Multi-component electrically responsive liquid photonic crystals, devices, and their preparation and applications

By modifying and mixing polyhydroxy compounds with different chemical color reflectivity, the problem of brightness and saturation regulation in electrically responded photonic crystals is solved, and simultaneous regulation and color uniformity are achieved while brightness and saturation are achieved.

CN118584562BActive Publication Date: 2024-11-08WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411069699.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

It is difficult for existing electrically responsive photonic crystals to simultaneously regulate brightness and saturation, and colloidal particles with different chemical chromatic reflectivity problems are prone to inconsistent agglomeration and electrophoretic rates.

Method used

Polyhydroxy compounds are used to coordinate complex or adsorb colloidal particles with different chemical color reflectivity, so that their surfaces have the same chemical and physical characteristics, avoid agglomeration, and control brightness and saturation through mixing in different proportions.

Benefits of technology

Continuous regulation of brightness and saturation during electrophoresis is achieved, color unevenness is avoided, and color performance and stability of electrically responded photonic crystals are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118584562B_ABST
    Figure CN118584562B_ABST
Patent Text Reader

Abstract

The present invention discloses a multi-component electrically responsive liquid photonic crystal, a device, and its preparation and application, comprising colloidal particles of two or more chemical colors with different reflectivity that are coordinated, complexed and adsorbed with polyhydroxy compounds, and a polar solvent for dispersing the two or more colloidal particles with different chemical colors and reflectivity; the effect of simultaneously regulating brightness and saturation is achieved through the compounding of multi-component colloidal nanoparticles and the modification of polyhydroxy compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photonic crystal display technology, and in particular to a multi-component electrically responsive liquid photonic crystal, a device, and preparation and application thereof. Background Art

[0002] Electrophoretic electroresponsive photonic crystals refer to responsive photonic crystals that, under the action of an external electric field, charged colloidal particles undergo electrophoretic movement toward the oppositely charged plates, causing the distance between particles to change, thereby achieving color change. It can achieve continuous color changes under relatively fine voltage control, so it has more development prospects in the fields of display, camouflage, smart windows and anti-counterfeiting. Based on this, electroresponsive photonic crystals have attracted a large number of researchers to improve their performance in terms of colloidal particles, dispersion media and electrodes. Since different types of colloidal particles are prepared by different processes, the charge states on their surfaces are not completely consistent, which leads to the fact that in previous studies of electroresponsive photonic crystals, only single-component colloidal particles are often selected to prepare electroresponsive photonic crystals. However, the types of materials that can be used to prepare monodisperse colloidal particle primitives for electrophoretic electroresponsive photonic crystals are limited, so the brightness and color saturation of the electrophoretic electroresponsive photonic crystals constructed by them are also limited. In practical applications, people's demand for color, brightness and saturation is the richer the better. Therefore, it is particularly important to develop a simple method to prepare electrophoretic electroresponsive photonic crystals with continuously adjustable brightness and saturation.

[0003] To solve the above problems, the present application proposes to treat monodisperse colloidal particles prepared from materials of various components with polyhydroxy compounds, so that the charge properties of their surfaces are similar but the chemical color reflectances are different. By compounding these various colloidal particles with different chemical color reflectances in different proportions, a scheme of an electrically responsive photonic crystal capable of continuously regulating brightness and saturation is obtained, thereby realizing the regulation of brightness and saturation of the electrically responsive photonic crystal. Summary of the invention

[0004] In view of this, the present application provides a multi-component electrically responsive liquid photonic crystal, device, and preparation and application thereof, which are used for liquid photonic crystals or devices to solve the technical problem that brightness and saturation cannot be adjusted simultaneously.

[0005] In order to achieve the above technical objectives, this application adopts the following technical solutions:

[0006] In a first aspect, the present application provides a multi-component electrically responsive liquid photonic crystal, comprising two or more colloidal particles with different chemical color reflectances; all the colloidal particles have polyhydroxy compounds coordinated, complexed or adsorbed on their surfaces; and all the particles are dispersed in a polar solvent.

[0007] Preferably, the average particle size of the colloidal particles is 80-300 nm.

[0008] Preferably, the solid content of the multi-component electrically responsive liquid photonic crystal is 10-80wt%.

[0009] Preferably, the colloidal particles include colloidal particles having any two or more of the oxides or sulfides of iron, copper, molybdenum, vanadium, manganese, cobalt, chromium, ruthenium, nickel, terbium, rhodium, tungsten, cerium, aluminum, zinc, cadmium, europium, gadolinium, zirconium on the surface or in the body, as well as SiO2 and polystyrene colloidal particles; the polar solvent includes one or more of carbonate, carboxylic acid ester, ether, alkanol, acetonitrile, dimethyl sulfoxide, pure water, and acetone; the carbonate includes propylene carbonate, ethylene carbonate, butylene carbonate, , dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate; the carboxylic acid ester includes at least one of γ-butyrolactone, ethyl acetate, and methyl formate; the ethers include at least one of tetrahydrofuran, 2-methyl-tetrahydrofuran, dimethoxymethane, and 1,2-dimethoxyethane; the polyhydroxy compound includes one or a mixture of tannic acid, catechin, epigallocatechin, epigallocatechin gallate, pyroxetine, gluconic acid, glucose, and gluconate.

[0010] In a second aspect, the present application provides a method for preparing a multi-component electrically responsive liquid photonic crystal, the steps of which are as follows:

[0011] S1. using a polar solution containing a polyhydroxy compound to coordinate, complex or adsorb two or more colloidal particles with different chemical color reflectances one or more times, and after the reaction is completed, washing away the free polyhydroxy compound in the system to obtain a mixture of two or more colloidal particles with different chemical color reflectances that are coordinated, complexed or adsorbed with polyhydroxy compounds;

[0012] S2. Disperse the mixture of two or more colloidal particles with different chemical color reflectivity that are coordinated, complexed or adsorbed with polyhydroxy compounds in a polar solution to form a colloidal particle dispersion system with a certain concentration, thereby obtaining the multi-component electrically responsive liquid photonic crystal.

[0013] In a third aspect, the present application provides an electrically responsive photonic crystal device, which is obtained by sealing a multi-component electrically responsive liquid photonic crystal between transparent conductive electrode plates, and the concentration of the polyhydroxy compound contained in the polar solution is greater than or equal to 0.1 mg / mL.

[0014] Preferably, the conductive electrode plates include one or more of high-purity silver sheets, high-purity copper sheets, transparent ITO conductive glass, FTO conductive glass, and ITO-PET flexible conductive film, and the spacing between the two conductive electrode plates is 10-1000 μm.

[0015] In a fourth aspect, the present application provides an application of an electrically responsive photonic crystal device in color control of an electrophoretic display.

[0016] Preferably, the voltage applied for color regulation is 0.1-2.0V.

[0017] The beneficial effect of the present invention is that, under the premise of using colloidal nanoparticles with different chemical color reflectances, this scheme uses polyhydroxy compounds to modify the two separately, and performs coordination, complexation and modification so that their surfaces have the same chemical and physical properties, thereby preventing them from agglomerating during the mixing process and the electrophoresis process, and also avoiding the phenomenon of uneven color due to inconsistent electrophoresis rates of particles caused by different surface charges of different particles under an electric field, thereby achieving the effect of simultaneously regulating brightness and saturation. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The maximum reflectance bar graph of dry powders with different particle sizes;

[0019] Figure 2 Field emission scanning electron microscope images of the two-component particles before and after mixing in Example 1;

[0020] Figure 3 This is a digital photo of the electrically responsive liquid photonic crystal prepared in Example 1-5 without applying an electric field;

[0021] Figure 4 This is a comparison chart of the reflectivity before and after applying an electric field after the two-component particles are mixed in different proportions in Examples 1-5;

[0022] Figure 5 The brightness relationship diagram of each sample before and after the electric field is applied after the two-component particles are mixed in different proportions in Examples 1-5;

[0023] Figure 6 Digital photos of the single-component electrically responsive photonic crystals prepared in Comparative Examples 1 and 2 and the dual-component electrically responsive photonic crystals of Example 2 under the condition of no electric field being applied;

[0024] Figure 7 The reflectivity spectra of the single-component electro-responsive photonic crystals of Comparative Examples 1 and 2 and the dual-component electro-responsive photonic crystals of Example 2 before and after the electric field is applied;

[0025] Figure 8 The figure is a relationship diagram of the brightness of the single-component electric response photonic crystals of comparative examples 1 and 2 and the two-component electric response photonic crystals of embodiment 2 before and after the electric field is applied;

[0026] Fig. 9 This is a digital photo of particles of different particle sizes in Examples 9-11 mixed at a ratio of 1:1 without applying an electric field;

[0027] Fig.10 is the reflectivity corresponding to the mixture of particles of different particle sizes in Examples 9-11 at a ratio of 1:1 under the condition that no electric field is applied;

[0028] Fig.11 These are digital photos of the two-component particles in Examples 12-18 after mixing at different mass fractions without applying an electric field;

[0029] Fig.12 is the reflectivity corresponding to the mixture of the two-component particles in Examples 12-18 at different mass fractions without applying an electric field;

[0030] Fig.13 The reflectivity spectra of the single-component electro-responsive photonic crystals of Comparative Examples 3 and 4 and the dual-component electro-responsive photonic crystals of Example 19 before and after the application of an electric field;

[0031] Fig.14 The figure is a relationship diagram of the brightness of the single components of comparative examples 3 and 4 and the electrically responsive photonic crystal of example 19 before and after the electric field is applied;

[0032] Fig.15 The reflectivity spectra of the single-component electro-responsive photonic crystals of Comparative Examples 5 and 6 and the dual-component electro-responsive photonic crystals of Example 20 before and after the application of an electric field;

[0033] Fig.16 The figure is a relationship diagram of the brightness of the single-component electric response photonic crystals of comparative examples 5 and 6 and the two-component electric response photonic crystals of embodiment 20 before and after the electric field is applied;

[0034] Fig.17 The reflectivity spectra of the single-component electro-responsive photonic crystals of Comparative Examples 7 and 8 and the dual-component electro-responsive photonic crystals of Example 21 before and after the application of an electric field;

[0035] Fig.18 The figure is a relationship diagram of the brightness of the single-component electric response photonic crystals of Comparative Examples 7 and 8 and the two-component electric response photonic crystals of Example 21 before and after the electric field is applied;

[0036] Fig.19 The reflectivity spectra of the single-component electric response photonic crystals of Comparative Examples 9 and 10 and the two-component electric response photonic crystals of Example 22 after crystallization;

[0037] Fig. 20 Spectra of the electrically responsive photonic crystal prepared by mixing the multi-component particles at different voltages in Example 23;

[0038] Fig.21 These are digital photos of the electrically responsive photonic crystal prepared by mixing the multi-component particles in a ratio of 1:1:1 under different voltages in Example 23;

[0039] Fig. 22This is the electrical response spectrum of the liquid photonic crystal prepared by mixing multi-component particles in a ratio of 1:1:1 in Example 23. DETAILED DESCRIPTION

[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The present application provides a multi-component electrically responsive liquid photonic crystal, comprising two or more colloidal particles with different chemical color reflectances; all the colloidal particles have polyhydroxy compounds coordinated, complexed or adsorbed on their surfaces; and all the particles are dispersed in a polar solvent.

[0042] The advantage of selecting multi-component colloidal particles over single-component colloidal particles for preparing electrically responsive photonic crystals in this application is that, for colloidal particles with high reflectivity, since their refractive index is relatively close to that of polar solvents, the structural color saturation exhibited is low. To solve this problem, the technical personnel in this field introduce light-absorbing substances such as carbon black or black paper into the system. However, the introduction of light-absorbing substances such as carbon black may cause agglomeration inside the system and uneven color. When using colloidal particles with low reflectivity, the photonic crystals prepared therefrom have high color saturation, but due to their low reflectivity, the reflectivity and brightness of the device prepared by such colloidal particles are very low. However, directly mixing colloidal particles with darker chemical colors with colloidal particles with brighter chemical colors will cause them to agglomerate during the mixing process and the electrophoresis process, and it is not possible to achieve simultaneous regulation of brightness and saturation.

[0043] Therefore, this scheme uses colloidal nanoparticles of different chemical colors and brightness, and uses polyhydroxy compounds to modify them separately, carry out coordination, complexation and adsorption, so that their surfaces have the same chemical and physical properties, so that they will not agglomerate during the mixing process and electrophoresis process, and avoid the phenomenon of uneven color due to inconsistent electrophoresis rates of particles caused by different surface charges of different particles under the electric field, so as to achieve the effect of simultaneously regulating brightness and saturation.

[0044] The average particle size of the colloidal particles is 80-300nm.

[0045] The solid content of the multi-component electrically responsive liquid photonic crystal is 10-80wt%.

[0046] The range of colloidal particles includes colloidal particles having any two or more of the oxides or sulfides of iron, copper, molybdenum, vanadium, manganese, cobalt, chromium, ruthenium, nickel, terbium, rhodium, tungsten, cerium, aluminum, zinc, cadmium, europium, gadolinium, zirconium elements on the surface or in the body, as well as SiO2 and polystyrene colloidal particles; the polar solvent includes one or more of carbonate, carboxylic acid ester, ether, alkanol, acetonitrile, dimethyl sulfoxide, pure water, and acetone; the carbonate includes propylene carbonate, ethylene carbonate, butylene carbonate, carbonate The invention discloses a novel polyol comprising at least one of dimethyl ester, ethyl methyl carbonate and diethyl carbonate; the carboxylic acid ester comprises at least one of γ-butyrolactone, ethyl acetate and methyl formate; the ether comprises at least one of tetrahydrofuran, 2-methyl-tetrahydrofuran, dimethoxymethane and 1,2-dimethoxyethane; the polyhydroxy compound comprises one or a mixture of several of tannic acid, catechin, epigallocatechin, epigallocatechin gallate, pyroxetine, gluconic acid, glucose and gluconate.

[0047] Under the condition of determining the structure and composition of colloidal nanoparticles, those skilled in the art can obtain colloidal nanoparticles using known channels; the structure of colloidal nanoparticles includes one or more of single-type colloidal particles, colloidal particles@polymer (coating structure), and mixed-type colloidal particles.

[0048] In this scheme, tannic acid has multiple ortho-phenolic hydroxyl structures that can undergo coordination and complex reactions with a variety of metal ions, as well as its strong adhesion and can be ionized in polar solvents. Therefore, tannic acid can be modified on different nanoparticles to make their surfaces have the same chemical and physical properties, so that they will not agglomerate during the mixing process and the electrophoresis process.

[0049] The present application provides a method for preparing a multi-component electrically responsive liquid photonic crystal, the steps of which are as follows:

[0050] S1. using a polar solution containing a polyhydroxy compound to carry out one or more (≥1) coordination complexation or adsorption of two or more colloidal particles with different chemical color reflectances, so that the coordination complexation reaction or adsorption is fully completed, separating and retaining the solid product after the reaction, washing away the free polyhydroxy compound in the system, and obtaining a mixture of two or more colloidal particles with different chemical color reflectances that are coordinated, complexed or adsorbed with polyhydroxy compounds;

[0051] S2. Disperse the coordination complex and adsorbed polyhydroxy compound and the mixture of two or more colloidal particles with different chemical color reflectivity in a polar solution to form a colloidal particle dispersion system with a certain concentration, thereby obtaining the multi-component electrically responsive liquid photonic crystal.

[0052] In step S1, conventional dispersing means are used to achieve the modification of two or more colloidal particles having different chemical color reflectances by polyhydroxy compounds.

[0053] In the third aspect, the present application provides an electrically responsive photonic crystal device, which is obtained by sealing a multi-component electrically responsive liquid photonic crystal between transparent conductive electrode plates, wherein the concentration of the polyhydroxy compound contained in the polar solution is greater than or equal to 0.1 mg / mL, and the device is a multi-component low-angle-dependent electrically responsive photonic crystal device; the electrically responsive photonic crystal device can change the lattice spacing under different voltages to achieve color control, and the color saturation and brightness are high.

[0054] The conductive electrode plates include one or more of high-purity silver sheets, high-purity copper sheets, transparent ITO conductive glass, FTO conductive glass, and ITO-PET flexible conductive film. The spacing between the two conductive electrode plates is 10-1000 μm.

[0055] The present application provides an application of an electrically responsive photonic crystal device in color control of an electrophoretic display; the voltage applied for color control in the present application is 0.1-2.0V, and under different voltages, the electrically responsive photonic crystal device of the present application can achieve different color control.

[0056] The present solution is further described below through specific embodiments.

[0057] Example 1

[0058] A two-component electrically responsive liquid photonic crystal comprises Fe3O4 particles coordinated and complexed with tannic acid, CeO2 particles coordinated and complexed with tannic acid (colloidal nanoparticles with high reflectivity coordinated and complexed with polyhydroxy compounds), and a propylene carbonate solution; the average particle size of the CeO2 particles is 100 nm, the particle size of the ferroferric oxide particles is 100 nm, the solid content of the two-component electrically responsive liquid photonic crystal is 20%, and the mass ratio of the CeO2 particles to the ferroferric oxide particles is 9:1.

[0059] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0060] S1. The Fe3O4 particles are dispersed in a 60 mg / ml tannic acid propylene carbonate solution, and the CeO2 particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Fe3O4 particles and the CeO2 particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain Fe3O4 particles with a coordination complex having a polyhydroxy compound and CeO2 particles with a coordination complex having a polyhydroxy compound;

[0061] S2. Take 60 mg of a mixture of Fe3O4 particles coordinated and complexed with polyhydroxy compounds and CeO2 particles coordinated and complexed with polyhydroxy compounds, wherein the mass ratio of CeO2 particles to Fe3O4 particles is 9:1, disperse the above mixture in a 150 mg / mL tannic acid propylene carbonate solution, ultrasonically disperse it evenly, wash it by centrifugation with the propylene carbonate solution for 1 to 2 times, and then ultrasonically disperse it evenly in 199 μL of propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 20%, which has a green structural color and exhibits angle-independent characteristics.

[0062] Embodiment 2-5

[0063] A two-component electrically responsive liquid photonic crystal, the other contents of which are the same as those of Example 1, except that the mass ratios of CeO2 particles to ferrosoferric oxide particles are 7:3, 5:5, 3:7, and 1:9, respectively.

[0064] Example 6

[0065] A two-component electrically responsive liquid photonic crystal comprises Fe3O4 particles coordinated and complexed with tannic acid, CeO2 particles coordinated and complexed with tannic acid, and a propylene carbonate solution; the average particle size of the CeO2 particles is 85 nm, the particle size of the ferroferric oxide particles is 85 nm, the solid content of the two-component electrically responsive liquid photonic crystal is 20%, and the mass ratio of the CeO2 particles to the ferroferric oxide particles is 1:1.

[0066] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0067] S1. The Fe3O4 particles are dispersed in a 60 mg / ml tannic acid propylene carbonate solution, and the CeO2 particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Fe3O4 particles and the CeO2 particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain Fe3O4 particles with a coordination complex having a polyhydroxy compound and CeO2 particles with a coordination complex having a polyhydroxy compound;

[0068] S2. Take 60 mg of a mixture of Fe3O4 particles coordinated and complexed with polyhydroxy compounds and CeO2 particles coordinated and complexed with polyhydroxy compounds, wherein the mass ratio of CeO2 particles to Fe3O4 particles is 1:1, disperse the above mixture in a 150 mg / mL tannic acid propylene carbonate solution, ultrasonically disperse it evenly, wash it by centrifugation with the propylene carbonate solution for 1 to 2 times, and then ultrasonically disperse it evenly in 199 μL of propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 20%, and its structural color is blue.

[0069] Example 7

[0070] A two-component electrically responsive liquid photonic crystal, the other contents of which are the same as those of Example 6, except that the average particle sizes of CeO2 particles and Fe3O4 particles are both 150nm; a two-component electrically responsive liquid photonic crystal with a solid content of 30% is obtained, and its structural color is yellow.

[0071] Example 8

[0072] A two-component electrically responsive liquid photonic crystal, the other contents of which are the same as those of Example 6, except that the average particle sizes of CeO2 particles and Fe3O4 particles are both 200nm; a two-component electrically responsive liquid photonic crystal with a solid content of 30% is obtained, and its structural color is reddish brown.

[0073] Example 9

[0074] A two-component electrically responsive liquid photonic crystal comprises Fe3O4 particles coordinated and complexed with tannic acid, CeO2 particles coordinated and complexed with tannic acid, and a propylene carbonate solution; the average particle size of the CeO2 particles is 85 nm, the average particle size of the Fe3O4 particles is 100 nm, the solid content of the two-component electrically responsive liquid photonic crystal is 20%, and the mass ratio of the CeO2 particles to the Fe3O4 particles is 1:1.

[0075] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0076] S1. The Fe3O4 particles are dispersed in a 60 mg / ml tannic acid propylene carbonate solution, and the CeO2 particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Fe3O4 particles and the CeO2 particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain Fe3O4 particles with a coordination complex having a polyhydroxy compound and CeO2 particles with a coordination complex having a polyhydroxy compound;

[0077] S2. Take 60 mg of a mixture of Fe3O4 particles coordinated and complexed with polyhydroxy compounds and CeO2 particles coordinated and complexed with polyhydroxy compounds, wherein the mass ratio of CeO2 particles to Fe3O4 particles is 1:1, disperse the above mixture in a 150 mg / mL tannic acid propylene carbonate solution, ultrasonically disperse it evenly, wash it by centrifugation with the propylene carbonate solution for 1 to 2 times, and then ultrasonically disperse it evenly in 199 μL of propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 20%, and its structural color is blue.

[0078] Example 10

[0079] A two-component electrically responsive liquid photonic crystal, the other contents are the same as those of Example 9, except that the average particle size of CeO2 particles is 100nm, and the average particle size of Fe3O4 particles is 100nm; a two-component electrically responsive liquid photonic crystal with a solid content of 20% is obtained, and its structural color is green.

[0080] Embodiment 11

[0081] A two-component electrically responsive liquid photonic crystal, the other contents of which are the same as those of Example 9, except that the average particle size of CeO2 particles is 130nm, and the average particle size of Fe3O4 particles is 100nm; a two-component electrically responsive liquid photonic crystal with a solid content of 20% is obtained, and its structural color is yellow.

[0082] Example 12

[0083] A two-component electrically responsive liquid photonic crystal comprises Fe3O4 particles coordinated and complexed with tannic acid, CeO2 particles coordinated and complexed with tannic acid, and a propylene carbonate solution; the average particle size of the CeO2 particles is 100 nm, the average particle size of the Fe3O4 particles is 100 nm, the solid content of the two-component electrically responsive liquid photonic crystal is 5%, and the mass ratio of the CeO2 particles to the Fe3O4 particles is 1:1.

[0084] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0085] S1. The Fe3O4 particles are dispersed in a 60 mg / ml tannic acid propylene carbonate solution, and the CeO2 particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Fe3O4 particles and the CeO2 particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain Fe3O4 particles with a coordination complex having a polyhydroxy compound and CeO2 particles with a coordination complex having a polyhydroxy compound;

[0086] S2. Take 60 mg of a mixture of Fe3O4 particles coordinated and complexed with polyhydroxy compounds and CeO2 particles coordinated and complexed with polyhydroxy compounds, wherein the mass ratio of CeO2 particles to Fe3O4 particles is 1:1, disperse the above mixture in a 150 mg / mL tannic acid propylene carbonate solution, disperse it evenly by ultrasonication, and then wash it by centrifugation with the propylene carbonate solution for 1 to 2 times to obtain a mixed solution, and then ultrasonically disperse the mixed solution evenly in 946 μL of propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 5%, and its structural color is brown.

[0087] Embodiment 13

[0088] A two-component electrically responsive liquid photonic crystal, the other contents are the same as those of Example 8, except that in step S2, the mixed liquid is ultrasonically uniformly dispersed in 448 μL of propylene carbonate solution, so as to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 10%, and its structural color is red.

[0089] Embodiment 14

[0090] A two-component electrically responsive liquid photonic crystal, the other contents are the same as those of Example 8, except that in step S2, the mixed liquid is ultrasonically uniformly dispersed in 199 μL of propylene carbonate solution, so as to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 20%, and its structural color is green.

[0091] Embodiment 15

[0092] A two-component electrically responsive liquid photonic crystal, the other contents are the same as those of Example 8, except that in step S2, the mixed liquid is ultrasonically uniformly dispersed in 116 μL of propylene carbonate solution, so as to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 30%, and its structural color is blue.

[0093] Example 16

[0094] A two-component electrically responsive liquid photonic crystal, the other contents are the same as those of Example 8, except that in step S2, the mixed liquid is ultrasonically evenly dispersed in 75 μL of propylene carbonate solution, so as to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 40%, and its structural color is blue.

[0095] Embodiment 17

[0096] A two-component electrically responsive liquid photonic crystal, the other contents are the same as those of Example 8, except that in step S2, the mixed liquid is ultrasonically uniformly dispersed in 50 μL of propylene carbonate solution, so as to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 50%, and its structural color is blue.

[0097] Embodiment 18

[0098] A two-component electrically responsive liquid photonic crystal, the other contents are the same as those of Example 8, except that in step S2, the mixed liquid is ultrasonically evenly dispersed in 33 μL of propylene carbonate solution, so as to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 60%, and its structural color is blue.

[0099] Embodiment 19

[0100] A two-component electrically responsive liquid photonic crystal comprises Cu2O particles coordinated with tannic acid, CeO2 particles coordinated with tannic acid, and a propylene carbonate solution; the average particle size of the CeO2 particles is 120 nm, the average particle size of the Cu2O particles is 120 nm, the solid content of the two-component electrically responsive liquid photonic crystal is 25%, and the mass ratio of the CeO2 particles to the Cu2O particles is 7:3.

[0101] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0102] S1. The Cu2O particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, and the CeO2 particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Cu2O particles and the CeO2 particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain the coordinated complexed Cu2O particles with polyhydroxy compounds and the coordinated complexed CeO2 particles with polyhydroxy compounds;

[0103] S2. Take 60 mg of a mixture of Cu2O particles with coordinated complexes containing polyhydroxy compounds and CeO2 particles with coordinated complexes containing polyhydroxy compounds, wherein the mass ratio of CeO2 particles to Cu2O particles is 7:3, disperse the above mixture in a 150 mg / mL tannic acid propylene carbonate solution, ultrasonically disperse it uniformly, wash it by centrifugation with the propylene carbonate solution for 1 to 2 times, and then ultrasonically disperse it uniformly in 149 μL propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 25%, and its structural color is green.

[0104] Embodiment 20

[0105] A two-component electrically responsive liquid photonic crystal comprises Fe3O4 particles coordinated and complexed with tannic acid, ZnS particles coordinated and complexed with tannic acid, and a propylene carbonate solution; the average particle size of the ZnS particles is 100 nm, the average particle size of the Fe3O4 particles is 100 nm, the solid content of the two-component electrically responsive liquid photonic crystal is 20%, and the mass ratio of the ZnS particles to the Fe3O4 particles is 7:3.

[0106] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0107] S1. The Fe3O4 particles are dispersed in a 60 mg / ml tannic acid propylene carbonate solution, and the ZnS particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Fe3O4 particles and the ZnS particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain Fe3O4 particles with a coordination complex having a polyhydroxy compound and ZnS particles with a coordination complex having a polyhydroxy compound;

[0108] S2. Take 60 mg of a mixture of Fe3O4 particles coordinated with polyhydroxy compounds and ZnS particles coordinated with polyhydroxy compounds, wherein the mass ratio of ZnS particles to Fe3O4 particles is 7:3, disperse the above mixture in a 150 mg / mL tannic acid propylene carbonate solution, ultrasonically disperse it evenly, wash it by centrifugation with the propylene carbonate solution for 1 to 2 times, and then ultrasonically disperse it evenly in 199 μL of propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 20%, and its structural color is green.

[0109] Embodiment 21

[0110] A two-component electrically responsive liquid photonic crystal comprises Cu2O particles coordinated with tannic acid, ZnS particles coordinated with tannic acid, and a propylene carbonate solution; the average particle size of the ZnS particles is 120 nm, the average particle size of the Cu2O particles is 120 nm, the solid content of the two-component electrically responsive liquid photonic crystal is 25%, and the mass ratio of the ZnS particles to the Cu2O particles is 7:3.

[0111] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0112] S1. The Cu2O particles are dispersed in a 60 mg / ml tannic acid propylene carbonate solution, and the ZnS particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Cu2O particles and the ZnS particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain the coordinated complexed Cu2O particles with polyhydroxy compounds and the coordinated complexed ZnS particles with polyhydroxy compounds;

[0113] S2. Take 60 mg of a mixture of Cu2O particles with coordinated complexes containing polyhydroxy compounds and ZnS particles with coordinated complexes containing polyhydroxy compounds, wherein the mass ratio of ZnS particles to Cu2O particles is 7:3, disperse the above mixture in a 150 mg / mL tannic acid propylene carbonate solution, ultrasonically disperse it evenly, wash it by centrifugation with the propylene carbonate solution for 1 to 2 times, and then ultrasonically disperse it evenly in 149 μL of propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 25%, and its structural color is green.

[0114] Embodiment 22

[0115] A two-component electrically responsive liquid photonic crystal comprises Fe3O4 particles coordinated with tannic acid, ZnS particles coordinated with tannic acid, and a propylene carbonate solution; the average particle size of the ZnS particles is 115 nm, the average particle size of the Fe3O4 particles is 115 nm, the solid content of the two-component electrically responsive liquid photonic crystal is 15%, and the mass ratio of the ZnS particles to the Fe3O4 particles is 1:1.

[0116] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0117] S1. The Fe3O4 particles are dispersed in a 60 mg / ml tannic acid propylene carbonate solution, and the ZnS particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Fe3O4 particles and the ZnS particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain Fe3O4 particles with a coordination complex having a polyhydroxy compound and ZnS particles with a coordination complex having a polyhydroxy compound;

[0118] S2. Take 60 mg of a mixture of Fe3O4 particles coordinated with polyhydroxy compounds and ZnS particles coordinated with polyhydroxy compounds, wherein the mass ratio of ZnS particles to Fe3O4 particles is 1:1, disperse the above mixture in a 150 mg / mL tannic acid propylene carbonate solution, ultrasonically disperse it evenly, wash it by centrifugation with the propylene carbonate solution for 1 to 2 times, and then ultrasonically disperse it evenly in 282 μL of propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 15%, and its structural color is red.

[0119] Embodiment 23

[0120] A two-component electrically responsive liquid photonic crystal comprises Fe3O4 particles coordinated and complexed with tannic acid, SiO2 particles adsorbed with tannic acid, and propylene carbonate solution; the average particle size of the SiO2 particles is 100 nm, the average particle size of the Fe3O4 particles is 100 nm, the solid content of the two-component electrically responsive liquid photonic crystal is 15%, and the mass ratio of the SiO2 particles to the Fe3O4 particles is 3:7.

[0121] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0122] S1. The Fe3O4 particles are dispersed in a 60 mg / ml tannic acid propylene carbonate solution, and the SiO2 particles are dispersed in a 300 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Fe3O4 particles and the SiO2 particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain Fe3O4 particles with coordinated complexation and polyhydroxy compounds and SiO2 particles adsorbed with polyhydroxy compounds;

[0123] S2. Take 60 mg of a mixture of Fe3O4 particles with coordinated complexation and SiO2 particles with adsorbed polyhydroxy compounds, wherein the mass ratio of SiO2 particles to Fe3O4 particles is 3:7, disperse the above mixture in 300 mg / mL tannic acid propylene carbonate solution, ultrasonically disperse it evenly, wash it by centrifugation with the propylene carbonate solution for 1 to 2 times, and then ultrasonically disperse it evenly in 282 μL of propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 15%, and its structural color is red.

[0124] Embodiment 24

[0125] A multi-component electrically responsive liquid photonic crystal comprises Fe3O4 particles coordinated with tannic acid, ZnS particles coordinated with tannic acid, CeO2 particles coordinated with tannic acid, and propylene carbonate solution; the average particle size of the ZnS particles is 100 nm, the average particle size of the Fe3O4 particles is 100 nm, the average particle size of the CeO2 particles is 100 nm, the solid content of the multi-component electrically responsive liquid photonic crystal is 20%, and the mass ratio of the Fe3O4 particles, the ZnS particles, and the CeO2 particles is 1:1:1.

[0126] The preparation method of the above two-component electrically responsive liquid photonic crystal comprises the following steps:

[0127] S1. The Fe3O4 particles are dispersed in a 60 mg / ml tannic acid propylene carbonate solution, and the ZnS and CeO2 particles are dispersed in a 200 mg / ml tannic acid propylene carbonate solution, so that the mass concentration of the Fe3O4 particles, ZnS and CeO2 particles in the tannic acid propylene carbonate solution is 60 mg / ml, and after ultrasonic homogenization, the propylene carbonate solution is centrifuged and washed 1-2 times, and then dispersed in the propylene carbonate solution for subsequent use to obtain Fe3O4 particles with a coordination complex having a polyhydroxy compound and ZnS and CeO2 particles with a coordination complex having a polyhydroxy compound;

[0128] S2. Take 60 mg of a mixture of Fe3O4 particles coordinated with polyhydroxy compounds and ZnS and CeO2 particles coordinated with polyhydroxy compounds, wherein the mass ratio of CeO2 particles, ZnS particles and Fe3O4 particles is 1:1:1, disperse the above mixture in a 150 mg / mL tannic acid propylene carbonate solution, ultrasonically disperse it evenly, wash it by centrifugation with the propylene carbonate solution for 1 to 2 times, and then ultrasonically disperse it evenly in 222 μL of propylene carbonate solution to obtain a two-component electrically responsive liquid photonic crystal with a solid content of 25%, and its structural color is green.

[0129] Comparative Example 1-2

[0130] An electrically responsive liquid photonic crystal, the other contents of which are the same as those of Example 1, except that the mass ratios of CeO2 particles to Fe3O4 particles are 10:0 and 0:10 respectively.

[0131] Comparative Examples 3-4

[0132] An electrically responsive liquid photonic crystal, the other contents of which are the same as those of Example 18, except that the mass ratios of CeO2 particles to Cu2O particles are 10:0 and 0:10 respectively.

[0133] Comparative Examples 5-6

[0134] An electrically responsive liquid photonic crystal, the other contents of which are the same as those of Example 20, except that the mass ratios of ZnS particles to Fe3O4 particles are 10:0 and 0:10 respectively.

[0135] Comparative Examples 7-8

[0136] An electrically responsive liquid photonic crystal, the other contents of which are the same as those of Example 21, except that the mass ratios of ZnS particles to Cu2O particles are 10:0 and 0:10 respectively.

[0137] Comparative Examples 9-10

[0138] An electrically responsive liquid photonic crystal, the other contents of which are the same as those of Example 22, except that the mass ratios of ZnS particles to Fe3O4 particles are 10:0 and 0:10 respectively.

[0139] Test and Evaluation

[0140] The electrically responsive liquid photonic crystals obtained in the embodiment and the comparative example were respectively encapsulated between two transparent ITO conductive glasses with a substrate spacing of 100 um, and a 1.2 V DC voltage was applied thereto to determine the structural color regulation status.

[0141] Figure 1 The maximum reflectance bar graph of dry powders with different particle sizes.

[0142] Figure 2 The field emission scanning electron microscope images of the two-component particles before and after mixing in Example 1 show that the electrically responsive liquid photonic crystal prepared by the solution of the present application does not show any agglomeration phenomenon.

[0143] The digital photographs of the electrically responsive liquid photonic crystals prepared in Example 1-5 without applying an electric field are shown in FIG. Figure 3 As shown, the entire device displays a uniform green structural color, from which it can be inferred that there is no agglomeration in the entire system.

[0144] Examples 1-5 show the reflectivity and brightness of the electrically responsive liquid photonic crystals prepared in different proportions. Figure 4 , Figure 5 As shown in the figure, as the proportion of CeO2 in the system increases, its brightness gradually increases, but its saturation gradually decreases. After applying a forward voltage of 1.2V, the negative electrode changes from green structural color to yellow, and its overall structural color is uniform, and no stratification occurs during the color change process. The relationship between reflectivity and brightness changes with the proportion trend as shown in the figure Figure 4 , Figure 5 shown.

[0145] Digital photos of the single-component electrically responsive photonic crystals prepared in Examples 1 and 2 and the two-component electrically responsive photonic crystals in Example 2 without applying an electric field are shown in FIG. Figure 6 As shown, Figure 7 (Reflectivity spectra of the single-component electro-responsive photonic crystals of Comparative Examples 1 and 2 and the dual-component electro-responsive photonic crystals of Example 2 before and after the application of an electric field), Figure 8 (Brightness relationship diagram of the single-component electro-responsive photonic crystals of Comparative Examples 1 and 2 and the two-component electro-responsive photonic crystals of Example 2 before and after the application of the electric field) It can be seen that although the electro-responsive photonic crystal composed only of CeO2 colloidal particles has a higher reflectivity, its overall baseline will move up, resulting in a widening of its half-width, while the electro-responsive photonic crystal composed only of Fe3O4 colloidal particles has a narrower half-width, but its reflectivity is lower. After mixing them in a certain proportion, the electro-responsive photonic crystal composed of two-component colloidal particles not only has a higher reflectivity and brightness, but also has a narrower half-width.

[0146] In Examples 6-8, Fe3O4 colloidal particles and CeO2 colloidal particles having similar average particle sizes are mixed in a ratio of 1:1. Among them, when the average particle size of both is 85 nm, the structural color of the electrically responsive liquid photonic crystal with a solid content of 20% prepared therefrom presents a uniform blue color; when the average particle size of both is 150 nm, the structural color of the electrically responsive liquid photonic crystal with a solid content of 30% prepared therefrom is yellow; when the average particle size of both is 200 nm, due to its excessively large particle size, its reflectivity peak at a solid content of 30% exceeds the visible light range and is in the infrared position, and the structural color appears reddish brown; for colloidal particles with an average particle size that is too small, a lower solid content is often required to achieve self-assembly and present a structural color, and when the solid content is lower than the specified concentration, the electrostatic repulsion on the particle surface is insufficient to balance the van der Waals force, and it will not be able to self-assemble to form a structural color; for colloidal particles with an average particle size that is too large, a higher solid content is often required to enable them to self-assemble in the system, and when the solid content is too high, uneven dispersion will occur.

[0147] Digital photos of the electrically responsive liquid photonic crystals obtained in Examples 9, 10, and 11 without applying an electric field are shown in FIG. Fig. 9 As shown in Figure 2, the uniform blue, green and yellow structural colors are displayed respectively. The corresponding reflectivity spectra are shown in Figure 2. Fig.10 As shown, it is shown that particles of different sizes can be mixed and self-assembled to form structural colors.

[0148] The digital photos and spectra of the electrically responsive liquid photonic crystals obtained in Examples 12-18 without applying an electric field are shown in FIG. Fig.11 , Fig.12As shown, it can be seen that when the solid content in the system is lower than the specified concentration, the electrostatic repulsion on the particle surface is not sufficient to balance the van der Waals force, and it fails to self-assemble to form structural color, but shows its intrinsic color; and when the solid content in the system is higher than the specified concentration, although it can form structural color, it cannot be completely dispersed due to the excessively high solid content, resulting in uneven dispersion.

[0149] Compare Example 19 with Comparative Examples 3 and 4. Fig.13 (Reflectivity spectra of the single-component electro-responsive photonic crystals of Comparative Examples 3 and 4 and the dual-component electro-responsive photonic crystals of Example 19 before and after application of an electric field), Fig.14 (Brightness relationship diagram of the single-component electrically responsive photonic crystals of Comparative Examples 3 and 4 and the two-component electrically responsive photonic crystals of Example 19 before and after the application of the electric field) It can be seen that for the Cu2O colloidal particles with lower chemical color, when they constitute the electrically responsive photonic crystal alone, they have a narrower half-width at half maximum, but their reflectivity is lower. The two-component electrically responsive photonic crystal formed by mixing them with CeO2 colloidal particles not only has higher reflectivity and brightness, but also has a narrower half-width at half maximum, indicating that the other metal oxides with lower chemical color that can coordinate and complex with tannic acid except Fe3O4 colloidal particles can also use the particle compounding method to achieve brightness and saturation regulation.

[0150] Compare Example 20 with Comparative Examples 5 and 6. Fig.15 (Reflectivity spectra of the single-component electro-responsive photonic crystals of Comparative Examples 5 and 6 and the dual-component electro-responsive photonic crystals of Example 20 before and after application of an electric field), Fig.16 (Brightness relationship diagram of the single-component electro-responsive photonic crystals of Comparative Examples 5 and 6 and the two-component electro-responsive photonic crystals of Example 20 before and after the application of the electric field) It can be seen that for the ZnS colloidal particles with higher chemical color, when they constitute the electro-responsive photonic crystal alone, they have higher brightness and reflectivity, but their overall baseline will move up, resulting in a widening of their half-peak width. The two-component electro-responsive photonic crystal formed by mixing them with Fe3O4 colloidal particles not only has higher reflectivity and brightness, but also has a narrower half-peak width, indicating that the other metal oxides with higher chemical color that can coordinate and complex with tannic acid except CeO2 colloidal particles can also use the particle compounding method to achieve saturation regulation.

[0151] Compare Example 21 with Comparative Examples 7 and 8. Fig.17 (Reflectivity spectra of the single-component electro-responsive photonic crystals of Comparative Examples 7 and 8 and the dual-component electro-responsive photonic crystals of Example 20 before and after the application of an electric field), Fig.18 (Brightness relationship diagram of the single-component electrically responsive photonic crystals of Comparative Examples 7 and 8 and the dual-component electrically responsive photonic crystals of Example 21 before and after application of an electric field) It can be seen that the electrically responsive photonic crystal formed by mixing ZnS and Cu2O in a certain proportion not only has a higher reflectivity and brightness but also has a narrower half-width.

[0152] Compare Example 22 with Comparative Examples 9 and 10. Fig.19 (Reflectivity spectra of the single-component electrically responsive photonic crystals of Comparative Examples 9 and 10 and the two-component electrically responsive photonic crystals of Example 22 after crystallization) It can be seen that the individual ZnS and Fe3O4 colloidal particles and the electrically responsive photonic crystals formed by mixing them in a certain proportion showed crystallization at a mass fraction of 15%, and the two-component electrically responsive photonic crystals mixed in a certain proportion also had higher reflectivity and brightness after crystallization than the single-component electrically responsive photonic crystals, and also had a narrower half-width.

[0153] The spectrum of the multi-component electrically responsive liquid photonic crystal prepared in Example 23 after applying an electric field is as follows: Fig. 20 As shown, it can be seen that the prepared multi-component electrically responsive photonic crystal can achieve a peak position change from red to green under the action of an electric field, indicating that by adsorbing on the surface of SiO2 particles, particles can also be compounded to adjust brightness and saturation.

[0154] The digital photos and spectra of the multi-component electrically responsive liquid photonic crystal prepared in Example 24 before and after the electric field is applied are as follows: Fig.21 , Fig. 22 As shown, it can be seen that the prepared multi-component electrically responsive photonic crystal presents a uniform green structural color as a whole, and when an electric field is applied, the negative electrode changes from a uniform green to a uniform red.

[0155] The present application uses tannic acid to modify multiple different types of particles at the same time, so that their surfaces have similar physical and chemical properties, avoiding the phenomenon of agglomeration during the mixing process, and also avoiding the phenomenon of uneven color due to inconsistent electrophoretic rates of particles caused by different surface charges of different particles under an electric field. In addition, the modification process is simple and has good repeatability and can be carried out at room temperature. Compared with the existing reported electro-responsive photonic crystals, the present invention proposes and realizes the concept of multi-component electro-responsive photonic crystals for the first time, wherein the brightness and saturation of the photonic crystals are controlled by controlling the proportion and particle size of the different components, making it more promising in the field of electrophoretic displays.

[0156] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.

[0157] The above embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A multi-component electrically responsive liquid photonic crystal, characterized in that: It comprises two or more colloidal particles with different chemical color reflectivity; all the colloidal particles have polyhydroxy compounds coordinated, complexed or adsorbed on their surfaces; all the colloidal particles are dispersed in a polar solvent; and the different colloidal particles are used to continuously regulate the brightness and saturation of the electrically responsive photonic crystal.

2. The multi-component electrically responsive liquid photonic crystal according to claim 1, characterized in that: The average particle size of the colloidal particles is 80-300 nm.

3. The multi-component electrically responsive liquid photonic crystal according to claim 1, characterized in that: The solid content is 5-80wt%.

4. The multi-component electrically responsive liquid photonic crystal according to claim 1, characterized in that: The colloidal particles can be selected from colloidal particles having at least one of iron, copper, molybdenum, vanadium, manganese, cobalt, chromium, ruthenium, nickel, terbium, rhodium, tungsten, cerium, aluminum, zinc, cadmium, europium, gadolinium, and zirconium ions on the surface or in the colloidal particles, as well as SiO2 and polystyrene colloidal particles.

5. A method for preparing a multi-component electrically responsive liquid photonic crystal according to any one of claims 1 to 4, characterized in that: Here are the steps: S1. using a polar solution containing a polyhydroxy compound to coordinate, complex or adsorb two or more colloidal particles with different chemical color reflectances once or multiple times, washing away the free polyhydroxy compound in the system after the reaction, separating and retaining the solid product, and obtaining a mixture of two or more colloidal particles with different chemical color reflectances that are coordinated, complexed or adsorbed with polyhydroxy compounds; S2. Disperse the mixture of two or more colloidal particles with different chemical color reflectivity that are coordinated, complexed or adsorbed with polyhydroxy compounds in a polar solution to form a colloidal particle dispersion system with a certain concentration, thereby obtaining the multi-component electrically responsive liquid photonic crystal.

6. An electrically responsive photonic crystal device, characterized in that: The multi-component electrically responsive liquid photonic crystal obtained by the preparation method of claim 5 is sealed between transparent conductive electrode plates, and the concentration of the polyhydroxy compound contained in the polar solution is greater than or equal to 0.1 mg / mL.

7. The electrically responsive photonic crystal device according to claim 6, characterized in that: The conductive electrode plate comprises one or more of a high-purity silver sheet, a high-purity copper sheet, a transparent ITO conductive glass, a FTO conductive glass, and an ITO-PET flexible conductive film, and the spacing between two conductive electrode plates is 10-1000 μm.

8. Use of the electrically responsive photonic crystal device as claimed in claim 7 in color control of an electrophoretic display.