Medium manganese hot-formed steel and its preparation method and application

By adjusting process parameters and optimizing raw material components, a medium-manganese-based thermoformed steel was prepared to form a composite structure, which solved the problem of low elongation of the thermoformed steel, achieved high yield and high plasticity, and was suitable for automotive parts. manufacturing.

CN118581391BActive Publication Date: 2024-11-01GUANGDONG INST OF NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411066982.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-01
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing thermoformed steel has low elongation during collision, which can easily lead to fracture, making it difficult to meet the high plasticity requirements of the automotive industry, and the quenching-distribution process is complex and operation is difficult.

Method used

By adjusting the process parameters and optimizing the raw material components, a medium-manganese hot-formed steel is prepared to form a complex phase structure of residual austenite and laminated martensite. Multiple hot rolling, cold rolling, heating and quenching treatment methods are used to prepare Get thermoformed steel with high yield and high plasticity.

Benefits of technology

Without changing the existing thermoformed steel production line, a medium-manganese-based thermoformed steel with excellent resistance to deformation was prepared, which is suitable for the manufacture of automotive parts, such as A-pillar, B-pillar, roof beam and bumper, improving the Material strength and toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118581391B_ABST
    Figure CN118581391B_ABST
Patent Text Reader

Abstract

The invention discloses a medium manganese hot-forming steel and a preparation method and application thereof, and relates to the technical field of metal materials. The medium manganese hot-forming steel comprises the following components: C 0.20%-0.40%, Mn 5.0%-11.0%, Cr 0.90%-2.00%, Al 0.10%-0.30%, microalloying elements 0.05%-0.15%, Si 1.0%-2.0%, and the rest are Fe and inevitable impurities; the microalloying elements are selected from any one of Nb elements and Ti elements. The complex phase structure of residual austenite and lath martensite is obtained by adjusting the process parameters and optimizing the raw material components; the prepared hot-forming steel is a medium manganese hot-forming steel with high yield and high plasticity, and has excellent resistance to deformation. The preparation method is applicable to all existing hot-forming steel production lines and can be widely promoted and applied in industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal materials, and in particular to a medium manganese hot-formed steel and a preparation method and application thereof. Background Art

[0002] With the increasing demand for lightweight and collision safety of automobiles, the automotive industry is constantly developing new materials and manufacturing processes. Hot stamping is an emerging technology that integrates stamping and synchronous quenching. It can effectively solve the problems of easy cracking, severe springback and poor dimensional accuracy of high-strength complex parts during the stamping process. Therefore, it has been widely used, mainly for the manufacture of key parts such as A-pillars, B-pillars, roof beams, anti-collision beams and bumpers.

[0003] At present, the hot stamping steel with the largest consumption and the widest application in the world is 1500 MPa grade 22MnB5. However, because its elongation is generally less than 8%, it is easy to break under small deformation during a collision and lose its protective performance. Therefore, the automotive industry has gradually put forward higher requirements for the plasticity of hot-formed steel. At present, the introduction of residual austenite is one of the feasible ways to improve the plasticity of hot-formed steel, and the quenching-partitioning process is a common method for introducing residual austenite. This process requires quenching the steel to a certain temperature and keeping it warm, so that the carbon element in the martensite diffuses to the critical residual austenite, so that it can be retained at room temperature. However, the process complexity of this process is relatively high and the operation is difficult.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a medium manganese hot-formed steel and a preparation method and application thereof, so as to solve the above-mentioned technical problems.

[0006] The present invention is achieved in that:

[0007] In a first aspect, an embodiment of the present invention provides a medium manganese hot-formed steel, wherein the hot-formed steel comprises the following components by mass fraction:

[0008] C 0.20%-0.40%, Mn 5.0%-11.0%, Cr 0.90%-2.00%, Al 0.10%-0.30%, micro-alloying elements 0.05%-0.15%, Si 1.0%-2.0%, and the rest are Fe and unavoidable impurities; the micro-alloying element is selected from any one of Nb element and Ti element.

[0009] In a second aspect, an embodiment of the present invention provides a method for preparing the aforementioned hot-formed steel, comprising the following steps:

[0010] preparing raw materials according to the composition ratio of hot-formed steel, and forming the raw materials into slabs;

[0011] The slab is subjected to multiple hot rolling treatments, multiple cold rolling treatments, heating treatments and quenching treatments to obtain hot-formed steel.

[0012] In a third aspect, an embodiment of the present invention provides a use of the aforementioned hot-formed steel or the hot-formed steel obtained by the aforementioned preparation method in manufacturing automobile parts;

[0013] The components include at least one of an A-pillar, a B-pillar, a roof beam, an anti-collision beam and a bumper.

[0014] The present invention has the following beneficial effects:

[0015] The medium manganese hot-forming steel and its preparation method and application provided by the present invention, on the basis of not changing the existing hot-forming steel production line, adjusts the process parameters and optimizes the raw material components to obtain a complex phase structure of residual austenite and lath martensite; the prepared hot-forming steel is a medium manganese hot-forming steel with high yield and high plasticity, and has excellent deformation resistance. The preparation method is applicable to all existing hot-forming steel production lines and can be widely promoted and applied in industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0017] Figure 1 Phase distribution diagram of hot-formed steel prepared in Examples 1-3 and Comparative Example 1;

[0018] Figure 2 Engineering strain-engineering stress curves of the hot-formed steels prepared in Examples 1-3 and Comparative Example 1. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0020] In a first aspect, an embodiment of the present invention provides a medium manganese hot-formed steel, wherein the hot-formed steel comprises the following components by mass fraction:

[0021] C 0.20%-0.40%, Mn 5.0%-11.0%, Cr 0.90%-2.00%, Al 0.10%-0.30%, micro-alloying elements 0.05%-0.15%, Si 1.0%-2.0%, and the rest are Fe and unavoidable impurities; the micro-alloying element is selected from any one of Nb element and Ti element.

[0022] Manganese is one of the alloying elements in steel, forming a hard compound with iron, which can not only improve the hardness of steel, but also improve the toughness, wear resistance and other properties of steel. The effects of manganese on steel are mainly as follows:

[0023] Improve hardness: The hard compounds formed by manganese in steel can increase the hardness of steel, making it suitable for manufacturing high-strength, high-hardness parts and tools.

[0024] Improve toughness: Manganese can be evenly distributed in the steel, improving the size and structure of the crystals in the steel, thereby improving the toughness of the steel.

[0025] Improve wear resistance: Under certain working conditions, steel parts need to have higher wear resistance. At this time, the wear resistance of steel can be improved by increasing the manganese content.

[0026] Impact resistance: Some mechanical parts or tools need to have certain impact resistance. Manganese can increase the carbon content in steel and improve the impact resistance of steel to a certain extent.

[0027] Among them, steel with a Mn content of 1.0%-11.0% belongs to the medium manganese steel series, and the Mn content in the present invention is 5.0%-11.0%, which belongs to the medium manganese steel series; medium manganese steel has good strength, toughness and wear resistance, and can be widely used in the manufacture of mechanical parts and tools for railways, automobiles, ships, etc.

[0028] Microalloying elements are a class of alloying elements that can effectively stabilize austenite. In steel materials, adding these elements can improve the stability of austenite, thereby improving the mechanical properties of the material. The microalloying element in the present invention is selected from any one of Nb and Ti.

[0029] The introduction of Nb element in hot-formed steel can combine with carbon in the steel to form carbides. These compounds dissolve at high temperatures and precipitate at low temperatures, thereby inhibiting grain growth and playing a precipitation strengthening role. This mechanism of action helps to reduce the carbon equivalent of steel, while significantly improving the strength and toughness of steel, and has cost advantages. In addition, the addition of Nb element can further refine the ferrite grains after rolling by preventing the growth of residual austenite grains during heating and inhibiting the deformation and recrystallization of residual austenite, so that the steel has a better strength and toughness combination.

[0030] The introduction of Ti element into hot-formed steel can refine the grains and enhance the strength of the material by forming compounds such as TiC. In addition, the presence of titanium helps stabilize austenite. The role of titanium in hot-formed steel also includes refining grains, preventing intergranular corrosion, improving welding performance, and forming precipitation hardening. Titanium can prevent the precipitation of chromium carbide along the austenite grain boundaries, thereby avoiding the formation of chromium-poor areas of grain boundary solid solution and reducing the possibility of intergranular corrosion.

[0031] In an optional embodiment of the present invention, the hot-formed steel comprises the following components by mass fraction:

[0032] C 0.20%-0.30%, Mn 7.0%-10.0%, Cr 0.90%-1.50%, Al 0.15%-0.25%, microalloying elements 0.10%-0.15%, Si 1.0%-1.5%, and the rest are Fe and unavoidable impurities.

[0033] In an optional embodiment of the present invention, the hot-formed steel contains retained austenite and martensite, and the martensite is lath martensite.

[0034] It should be noted that after the martensitic transformation of steel, a part of the untransformed austenite that is always retained after quenching is called retained austenite.

[0035] Martensite and residual austenite are both important components of steel, and they belong to two different metal structures. Among them, austenite is a very soft and tough structure, which is formed in the process of maintaining a certain period of time at high temperature. Austenite is a balanced structure. In an iron-carbon alloy at high temperature, due to the increase in temperature, carbon atoms transform from body-centered cubic iron to face-centered cubic iron, forming a uniform solid solution. This solid solution is austenite, which has high toughness. The formation of austenite is a diffusion transformation process, that is, the formation of austenite requires the migration of carbon atoms, and this process is very slow and needs to be maintained at high temperature for a certain period of time to complete. Therefore, the formation of austenite is affected by time and temperature. The longer the time and the higher the temperature, the more austenite is formed, and the shorter the time and the lower the temperature, the less austenite is formed.

[0036] Austenite is a mass structure formed by single crystal crystallization, embedded in steel material, improving the performance of steel. Austenite toughening includes deformation of austenite to relieve stress concentration at crack tip and inhibit crack propagation, and also includes plasticity induced by phase transformation of austenite to martensite. Since reverse transformed austenite cuts the deformation nucleus and grows by diffusion, reverse transformed austenite contains a large number of crystal defects and a high solute content, and its mechanical stability is improved. The residual reverse transformed austenite with high mechanical stability is distributed in thin sheets between the lath martensite bundles or around the lamellar martensite, which is very beneficial to improving the toughness of the material. It can not only prevent the crack from propagating between martensite laths, but also slow down the stress concentration caused by the dislocation front when the crack is densely arranged between martensite laths.

[0037] Martensite is a structure with high hardness and low toughness. It is formed in the process of rapid cooling at high temperature. Martensite is a non-equilibrium structure. When austenite at high temperature is rapidly cooled to low temperature, due to the rapid cooling rate, austenite does not have time to transform into other structures, but directly becomes a supersaturated solid solution, which contains a large number of carbon atoms. These carbon atoms cause the lattice of martensite to distort, resulting in high hardness and low toughness of martensite. The formation of martensite is a non-diffusion transformation process, that is, the formation of martensite does not require the migration of atoms, but is achieved through the rearrangement of atoms. This process is very fast and can be completed in a few seconds or even milliseconds. Therefore, the formation of martensite is not affected by time, but only by temperature. The lower the temperature, the more martensite is formed, and the higher the temperature, the less martensite is formed. In the martensitic transformation process, the untransformed austenite is the residual austenite.

[0038] The hot-formed steel produced by the present invention is a complex phase structure of residual austenite and martensite. The hot-formed steel with the complex phase structure has the characteristics of high yield and high plasticity and has excellent deformation resistance.

[0039] Furthermore, in terms of volume fraction, the volume fraction of retained austenite is 10%-20%; and the volume fraction of martensite is 80%-90%.

[0040] In a second aspect, an embodiment of the present invention provides a method for preparing the aforementioned hot-formed steel, comprising the following steps:

[0041] preparing raw materials according to the composition ratio of hot-formed steel, and forming the raw materials into slabs;

[0042] The slab is subjected to multiple hot rolling treatments, multiple cold rolling treatments, heating treatments and quenching treatments to obtain hot-formed steel.

[0043] In an optional embodiment of the present invention, the raw material is subjected to a melting process, a casting process and a forging process to obtain a slab;

[0044] The melting temperature of the raw materials is 1200°C-2000°C, and the thickness of the produced slab is 8mm-12mm.

[0045] It should be noted that the present invention does not impose any particular limitation on the time of the melting treatment, and the setting of the melting temperature is directly related to the raw material composition and raw material amount of the hot-formed steel; the setting of the melting temperature and time can be reasonably adjusted according to the amount of raw materials to be processed, so that all the raw materials are finally melted into molten steel.

[0046] Specifically, the raw materials prepared according to the ratio are placed in a blast furnace or an electric arc furnace for high-temperature melting treatment to produce molten steel; after the raw materials of the molten steel are evenly mixed, they are cast and forged to produce slabs.

[0047] It should be noted that the specific size of the slab can be reasonably cut according to actual needs. The thickness of the slab prepared in the present invention is 8mm-12mm.

[0048] In an optional embodiment of the present invention, before the slab is hot-rolled, the process further includes: heating the slab to 1200° C.-1300° C. and keeping the temperature for 1 h-2 h.

[0049] The purpose of heating and heat preservation before hot rolling is to make the raw materials have sufficient plasticity and reduce deformation resistance; by controlling the heating temperature and time, the grain size and distribution of the metal can be changed, the internal structure of the metal can be improved, and thus the performance of the metal can be improved; in addition, heating and heat preservation can make the metal more uniform during the rolling process, reduce internal stress, and improve product quality and performance.

[0050] Furthermore, the starting temperature of the hot rolling process is 1150°C-1250°C, and the final rolling temperature of the hot rolling process is 800°C-850°C.

[0051] It should be noted that the starting rolling temperature is 1150℃-1250℃, which makes the steel billet easy to deform and process, improves plasticity, and makes the rolling process easier; the final rolling temperature is usually controlled at 800℃-850℃ to ensure that the hot-rolled steel strip can form an ideal metallographic structure and grain size during the rolling process, so as to obtain good mechanical properties.

[0052] In an optional embodiment of the present invention, the number of hot rolling treatments is 3-6 times, and the reduction amount of each hot rolling treatment is 10%-15%; the total reduction amount of the hot rolling treatment is 45%-60%; and the thickness of the hot-rolled steel plate obtained by the hot rolling treatment is 3mm-4mm.

[0053] It should be noted that the reduction refers to the amount by which the height of the rolled piece is reduced during the rolling process. It is directly related to the degree of deformation of the material and the dimensional accuracy of the final product. During the rolling process, precise control of the height, width and length of the material can be achieved by controlling the reduction. Specifically, the calculation of the reduction involves the change in height of the rolled piece before and after rolling, which is usually expressed as a percentage, that is, the ratio of the reduction to the original height of the rolled piece. This deformation parameter is of great significance for ensuring product quality, improving material properties and optimizing the production process.

[0054] Hot rolled steel sheets are obtained by air cooling after hot rolling; specifically, the hot rolled steel is placed in the atmosphere to cool naturally.

[0055] In an embodiment of the present invention, the number of hot rolling treatments and the reduction amount of each hot rolling treatment are set according to the specifications of the slab actually processed; it should be noted that it is directly related to the thickness of the hot-rolled steel plate and the hardness of the product to be finally obtained, and can be reasonably adjusted according to the specifications and needs of the slab actually processed.

[0056] In an optional embodiment of the present invention, the number of cold rolling treatments is 3-6 times, and the reduction amount of each cold rolling treatment is 10%-15%, and the total reduction amount of the cold rolling treatment is 45%-60%;

[0057] The thickness of the cold-rolled steel sheet obtained by cold rolling treatment is 1.2mm-2mm.

[0058] It should be noted that the number of cold rolling treatments and the amount of reduction for each cold rolling treatment are set according to the specifications of the hot-rolled steel plates actually processed; it is directly related to the thickness of the cold-rolled steel plates and the hardness of the products that are ultimately desired to be obtained, and can be reasonably adjusted according to the specifications and needs of the slabs actually processed.

[0059] In an optional embodiment of the present invention, the cold-rolled steel sheet is heated at a temperature 80° C.-90° C. higher than the Ac3 temperature of the cold-rolled steel sheet, and the heating time of the cold-rolled steel sheet is 5 min-10 min.

[0060] It should be noted that the Ac3 temperature represents the transformation process of ferrite to retained austenite in the steel material during heating, which is directly related to the raw materials in the steel.

[0061] The temperature of the embodiment of the present invention is 80°C-90°C higher than the Ac3 temperature of the cold-rolled steel plate. The setting of this temperature can ensure that the ferrite in the cold-rolled steel is converted into residual austenite as much as possible to obtain a single austenite structure; in addition, it also helps to reduce the chemical composition segregation and organizational heterogeneity in the metal casting.

[0062] If the temperature is lower than the Ac3 temperature, it will lead to the presence of soft tissue ferrite, which will affect the hardness and performance of the material.

[0063] Specifically, when the content of ferrite in steel is high, the following disadvantages will occur: mainly including low yield strength, easy deformation, high room temperature brittleness and crack sensitivity, easy wrinkling, poor resistance to intergranular corrosion and cold brittleness. The high content of ferrite in steel affects the hardness and performance of the material, which in turn limits its application areas. Therefore, it is necessary to heat the cold-rolled steel sheet to make it completely austenitic.

[0064] The heating treatment time of cold-rolled steel sheets needs to be reasonably adjusted according to the specific material type, heat treatment purpose and process requirements. Reasonable control of time is to avoid excessive grain growth or overburning while maintaining material properties.

[0065] In an optional embodiment of the present invention, the quenching treatment is selected from any one of mold quenching or water medium quenching; the temperature of the quenching treatment is 25°C-55°C, and the cooling rate of the quenching treatment is 50°C / s-100°C / s.

[0066] It should be noted that mold quenching is a heat treatment process that aims to change the internal structure of mold steel through heating, insulation and rapid cooling, thereby improving the hardness, strength and wear resistance of hot-formed steel and extending the service life of steel. The heating temperature, insulation time and cooling method need to be determined according to the specific material composition and requirements.

[0067] There is no universally applicable temperature for mold quenching. The quenching temperature varies according to the material of the workpiece being quenched. In the embodiment of the present invention, the quenching temperature is 50° C. and the holding time is 15s-20s.

[0068] Water medium quenching uses water as the quenching medium; it has strong cooling capacity, wide source, low price, and its composition is not easy to deteriorate. However, the rapid cooling rate of water also brings some potential problems. Due to the excessive cooling capacity in the low temperature zone, metals quenched by water usually have higher hardness, but may also become relatively brittle, increasing the risk of cracking of metal materials during the quenching process.

[0069] Furthermore, the specific implementation process of mold quenching in the embodiment of the present invention is: quickly transfer the completely austenitized cold-rolled steel plate to the copper mold for rapid cooling, and accurately control the temperature of the copper mold by adjusting the water cooling system.

[0070] The specific implementation process of water medium quenching is: quickly transfer the completely austenitized cold-rolled steel sheet to the water medium for rapid cooling. In other embodiments of the present invention, other reasonable quenching methods can be selected according to actual needs.

[0071] It should be noted that the mold quenching adopted by the present invention does not require other processes such as quenching partitioning during the quenching treatment. It has the following advantages: it does not need to be kept warm at a specific temperature, and mold quenching can retain more austenite. This is mainly because the cooling rate of mold quenching is slow. During the quenching process, the supersaturated carbon atoms in the martensite have enough time to diffuse into the austenite, thereby stabilizing the austenite. After the mold quenching treatment of the present invention, a complex phase structure with residual austenite and lath martensite is obtained. The volume fraction of the residual austenite is 10%-20%; the volume fraction of the lath martensite is 80%-90%.

[0072] In the complex phase structure, the lath martensite matrix maintains the high yield strength of the hot-formed steel, and the phase transformation-induced plasticity of the residual austenite greatly improves the plasticity of the hot-formed steel. The resulting medium manganese hot-formed steel has both high yield and high plasticity and has excellent resistance to deformation.

[0073] In a third aspect, an embodiment of the present invention provides a use of the aforementioned hot-formed steel or the hot-formed steel obtained by the aforementioned preparation method in manufacturing automobile parts;

[0074] The components include at least one of an A-pillar, a B-pillar, a roof beam, an anti-collision beam and a bumper.

[0075] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0076] Example 1

[0077] This embodiment provides a medium manganese hot-formed steel, and the preparation method thereof comprises the following steps:

[0078] S1. Prepare raw materials according to the composition ratio of hot-formed steel, place the prepared raw materials in a blast furnace or an electric arc furnace for high-temperature melting treatment to obtain molten steel; after the molten steel is evenly mixed, it is cast and forged to obtain a slab; the slab includes the following components by mass fraction: C 0.21%, Mn 9.70%, Cr 0.98%, Al 0.20%, Nb 0.10%, Si1.2%, and the rest is Fe and unavoidable impurities.

[0079] S2. The slab obtained in step S1 is heated to 1200°C, kept warm for 1 hour, and then hot-rolled for 4 times. The starting rolling temperature is 1150°C, the reduction amount of each hot rolling treatment is about 12%, the total reduction amount is 50%, the final rolling temperature is 850°C, and the hot-rolled steel plate is air-cooled after hot rolling. The thickness of the hot-rolled steel plate is 4 mm.

[0080] S3. The hot-rolled steel sheet obtained in step S2 is cold-rolled 5 times, each cold-rolling treatment has a reduction of about 10%, and the total reduction is 50%, and finally a cold-rolled steel sheet A1 having a thickness of 2 mm is obtained;

[0081] S4. The cold-rolled steel sheet is heated at 810°C, which is 80°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0082] It should be noted that the Ac3 temperature of the cold-rolled steel sheet A1 measured by a thermal simulation tester (Gleeble-3500) is 730°C, so the heating treatment temperature of the cold-rolled steel sheet is 810°C.

[0083] S5. The cold-rolled steel sheet A2 obtained in step S4 is quickly placed in a pure copper mold for stamping and quenching treatment. The quenching cooling rate is 50°C / s and the temperature is 50°C to obtain hot-formed steel.

[0084] Example 2

[0085] This embodiment provides a medium manganese hot-formed steel, which differs from Embodiment 1 only in that:

[0086] S4. The cold-rolled steel sheet is heated at 780°C, which is 50°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0087] Example 3

[0088] This embodiment provides a medium manganese hot-formed steel, which differs from Embodiment 1 only in that:

[0089] S4. The cold-rolled steel sheet is heated at 840°C, which is 110°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining a cold-rolled steel sheet A2.

[0090] Example 4

[0091] This embodiment provides a medium manganese hot-formed steel, which differs from Embodiment 1 only in that:

[0092] S1. The prepared slab includes the following components by mass fraction: C 0.25%, Mn 7.10%, Cr 1.18%, Al 0.20%, Nb 0.15%, Si 1.0%, and the rest is Fe and unavoidable impurities.

[0093] S4. The cold-rolled steel sheet is heated at 840°C, which is 80°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0094] It should be noted that the Ac3 temperature of the cold-rolled steel sheet A1 measured by a thermal simulation tester (Gleeble-3500) is 760°C, so the heating treatment temperature of the cold-rolled steel sheet is 840°C.

[0095] Example 5

[0096] This embodiment provides a medium manganese hot-formed steel, which differs from Embodiment 4 only in that:

[0097] S4. The cold-rolled steel sheet is heated at 810°C, which is 50°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0098] Example 6

[0099] This embodiment provides a medium manganese hot-formed steel, which differs from Embodiment 4 only in that:

[0100] S4. The cold-rolled steel sheet is heated at 870°C, which is 110°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0101] Example 7

[0102] This embodiment provides a medium manganese hot-formed steel, which differs from Embodiment 1 only in that:

[0103] S1. The prepared slab includes the following components by mass fraction: C 0.21%, Mn 9.70%, Cr 0.98%, Al 0.20%, Ti 0.10%, Si 1.2%, and the rest is Fe and unavoidable impurities.

[0104] S4. The cold-rolled steel sheet is heated at 815°C, which is 80°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0105] It should be noted that the Ac3 temperature of the cold-rolled steel sheet A1 measured by a thermal simulation tester (Gleeble-3500) is 735°C, so the heating treatment temperature of the cold-rolled steel sheet is 815°C.

[0106] Example 8

[0107] This embodiment provides a medium manganese hot-formed steel, which differs from Embodiment 7 only in that:

[0108] S4. The cold-rolled steel sheet is heated at 785°C, which is 50°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0109] Example 9

[0110] This embodiment provides a medium manganese hot-formed steel, which differs from Embodiment 7 only in that:

[0111] S4. The cold-rolled steel sheet is heated at 845°C, which is 110°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0112] Example 10

[0113] This embodiment provides a medium manganese hot-formed steel, which differs from Embodiment 1 only in that:

[0114] S5. The cold-rolled steel sheet A2 obtained in step S4 is quenched with water as the quenching medium to obtain hot-formed steel.

[0115] Comparative Example 1

[0116] This comparative example provides a commercial hot-formed steel commonly used in the current market, namely 22MnB5, which differs from Example 1 only in that:

[0117] S1. The prepared slab includes the following components by mass fraction: C 0.22%, Mn 1.18%, Cr 0.16%, Al 0.03%, Ti 0.04%, Si 0.22%, B 0.002%, and the rest are Fe and unavoidable impurity elements.

[0118] S4. The cold-rolled steel sheet is heated at 920°C, which is 80°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0119] It should be noted that the Ac3 temperature of the cold-rolled steel sheet A1 measured by a thermal simulation tester (Gleeble-3500) is 840°C, so the heating treatment temperature of the cold-rolled steel sheet is 920°C.

[0120] Comparative Example 2

[0121] This comparative example provides a commercial hot-formed steel commonly used in the current market, namely 22MnB5, which differs from comparative example 1 only in that:

[0122] S4. The cold-rolled steel sheet is heated at 890°C, 50°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0123] Comparative Example 3

[0124] This comparative example provides a commercial hot-formed steel commonly used in the current market, namely 22MnB5, which differs from comparative example 1 only in that:

[0125] S4. The cold-rolled steel sheet is heated at 870°C, 30°C higher than the Ac3 temperature of the cold-rolled steel sheet A1 obtained in step S3, and kept warm for 5 minutes to completely austenitize the cold-rolled steel sheet, thereby obtaining the cold-rolled steel sheet A2.

[0126] Test Example 1

[0127] In this test example, the phase structure of the hot-formed steel prepared in Examples 1-3 and Comparative Example 1 was tested using an electron backscatter diffractometer (EBSD), model Oxford Symmetry S3, with parameters of 20 kV acceleration voltage and 0.1 μm step size. The specific phase distribution of Examples 1-3 and Comparative Example 1 is shown in Figure 1 .

[0128] from Figure 1 It can be seen that the medium manganese hot-formed steel prepared in Example 1 contains lath martensite and austenite, the medium manganese hot-formed steel prepared in Example 2 contains ferrite, lath martensite and austenite, and the medium manganese hot-formed steel prepared in Example 3 contains lath martensite and austenite. Compared with Example 1, the lath martensite and austenite in Example 3 are coarser. The hot-formed steel 22MnB5 prepared in Comparative Example 1 contains only lath martensite and no austenite.

[0129] Test Example 2

[0130] In this test example, the hot-formed steel prepared in Examples 1-3 and Comparative Example 1 was subjected to engineering strain-engineering stress test. The testing instrument was a universal tensile testing machine, model LE5504, and the parameters were strain rate 10 -3 s -1 , the strain value is monitored and controlled by the extensometer. See the relevant curve diagram Figure 2 .

[0131] from Figure 2 It can be seen that compared with Examples 2 and 3, Example 1 exhibits the highest yield strength, tensile strength and elongation after fracture. The yield strength of Example 2 is significantly lower than that of the other examples. In addition, the elongation after fracture of Examples 1 to 3 is more than twice that of Comparative Example 1.

[0132] Test Example 3

[0133] In this test example, the austenite and martensite contents of the hot-formed steels prepared in Examples 1-10 and Comparative Examples 1-3 were tested by electron backscatter diffraction technology. The testing instrument was an electron backscatter diffractometer (EBSD), model Oxford Symmetry S3, with parameters of acceleration voltage 20 kV and step length 0.1 μm. The specific contents of austenite and lath martensite in the hot-formed steels are shown in Table 1.

[0134] Table 1 Austenite content and martensite content in hot-formed steel

[0135]

[0136] Combination Figure 1 It can be seen from Table 1 that when the heating temperature is 80°C higher than the Ac3 temperature of the cold-rolled steel sheet and lower than 110°C, the structure of the medium manganese hot-formed steel (Examples 1, 3, 4, 6, 7 and 9) is a complex phase structure, which is composed of retained austenite and martensite, and the content of retained austenite is 10% to 15%. In addition to retained austenite and martensite, the medium manganese hot-formed steel prepared in Examples 2 and 8 also has untransformed ferrite. When the heating temperature exceeds 110°C, the content of retained austenite remains basically unchanged. When the heating temperature is 50°C higher than the Ac3 temperature of the cold-rolled steel sheet and lower than 80°C, ferrite will still exist despite the high content of retained austenite. The complex phase structure of the above-mentioned medium manganese hot-formed steel is less affected by the change of the type of microalloying elements. For commercial hot-formed steel 22MnB5, when the heating temperature is 30°C higher than the Ac3 temperature of the cold-rolled steel sheet, the retained austenite content is 0, and after the heating temperature is further increased, the retained austenite content remains at 0. However, the different quenching methods (die quenching in Example 1 and water medium quenching in Example 10) have little effect on the austenite content and martensite content in the manganese hot-formed steel in the product.

[0137] Test Example 4

[0138] In this test example, the mechanical properties of the hot-formed steel prepared in Examples 1-10 and Comparative Examples 1-3 were tested. Specifically, the yield strength, tensile strength and elongation after fracture of the hot-formed steel were tested according to the national standard GB / T228.1-2010; the testing instrument was a universal tensile testing machine, model LE5504, and the parameters were strain rate 10 -3 s -1 The strain value is monitored and controlled by the extensometer. The performance test results are shown in Table 2.

[0139] Table 2 Mechanical properties test data of hot-formed steel

[0140]

[0141] As can be seen from Table 2, the yield strength, tensile strength and elongation after fracture in Examples 1-10 all increase first and then decrease with the increase of the temperature of the cold-rolled steel sheet treatment, wherein the yield strength is as high as 1083MPa under the condition of 80°C higher than the Ac3 temperature of the cold-rolled steel sheet A1, which is 12.8% higher than the yield strength in Comparative Example 1; the elongation after fracture is as high as 18.7% under the condition of 80°C higher than the Ac3 temperature of the cold-rolled steel sheet A1, which is 152.7% higher than the yield strength in Comparative Example 1. The mechanical properties of the above-mentioned medium manganese hot-formed steel are slightly affected by the type of microalloying elements, and are mainly related to the heating temperature of the cold-rolled steel sheet A1.

[0142] The yield strength and tensile strength of the commercial hot-formed steel 22MnB5 in Comparative Examples 1-3 decrease with the increase of the temperature of the cold-rolled steel plate treatment, and the optimal values ​​of the yield strength and tensile strength are obtained under the condition of 30°C higher than the Ac3 temperature of the cold-rolled steel plate A1. When the structure of the medium manganese hot-formed steel (Examples 1, 3, 4, 6, 7 and 9) is mainly composed of 10%-15% retained austenite and 85%-90% martensite, it enables it to have both high yield strength and good plasticity. However, when a certain amount of ferrite is present (Examples 2 and 8), the yield strength is significantly reduced. When there is no retained austenite, the elongation after fracture of Comparative Example 1 is much lower than that of the medium manganese hot-formed steel. The different quenching treatment methods (Example 1 is die quenching, and Example 10 is water medium quenching) have little effect on the mechanical properties of the medium manganese hot-formed steel in the product.

[0143] In summary, the preparation method of the medium manganese hot-formed steel of the present invention can achieve full austenitization of the cold-rolled steel plate by controlling the heating temperature of the cold-rolled steel plate to be 80°C-90°C higher than its Ac3 temperature, thereby avoiding the presence of ferrite at room temperature. A large amount of residual austenite fraction can greatly improve the elongation of the medium manganese hot-formed steel, thereby achieving the purpose of improving the plasticity of the hot-formed steel while maintaining the strength of the hot-formed steel.

[0144] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A medium manganese hot-formed steel, characterized in that: The hot-formed steel comprises the following components by mass fraction: C 0.20%-0.40%, Mn 9.7%-11.0%, Cr 0.90%-2.00%, Al 0.10%-0.30%, microalloying elements 0.05%-0.15%, Si 1.0%-2.0%, the rest is Fe and unavoidable impurities; The microalloying element is selected from any one of Nb and Ti; The hot-formed steel contains 10%-20% by volume of retained austenite and 80%-90% by volume of lath martensite; The method for preparing the hot-formed steel comprises the following steps: preparing raw materials according to the composition ratio of the hot-formed steel, and forming the raw materials into slabs; The slab is subjected to multiple hot rolling treatments, multiple cold rolling treatments, heating treatments and quenching treatments to obtain the hot-formed steel; The cold-rolled steel sheet is subjected to a heating treatment at a temperature 80°C to 90°C higher than the Ac3 temperature of the cold-rolled steel sheet obtained by the cold rolling treatment, and the heating treatment time is 5min to 10min; The quenching treatment is selected from any one of mold quenching or water medium quenching; the temperature of the quenching treatment is 25°C-55°C; the cooling rate of the quenching treatment is 50°C / s-100°C / s.

2. The hot-formed steel according to claim 1, characterized in that: The hot-formed steel comprises the following components by mass fraction: C 0.20%-0.30%, Mn 9.7%-10.0%, Cr 0.90%-1.50%, Al 0.15%-0.25%, microalloying elements 0.10%-0.15%, Si 1.0%-1.5%, and the rest are Fe and unavoidable impurities.

3. The hot-formed steel according to claim 1, characterized in that: The raw material is subjected to melting, casting and forging processes to obtain the slab; The melting temperature of the raw material is 1200° C.-2000° C., and the thickness of the obtained slab is 8 mm-12 mm.

4. The hot-formed steel according to claim 1, characterized in that: The starting temperature of the hot rolling process is 1150°C-1250°C, and the final temperature of the hot rolling process is 800°C-850°C; The number of hot rolling treatments is 3-6 times, and the reduction amount of each hot rolling treatment is 10%-15%; the total reduction amount of the hot rolling treatment is 45%-60%; The thickness of the hot-rolled steel plate obtained by the hot rolling process is 3 mm to 4 mm.

5. The hot-formed steel according to claim 1, characterized in that: The number of cold rolling treatments is 3-6 times, and the reduction amount of each cold rolling treatment is 10%-15%, and the total reduction amount of the cold rolling treatment is 45%-60%; The thickness of the cold-rolled steel sheet obtained by the cold rolling process is 1.2 mm to 2 mm.

6. Application of the hot-formed steel according to any one of claims 1 to 5 in manufacturing automobile parts; The components include at least one of an A-pillar, a B-pillar, a roof beam, an anti-collision beam and a bumper.