and harmlessness after drying. It is the main solid waste discharged after tailings reduction and resource utilization. High-silicon tailings powder contains a large amount of relatively stable components such as silicon dioxide and aluminum oxide. Because its fineness can reach more than 400 mesh, its application scope and application effect in the field of building materials are limited. In practice, high-silicon tailings powder can be used as a filler for plastics such as PVC and PP. However, there are relatively few studies on the modification of high-silicon tailings powder, and there are few reports on the use of high-silicon tailings powder as a filler for PVC and PP plastics.
[0003] A Chinese invention patent with publication number CN106867028A discloses modified stone coal vanadium tailings powder used as plastic filler and its preparation method. The high silicon tailings powder is modified by the method in the patent and then added to PVC and PP plastics, but the mechanical performance parameters are poor. Summary of the invention
[0004] In view of the shortcomings of the prior art, the object of the present invention is to provide a modified high-silicon tailings powder and its application in plastics.
[0005] To achieve the above object, the present invention is implemented through the following technical solutions:
[0006] A modified high-silicon tailings powder is prepared by the following method:
[0007] (1) Add high-silicon tailings powder into dilute sulfuric acid and stir to prepare a suspension with a concentration of 30-50wt%;
[0008] (2) Adding a surfactant to the suspension, heating to 60-70°C, stirring for 0.5-2h, and obtaining a high-silicon tailings micropowder slurry;
[0009] (3) mixing the high-silicon tailings micropowder slurry and the modified lignin copolymer, and then grinding them with a colloid mill to obtain a modified high-silicon tailings micropowder slurry, filtering, and vacuum drying at 70-85° C. to obtain a modified high-silicon tailings micropowder;
[0010] The modified lignin copolymer is prepared by grafting glycidyl methacrylate and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol on lignin.
[0011] The modified lignin copolymer is prepared by the following method:
[0012] (1) Under nitrogen protection, add acetone and lignin into the reaction bottle, stir, and heat to 35-50°C;
[0013] (2) Add 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol to the reaction bottle, stir and mix, then slowly add glycidyl methacrylate and ammonium persulfate solution, add for 0.5-1h, and graft copolymerize for 1-2h to obtain a modified lignin copolymer. The copolymerization route is shown as follows:
[0014]
[0015] Among them, Lignin stands for lignin.
[0016] The mass ratio of the lignin, glycidyl methacrylate, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol and ammonium persulfate solution is 10:(2-3):(3-4):(0.5-0.8).
[0017] The concentration of the ammonium persulfate solution is 0.5-2 mol / L.
[0018] After the surfactant is added in step (2), the concentration of the surfactant in the system is 2-3 wt %.
[0019] The surfactant is composed of the following raw materials in parts by weight: 40 parts of hexadecyltrimethylammonium bromide and 15-20 parts of sodium petroleum sulfonate.
[0020] In the step (3), the feed mass ratio of the modified lignin to the modified high-silicon tailings micropowder slurry is (1-2):20.
[0021] The present invention also provides: application of modified high-silicon tailings powder in plastics.
[0022] Due to the adoption of the above technical solution, the beneficial effects of the present invention include:
[0023] 1. The present invention obtains a modified lignin by grafting copolymerization of methyl glycidyl methacrylate and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol on lignin, and obtains a new type of modified high-silicon tailings powder by grinding the modified lignin and activated modified high-silicon tailings powder slurry with a colloid mill. 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol contains benzotriazole groups and can be used as ultraviolet absorbers, but due to its small molecular weight, it is not resistant to migration and has poor anti-ultraviolet aging effect. In the present application, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol is grafted onto lignin to increase the molecular weight and improve the ability to resist migration and extraction. At the same time, the modified lignin contains epoxy groups provided by glycidyl methacrylate, which has good biocompatibility and can improve the compatibility of the modified high-silicon tailings powder with PP and PVC. In addition, the present application uses lignin, which can be naturally biodegraded. After the modified high-silicon tailings powder is applied to the plastic field, it can improve the biodegradability of plastics and reduce white pollution to a certain extent.
[0024] 2. The modified high-silicon tailings powder prepared by the method of the present invention is added to PVC / PP to significantly improve the mechanical properties and anti-ultraviolet aging properties of the plastic. DETAILED DESCRIPTION
[0025] The invention will be further described below in conjunction with the embodiments, but the invention is not limited to these embodiments.
[0026] Example 1 Preparation of modified lignin copolymer:
[0027] (1) Under nitrogen protection, add 400 g acetone and 100 g lignin into the reaction bottle, stir, and heat to 35 °C;
[0028] (2) Add 30 g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol to the reaction bottle and stir. Then slowly add 20 g of glycidyl methacrylate and 5 g of ammonium persulfate solution (2 mol / L) dropwise for 0.5 h. Perform the graft copolymerization reaction for 2 h and evaporate at 45 °C to obtain the modified lignin copolymer.
[0029] Example 2 Preparation of modified lignin copolymer:
[0030] (1) Under nitrogen protection, add 400 g acetone and 100 g lignin into the reaction bottle, stir, and heat to 40 °C;
[0031] (2) Add 35 g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol to the reaction bottle and stir. Then slowly add 25 g of glycidyl methacrylate and 6 g of ammonium persulfate solution (1.2 mol / L) dropwise for 0.5 h. Perform the graft copolymerization reaction for 1.5 h and evaporate at 40 °C to obtain the modified lignin copolymer.
[0032] Example 3 Preparation of modified lignin copolymer:
[0033] (1) Under nitrogen protection, add 400 g acetone and 100 g lignin into the reaction bottle, stir, and heat to 50 °C;
[0034] (2) Add 40 g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol to the reaction bottle and stir. Then slowly add 30 g of glycidyl methacrylate and 8 g of ammonium persulfate solution (0.5 mol / L) dropwise for 1 hour. The graft copolymerization reaction was carried out for 1 hour. The modified lignin copolymer was obtained by distillation at 50°C.
[0035] Example 4 Preparation of modified high silicon tailings powder:
[0036] (1) Add high-silicon tailings powder into 10wt% dilute sulfuric acid and stir to prepare a suspension with a concentration of 30wt%;
[0037] (2) adding a surfactant to the suspension (after adding the surfactant, the concentration of the surfactant in the system is 2 wt%), heating to 60° C., stirring for 2 h, and obtaining a high-silicon tailings micropowder slurry;
[0038] In this step, the surfactant is a mixture of hexadecyltrimethylammonium bromide and sodium petroleum sulfonate, and the mass ratio of hexadecyltrimethylammonium bromide to sodium petroleum sulfonate is 8:3;
[0039] (3) 2000 g of high-silicon tailings powder slurry and 100 g of modified lignin copolymer (prepared in Example 1) were mixed, and then ground by a colloid mill to obtain modified high-silicon tailings powder slurry. The slurry was filtered and vacuum dried at 70° C. for 8 h to obtain modified high-silicon tailings powder.
[0040] Example 5 Preparation of modified high silicon tailings powder:
[0041] (1) Add high-silicon tailings powder into 12wt% dilute sulfuric acid and stir to prepare a suspension with a concentration of 40wt%;
[0042] (2) adding a surfactant to the suspension (after adding the surfactant, the concentration of the surfactant in the system is 2.5 wt%), heating to 65° C., stirring for 1 h, and obtaining a high-silicon tailings micropowder slurry;
[0043] In this step, the surfactant is a mixture of hexadecyltrimethylammonium bromide and sodium petroleum sulfonate, and the mass ratio of hexadecyltrimethylammonium bromide to sodium petroleum sulfonate is 8:3.5;
[0044] (3) 2000 g of high-silicon tailings powder slurry and 150 g of modified lignin copolymer (prepared in Example 2) were mixed, and then ground by a colloid mill to obtain modified high-silicon tailings powder slurry. The slurry was filtered and vacuum dried at 80° C. for 8 h to obtain modified high-silicon tailings powder.
[0045] Example 6 Preparation of modified high silicon tailings powder:
[0046] (1) Add high-silicon tailings powder into 10wt% dilute sulfuric acid and stir to prepare a suspension with a concentration of 50wt%;
[0047] (2) adding a surfactant to the suspension (after adding the surfactant, the concentration of the surfactant in the system is 3 wt%), heating to 70° C., stirring for 0.5 h, and obtaining a high-silicon tailings micropowder slurry;
[0048] In this step, the surfactant is a mixture of hexadecyltrimethylammonium bromide and sodium petroleum sulfonate, and the mass ratio of hexadecyltrimethylammonium bromide to sodium petroleum sulfonate is 8:4;
[0049] (3) 2000 g of high-silicon tailings powder slurry and 200 g of modified lignin copolymer (prepared in Example 3) were mixed, and then ground by a colloid mill to obtain modified high-silicon tailings powder slurry. The slurry was filtered and vacuum dried at 85° C. for 7 h to obtain modified high-silicon tailings powder.
[0050] Application Example 1
[0051] 150 g of modified high-silicon tailings powder (prepared in Example 4), 100 g of PVC, 15 g of zinc stearate, and 20 g of dioctyl phthalate were mixed evenly, put into an open mill, and mixed at 190° C. for 15 min. After mixing evenly, vulcanized on a flat vulcanizer to obtain a PVC material.
[0052] Application Example 2
[0053] 150 g of modified high-silicon tailings powder (prepared in Example 5), 100 g of PVC, 15 g of zinc stearate, and 20 g of dioctyl phthalate were mixed evenly, put into an open mill, and mixed at 190° C. for 15 min. After mixing evenly, vulcanized on a flat vulcanizer to obtain a PVC material.
[0054] Application Example 3
[0055] 200 g of modified high-silicon tailings powder (prepared in Example 6), 100 g of PP, 15 g of zinc stearate, and 20 g of dioctyl phthalate were mixed evenly, put into an open mill, and mixed at 190° C. for 15 min. After mixing evenly, vulcanized on a flat vulcanizer to obtain a PP material.
[0056] Comparative application example 1
[0057] 150g of modified high-silicon tailings powder, 100g of PVC, 15g of zinc stearate and 20g of dioctyl phthalate were mixed evenly, put into an open mill, mixed at 190°C for 15min, and after mixing evenly, vulcanized on a flat vulcanizer to obtain a PVC material.
[0058] In this comparative application example, the modified high-silicon tailings powder is prepared by the following method:
[0059] (1) Slurry preparation: Add high-silicon tailings powder into 12wt% dilute sulfuric acid and stir to prepare a 40wt% suspension;
[0060] (2) Surface activation: add a surfactant to the suspension to make the concentration of the surfactant in the system 2.5wt%, heat to 65°C, stir for 1h, then add sodium hexametaphosphate to make the concentration of sodium hexametaphosphate in the system 0.5wt%, stir for 1h to obtain a modified high-silicon tailings micropowder slurry, filter, and vacuum dry at 80°C for 10h to obtain an activated high-silicon tailings micropowder dry powder; in this step, the surfactant is composed of the following raw materials in parts by weight: 40 parts of hexadecyltrimethylammonium bromide and 15 parts of sodium petroleum sulfonate;
[0061] (3) Surface coating: 10 g of the modified lignin copolymer (prepared in Example 2) and 2500 g of high-silicon tailings powder were added to a powder surface coating machine for high-speed mixing and coating. The temperature was controlled at 115°C during coating. After coating, the mixture was cooled and crushed to obtain modified high-silicon tailings powder.
[0062] Comparative Application Example 2
[0063] 150g of modified high-silicon tailings powder, 100g of PVC, 15g of zinc stearate and 20g of dioctyl phthalate were mixed evenly, put into an open mill, mixed at 190°C for 15min, and after mixing evenly, vulcanized on a flat vulcanizer to obtain a PVC material.
[0064] In this comparative application example, the modified high-silicon tailings powder is prepared by the following method:
[0065] (1) Slurry preparation: Add high-silicon tailings powder into 12wt% dilute sulfuric acid and stir to prepare a 40wt% suspension;
[0066] (2) Surface activation: add a surfactant to the suspension to make the concentration of the surfactant in the system 2.5wt%, heat to 65°C, stir for 1h, then add sodium hexametaphosphate to make the concentration of sodium hexametaphosphate in the system 0.5wt%, stir for 1h to obtain a modified high-silicon tailings micropowder slurry, filter, and vacuum dry at 80°C for 10h to obtain an activated high-silicon tailings micropowder dry powder; in this step, the surfactant is composed of the following raw materials in parts by weight: 40 parts of hexadecyltrimethylammonium bromide and 15 parts of sodium petroleum sulfonate;
[0067] (3) Surface coating: 150 g of the modified lignin copolymer (prepared in Example 2) and 2000 g of high-silicon tailings powder were added to a powder surface coating machine for high-speed mixing and coating. The temperature was controlled at 115°C during coating. After coating, the mixture was cooled and crushed to obtain modified high-silicon tailings powder.
[0068] Comparative Application Example 3
[0069] 150g of modified high-silicon tailings powder, 100g of PVC, 15g of zinc stearate and 20g of dioctyl phthalate were mixed evenly, put into an open mill, mixed at 190°C for 15min, and after mixing evenly, vulcanized on a flat vulcanizer to obtain a PVC material.
[0070] The preparation method of the modified high-silicon tailings powder in this comparative application example is basically the same as that in Example 5, except that 150 g of the modified lignin copolymer in step (3) is replaced by 94 g of lignin, 24 g of glycidyl methacrylate, and 33 g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol.
[0071] Comparative Application Example 4
[0072] 150g of modified high-silicon tailings powder, 100g of PVC, 15g of zinc stearate and 20g of dioctyl phthalate were mixed evenly, put into an open mill, mixed at 190°C for 15min, and after mixing evenly, vulcanized on a flat vulcanizer to obtain a PVC material.
[0073] The preparation method of the modified high-silicon tailings powder in this comparative application example adopts the method of Example 1 of the Chinese invention patent publication number CN106867028A, and only needs to replace the stone coal vanadium tailings with high-silicon tailings powder.
[0074] Comparative Application Example 5
[0075] 150g of modified high-silicon tailings powder, 100g of PVC, 15g of zinc stearate and 20g of dioctyl phthalate were mixed evenly, put into an open mill, mixed at 190°C for 15min, and after mixing evenly, vulcanized on a flat vulcanizer to obtain a PVC material.
[0076] The preparation method of the modified high-silicon tailings powder in this comparative application example is basically the same as that in Example 5, except that the modified lignin used is different. The modified lignin in this comparative application example is prepared by the following method: under nitrogen protection, 400g of acetone and 100g of lignin are added to the reaction bottle, stirred, and heated to 40°C; 35g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol is added to the reaction bottle, and then 6g of ammonium persulfate solution (1.2mol / L) is slowly added dropwise for 0.5h, the graft copolymerization reaction is carried out for 1.5h, and the modified lignin copolymer is obtained by distillation at 40°C.
[0077] In the embodiments, comparative examples and comparative application examples of the present application, the shear temperature during colloid mill grinding is 190°C, the shear rate is 7000r / min, and the shear time is 30min; the main components of the high-silicon tailings powder used are silicon dioxide (70.05wt%), aluminum oxide (20.93wt%), calcium oxide (1.87wt%), and iron oxide (3.84 wt%); the PP used is polypropylene T36F; the PVC used is S-700 from Qilu Petrochemical, and the lignin used is guaiac-syringyl lignin produced by Henan Qiangxing Chemical Co., Ltd.
[0078] The materials prepared in the application examples and comparative application examples were subjected to UV aging tests, and the test method was carried out in accordance with the method of GB / T16422.3-2014 "Plastic Laboratory Light Source Exposure Test Method".
[0079] The materials prepared in the application examples of this application and the comparative application examples as well as the materials after UV aging were tested for impact strength (GB / T 1043.2-2018) and tensile strength (GB / T1040.2-2022). The test results are shown in Table 1.
[0080] Table 1
[0081]
[0082] It can be seen from Application Examples 1-3 in Table 1 that the composite materials obtained by compounding the modified high-silicon tailings powder prepared by the present invention with PVC and PP have excellent mechanical properties and anti-ultraviolet aging properties.
[0083] Comparative Application Examples 1 and 2 are application examples of modified high-silicon tailings powder prepared by different surface activation methods and applied to PVC. It can be seen from Table 1 that the impact strength after aging is less than 80KJ / m 2 , the tensile strength is less than 40MPa.
[0084] The difference between the modified high silicon tailings powder used in comparative application example 3 and example 5 is that when preparing the modified high silicon tailings powder, the modified lignin copolymer is replaced with lignin, glycidyl methacrylate, and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol. It can be seen from the data in Table 1 that the impact strength before aging is 96KJ / m 2 , the tensile strength is 45MPa, and the impact strength after aging is 67KJ / m 2 , the tensile strength is 31MPa. The reason for its poor mechanical properties before aging may be the mixing uniformity of the two ungrafted compounds and lignin in the preparation of modified high-silicon tailings powder; the reason for the large loss of mechanical properties after aging may be that the molecular weight of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol is small, easy to migrate and extract to the plastic surface, resulting in poor anti-ultraviolet aging ability.
[0085] Comparative Application Example 4 is a comparative application example of the modified high silicon tailings powder prepared by the method of Example 1 of the Chinese invention patent with publication number CN106867028A and applied to PVC. It can be seen from Table 1 that its impact strength after aging is 56KJ / m 2 , the tensile strength is 29MPa.
[0086] Comparative Application Example 5 is a comparative application example using modified lignin without glycidyl methacrylate grafting. It can be seen from Table 1 that although the mechanical property loss after the UV aging test is small, its mechanical property is lower than that of Application Example 2.
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. However, any equivalent changes, modifications and evolutions made by ordinary technicians in the field without departing from the scope of the technical solution of the present invention by using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. A modified high silicon tailings powder, characterized in that: Prepared by the following method: (1) Add high-silicon tailings powder into dilute sulfuric acid and stir to prepare a suspension with a concentration of 30-50wt%; (2) Adding a surfactant to the suspension, heating to 60-70°C, stirring for 0.5-2h, and obtaining a high-silicon tailings micropowder slurry; (3) mixing the high-silicon tailings micropowder slurry and the modified lignin copolymer, and then grinding them with a colloid mill to obtain a modified high-silicon tailings micropowder slurry, filtering, and vacuum drying at 70-85° C. to obtain a modified high-silicon tailings micropowder; The modified lignin copolymer is prepared by grafting glycidyl methacrylate and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol on lignin; The surfactant is composed of the following raw materials in parts by weight: 40 parts of hexadecyltrimethylammonium bromide and 15-20 parts of sodium petroleum sulfonate.
2. The modified high silicon tailings powder according to claim 1, characterized in that: The modified lignin copolymer is prepared by the following method: (1) Under nitrogen protection, add acetone and lignin into the reaction bottle, stir, and heat to 35-50°C; (2) Add 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol to the reaction bottle, stir, and then slowly add glycidyl methacrylate and ammonium persulfate solution dropwise for 0.5-1h. The graft copolymerization reaction is carried out for 1-2h to obtain a modified lignin copolymer.
3. The modified high silicon tailings powder according to claim 2, characterized in that: The mass ratio of the lignin, glycidyl methacrylate, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol and ammonium persulfate solution is 10:(2-3):(3-4):(0.5-0.8).
4. The modified high-silicon tailings powder according to claim 2, characterized in that: The concentration of the ammonium persulfate solution is 0.5-2 mol / L.
5. The modified high silicon tailings powder according to claim 1, characterized in that: After the surfactant is added in step (2), the concentration of the surfactant in the system is 2-3 wt %.
6. The modified high silicon tailings powder according to claim 1, characterized in that: In the step (3), the feed mass ratio of the modified lignin to the modified high-silicon tailings micropowder slurry is (1-2):
20.