Metal nanocone plasmon resonant cavity, preparation method and application thereof

By forming a metal nanoconical tube plasmon resonance cavity with a large aspect ratio in the nano-scale hollow metal conical tube array structure, the problem of low light absorption in the near-infrared band in the prior art is solved, and efficient light absorption is achieved Effect.

CN118584569BActive Publication Date: 2024-11-01INST OF MODERN PHYSICS CHINESE ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410981259.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-01
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The light absorption rate of existing metal nanoconical tubes in the near-infrared band is low, and they cannot effectively utilize the absorption characteristics of the metal itself, resulting in insufficient absorption efficiency.

Method used

Using a nanoscale hollow metal conical tube array structure, including irregular hollow metal conical tubes and conical pit structures, metal nanoconical tubes with large aspect ratios are formed by high-energy heavy ion beam irradiation and template preparation method. The elemental resonance cavity is combined with coating technology to deposit a metal layer to form a metal nanoconical tube plasmon resonance cavity.

Benefits of technology

The light absorption rate is significantly improved, especially in the 300 nm-2300 nm band, which reaches more than 99.5%, reduces Fresnel scattering at the interface, supports more plasmon resonance modes, and achieves wide-angle high-efficiency light absorption. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118584569B_ABST
    Figure CN118584569B_ABST
Patent Text Reader

Abstract

The present application relates to a metal nano-cone tube plasmon resonance cavity, a preparation method and its application, wherein the metal nano-cone tube plasmon resonance cavity includes a nanoscale hollow metal cone tube array structure, the hollow metal cone tube array structure includes irregular hollow metal cone tubes and irregular conical pit structures formed between the hollow metal cone tubes, the aspect ratio of the hollow metal cone tube is greater than 20, and the thinnest tube wall of the hollow metal cone tube is less than or equal to 10 nm. The present application mainly relies on plasmon resonance to achieve strong absorption of incident light. Compared with columnar nanotubes, the cross-sectional diameter of the conical nanotube gradually increases from top to bottom, which can support more plasmon resonance modes, making the absorption rate higher and the absorption band wider; the large aspect ratio of the cone tube array makes the effective refractive index change gradually from top to bottom, reducing Fresnel scattering at the interface, promoting the absorption of incident light, and facilitating wide-angle absorption; the cone tube structure is adjustable, the tube wall is smooth, and it can be prepared on a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of nanophotonics, and in particular to a metal nanocone plasmon resonant cavity, a preparation method and applications thereof. Background Art

[0002] Under the action of incident light, metal nanostructures will cause collective oscillation of free electrons, forming surface plasmons, which will strongly absorb the incident light.

[0003] However, currently in the near-infrared band, the absorption rate is low due to the limited absorption of the metal itself by the metal nanocone tube. Summary of the invention

[0004] To solve the above problems, the present application provides a metal nanocone plasmon resonant cavity, a preparation method and an application thereof, so as to overcome or at least partially overcome the deficiencies of the prior art.

[0005] In a first aspect, the present application provides a metal nano-cone tube plasmon resonant cavity, wherein the metal nano-cone tube plasmon resonant cavity comprises a nanoscale hollow metal cone tube array structure, wherein the hollow metal cone tube array structure comprises irregular hollow metal cone tubes and irregular conical pit structures formed between the hollow metal cone tubes;

[0006] Wherein, the aspect ratio of the hollow metal conical tube is greater than 20, and the thinnest tube wall of the hollow metal conical tube is less than or equal to 10 nm.

[0007] Optionally, in the above-mentioned metal nanocone tube plasmon resonant cavity, the material of the hollow metal cone tube is selected from one or more alloys formed by gold, silver, copper, aluminum, palladium, cobalt, chromium, iron, indium, molybdenum, niobium, nickel, lead, platinum, tin, tantalum, vanadium, tungsten, zinc, manganese, antimony, bismuth and germanium, or selected from SiO 2 、Al 2 O 3 , HfO 2 , TiN, AlN and TaN.

[0008] Optionally, in the above-mentioned metal nanocone tube plasmon resonant cavity, when the material of the hollow metal cone tube is palladium, the absorption rate of the metal nanocone tube plasmon resonant cavity to light in the band of 300 nm-2300 nm is greater than 99.5%.

[0009] In a second aspect, the present application also provides a method for preparing the above-mentioned metal nanocone tube plasmon resonant cavity, comprising:

[0010] The template preparation step comprises: irradiating a polymer substrate with a high-energy heavy ion beam to cause track damage on the surface of the polymer substrate; and placing the irradiated polymer substrate in a first etching solution for etching to form irregular polymer cones and cone holes between the irregular polymer cones to obtain an ion track template;

[0011] Metal deposition step: depositing a metal layer on the surface of the ion track template by using a coating technology to form a metal substrate;

[0012] Template dissolving step: using a second etching solution to dissolve the ion track template to obtain a metal nanocone plasmon resonant cavity.

[0013] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, before the template dissolving step, the method further comprises:

[0014] Support enhancement step: adding a support layer on the surface of the metal substrate, wherein the support layer is a polymer support layer or a metal support layer.

[0015] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, in the template preparation step, the polymer substrate is selected from one of polyethylene terephthalate, polyimide and polycarbonate;

[0016] The thickness of the polymer substrate is greater than 50 μm.

[0017] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, in the template preparation step, if the polymer substrate is polyethylene terephthalate or polycarbonate, the first etching solution is a first mixed solution of a first sodium hydroxide aqueous solution and methanol in any proportion, wherein the concentration of the first sodium hydroxide aqueous solution is 2.5-9 mol / L, and the methanol is of analytical grade;

[0018] If the polymer substrate is polyimide, the first etching solution is a second mixed solution of a second sodium hydroxide aqueous solution and sodium hypochlorite in any ratio, wherein the concentration of the second sodium hydroxide aqueous solution is 2.5-9 mol / L, and the sodium hypochlorite is of analytical grade.

[0019] Optionally, in the above-mentioned method for preparing the metal nanocone plasmon resonant cavity, the concentration of the first sodium hydroxide aqueous solution is 9 mol / L, and the mass content of methanol in the first mixed liquid is 95%; the concentration of the second sodium hydroxide aqueous solution is 5 mol / L, and the mass content of sodium hypochlorite in the second mixed liquid is 90%.

[0020] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, the high-energy heavy ions are selected from 86 Kr, 129 Xe, 183 Ta and 209 At least one of Bi; and the ion energy of the high-energy heavy ions is greater than 1500 MeV.

[0021] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, the irradiation dose of the high-energy heavy ions is 1×10 7 ions / cm 2 -1×10 9 ions / cm 2 .

[0022] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, the irradiation dose of the high-energy heavy ions is 1×10 7 ions / cm 2 , 2×10 7 ions / cm 2 , 3×10 7 ions / cm 2 , 4×10 7 ions / cm 2 , 5×10 7 ions / cm 2 , 6×10 7 ions / cm 2 ,7×10 7 ions / cm 2 , 8×10 7 ions / cm 2 ,9×10 7 ions / cm 2 , 1×10 8 ions / cm 2 , 2×10 8 ions / cm 2 , 3×10 8 ions / cm 2 , 4×10 8 ions / cm 2 , 5×10 8 ions / cm 2 , 6×10 8 ions / cm 2 ,7×10 8 ions / cm 2 , 8×10 8 ions / cm 2 ,9×108 ions / cm 2 and 1×10 9 ions / cm 2 Any one of .

[0023] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, the irradiation injection is 2×10 8 ions / cm 2 .

[0024] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, in the template preparation step, the etching is performed in a water bath heating environment, the water bath temperature is 25° C.-70° C., and the etching time is 1 h-10 h.

[0025] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, in the metal deposition step, the coating technology is magnetron sputtering or evaporation.

[0026] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, the coating technology is magnetron sputtering.

[0027] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, in the metal deposition step, the material of the metal layer is selected from one or more alloys formed by gold, silver, copper, aluminum, palladium, cobalt, chromium, iron, indium, molybdenum, niobium, nickel, lead, platinum, tin, tantalum, vanadium, tungsten, zinc, manganese, antimony, bismuth and germanium, or selected from SiO 2 、Al 2 O 3 , HfO 2 , TiN, AlN and TaN.

[0028] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, in the template dissolving step, if the polymer substrate is polyethylene terephthalate or polycarbonate, the second etching solution is a third mixed solution of a third sodium hydroxide aqueous solution and methanol in any proportion, wherein the concentration of the third sodium hydroxide aqueous solution is 2.5-9 mol / L, and the methanol is of analytical grade;

[0029] If the polymer substrate is polyimide, the second etching solution is a fourth mixed solution of a fourth sodium hydroxide aqueous solution and sodium hypochlorite in any ratio, wherein the concentration of the fourth sodium hydroxide aqueous solution is 2.5-9 mol / L, and the sodium hypochlorite is of analytical grade;

[0030] The mass content of the third aqueous sodium hydroxide solution in the third mixed solution is greater than 50%; the mass content of the fourth aqueous sodium hydroxide solution in the fourth mixed solution is greater than 50%.

[0031] Optionally, in the above-mentioned method for preparing the metal nanocone tube plasmon resonant cavity, in the template dissolution step, the template dissolution step is carried out in a water bath environment, the water bath temperature is 50° C.-70° C., and the dissolution time is 5h-10h.

[0032] In the third aspect, the present application also provides an application of any of the above-mentioned metal nanocone tube plasmon resonance cavities or a metal nanocone tube plasmon resonance cavity prepared by any of the above-mentioned preparation methods of the metal nanocone tube plasmon resonance cavity in photocatalysis, sensing technology and detection technology.

[0033] At least one of the above technical solutions adopted in this application can achieve the following beneficial effects:

[0034] The present invention provides a metal nano-cone tube plasmon resonance cavity, which includes a nano-scale hollow metal cone tube array structure, wherein the hollow metal cone tube array structure includes irregular hollow metal cone tubes and irregular conical pit structures formed between the hollow metal cone tubes. Compared with a solid structure, the metal nano-cone tube plasmon resonance cavity of the present application forms a plasmon resonance cavity inside the nano-cone tube, which mainly relies on plasmon resonance to achieve strong absorption of incident light in addition to the electron transition absorption of the material itself; compared with columnar nanotubes, the cross-sectional diameter of the conical nanotube gradually increases from top to bottom, which can support more plasmon resonance modes, making the absorption rate higher and the absorption band wider; the large aspect ratio of the cone tube array makes the effective refractive index change gradually from top to bottom, reducing Fresnel scattering at the interface, further promoting the absorption of incident light, and facilitating wide-angle absorption; the cone tube structure is adjustable, the tube wall is smooth, and can be prepared on a large scale; and the metal nano-cone tube plasmon resonance cavity is widely used and highly practical. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0036] Figure 1 A schematic diagram of the structure of a metal nanocone tube plasmon resonant cavity according to an embodiment of the present application is shown;

[0037] Figure 2 shows a scanning electron microscope image of an ion track template prepared according to Example 1 of the present application;

[0038] Figure 3is a schematic diagram showing a nanocone tube formation process according to an embodiment of the present application;

[0039] Figure 4 A scanning electron microscope image of a "match head" structure formed by sputtering metal on a polymer substrate prepared according to Example 1 of the present application is shown;

[0040] Figure 5 The structure of the metal nanocone tube plasmon resonant cavity prepared according to Example 1 of the present application under a scanning electron microscope is shown. Figure 1 ;

[0041] Figure 6 The structure of the metal nanocone tube plasmon resonant cavity prepared according to Example 1 of the present application under a scanning electron microscope is shown. Figure 2 ;

[0042] Figure 7 The structure of the metal nanocone tube plasmon resonant cavity prepared according to Example 1 of the present application under a scanning electron microscope is shown. Figure 3 ;

[0043] Figure 8 The absorption spectra of the metal nanocone plasmon resonant cavity array according to the present application are shown when the incident light is at 0°, 30°, and 50° to the film normal direction. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present application clearer, the technical solution of the present application will be clearly and completely described below in combination with the specific embodiments of the present application and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0045] Metal nanostructures will cause collective oscillation of free electrons under the action of incident light, forming surface plasmons, which strongly absorb the incident light. The present application has found through research that the incident light is reflected on the side walls of the large aspect ratio conical structure. Taking vertical incidence as an example, due to the large aspect ratio, the angle between these side walls and the incident light is very small, and the reflected light is located below the air-substrate interface. Most of the incident light is trapped in these conical structure areas. The plasmon resonant cavity formed by the hollow metal nanostructure can support more resonance modes than the solid structure. Therefore, the large aspect ratio metal nanoconical tube array is an ideal light absorber in the visible-near infrared band. In addition, this structure has the characteristics of high specific surface area, low density, high porosity, etc., and has potential application value in photocatalysis, highly sensitive gas sensing, energy storage, surface enhanced Raman scattering, etc. Based on this, the present application provides a metal nanocone tube plasmon resonant cavity, which includes a nanoscale hollow metal cone tube array structure, and the hollow metal cone tube array structure includes irregular hollow metal cone tubes and irregular conical pit structures formed between the hollow metal cone tubes.

[0046] The schematic structure is as follows Figure 1 As shown in the figure, there is an irregular conical pit structure rather than a planar structure between each conical nanotube. Compared with a solid structure, a plasmon resonance cavity is formed inside the nanoconical tube. In addition to the electron transition absorption of the material itself, it mainly relies on plasmon resonance to achieve strong absorption of incident light. Compared with columnar nanotubes, the cross-sectional diameter of the conical nanotube gradually increases from top to bottom, which can support more plasmon resonance modes, making the absorption rate higher and the absorption band wider. In addition, the effective refractive index of the large aspect ratio conical tube array changes gradually from top to bottom, which reduces Fresnel scattering at the interface, further promotes the absorption of incident light, and contributes to wide-angle absorption.

[0047] In some embodiments, the aspect ratio of the metal conical nanotubes is preferably greater than 20, and the thinnest tube wall is preferably less than or equal to 10 nm, which is more conducive to improving the absorption rate.

[0048] In some embodiments, the material of the hollow metal cone tube can be gold, silver, copper, aluminum, palladium, cobalt, chromium, iron, indium, molybdenum, niobium, nickel, lead, platinum, tin, tantalum, vanadium, tungsten, zinc, manganese, antimony, bismuth, germanium, etc., or nickel-chromium, nickel-iron, titanium-aluminum, etc. In other embodiments, the material of the hollow metal cone tube can also refer to SiO 2 、Al 2 O 3 , HfO 2 , TiN, AlN and TaN and other oxides or nitrides.

[0049] In some embodiments, when the material of the hollow metal cone tube is palladium, the absorption rate of the metal nanocone tube plasmon resonant cavity to light in the wavelength band of 300 nm-2300 nm is greater than 99.5%.

[0050] The present application also provides a method for preparing a metal nanocone plasmon resonant cavity, the method comprising steps S110 to S130:

[0051] Template preparation step S110: using a high-energy heavy ion beam to irradiate a polymer substrate to cause track damage on the surface of the polymer substrate; and placing the irradiated polymer substrate into a first etching solution for etching to form irregular polymer cones and cone holes between the irregular polymer cones, thereby obtaining an ion track template.

[0052] In the near-infrared band, due to the limited absorption of infrared light by metal itself, the absorption rate of light by the nano-cone tube plasmon resonant cavity prepared by metal in the prior art is generally not high. In view of this situation, the present application uses a template method to prepare a metal nano-cone tube plasmon resonant cavity, which has a metal nano-cone tube array with a large aspect ratio and is an ideal light absorber in the visible-near infrared band.

[0053] First, the ion track template is prepared. The polymer substrate is irradiated with a heavy ion beam to break the chemical bonds on the ion path, resulting in a potential track damage area. The polymer substrate is etched with a special etching solution, and the etching rate V along the track direction is t Much larger than the bulk etch rate V b , forming a tapered hole with a large aspect ratio, where the body etching rate V b It can be understood as the average rate of etching in all directions in the body of the polymer substrate. In some embodiments, it can be characterized by the rate of decrease of the thickness of the polymer substrate before and after etching, that is, the ratio of the difference in thickness or average thickness of the polymer substrate before and after etching to the etching time. As the etching time increases, the bottoms of the cone holes overlap, and the platform area between the cone holes gradually decreases, eventually forming an irregular polymer cone structure. The complex micro-nano structure finally formed is composed of two types of structural units: cone holes with a large aspect ratio and irregular polymer cones. The cone holes with a large aspect ratio are the basis of the conical pit structure. The polymer substrate with a micro-nano structure obtained after etching is the ion track template. For details, please refer to Figure 2 , Figure 2 The microstructure on the ion track template shown has many irregular polymer cones, and there are cone holes between the irregular polymer cones.

[0054] In some embodiments, in the template preparation step, the polymer substrate is preferably selected from one of polyethylene terephthalate, polyimide and polycarbonate; and the thickness of the polymer substrate is preferably greater than 50 μm.

[0055] In some embodiments, the high energy heavy ions are selected from 86 Kr, 129 Xe, 183 Ta and 209 Bi; and the ion energy of the high-energy heavy ions is preferably greater than 1500 MeV. It should be noted that the large V t / V b The value is helpful to form a conical hole with a large aspect ratio, corresponding to a nano-conical tube with a large aspect ratio. In some embodiments, the ion energy is preferably greater than 1500 MeV. If the energy is too small, it is not conducive to the subsequent coating to form a conical tube structure with a large aspect ratio. For example, the damage caused by neon or oxygen ions with an energy of 200-300 MeV in the polymer substrate is relatively limited, and the conical holes formed by subsequent etching are of different sizes and have a small aspect ratio, which is not conducive to the subsequent coating to form a conical tube structure with a large aspect ratio.

[0056] In some embodiments, the high energy heavy ion irradiation dose is preferably 1×10 7 ions / cm 2 -1×10 9 ions / cm 2 If the injection amount is too small, the size of the micro-nano structure of the ion track template finally etched is too large, the shadow effect during subsequent coating is not significant, it is difficult to form a "match head" structure at the tip of the irregular polymer cone, and the opening at the bottom of the cone hole structure cannot be closed. Continuous deposition will form a solid cone structure; if the injection amount is too large, the size of the micro-nano structure of the ion track template finally etched is too small, the opening at the bottom of the cone hole structure is closed prematurely during the subsequent coating process, the wall of the nanoconical tube is too thin and not completely continuous, and after the ion track template is dissolved, the cone tube cannot support itself.

[0057] In some embodiments, the irradiation dose of the high energy heavy ions is preferably 1×10 7 ions / cm 2 , 2×10 7 ions / cm 2 , 3×10 7 ions / cm 2 , 4×10 7 ions / cm 2 , 5×10 7 ions / cm 2 , 6×10 7 ions / cm 2 ,7×10 7ions / cm 2 , 8×10 7 ions / cm 2 ,9×10 7 ions / cm 2 , 1×10 8 ions / cm 2 , 2×10 8 ions / cm 2 , 3×10 8 ions / cm 2 , 4×10 8 ions / cm 2 , 5×10 8 ions / cm 2 , 6×10 8 ions / cm 2 ,7×10 8 ions / cm 2 , 8×10 8 ions / cm 2 ,9×10 8 ions / cm 2 and 1×10 9 ions / cm 2 Any one of .

[0058] In some embodiments, the irradiation fluence is more preferably 2×10 8 ions / cm 2 .

[0059] In some embodiments, in step S110, for different polymer substrates, the composition and ratio of the etching solution are also different. For PC and PET, the first etching solution is preferably a mixture of sodium hydroxide (NaOH) aqueous solution and methanol, the sodium hydroxide (NaOH) aqueous solution is recorded as the first sodium hydroxide aqueous solution, and the mixed solution is recorded as the first mixed solution, wherein the concentration of the first sodium hydroxide aqueous solution is preferably 2.5-9 mol / L, and methanol can be commercially available from any manufacturer of analytical grade, and the first sodium hydroxide aqueous solution and methanol can be mixed in any proportion, wherein the content of one of the first sodium hydroxide aqueous solution and methanol can be zero, preferably not zero; more preferably, a first mixed solution of 9 mol / L NaOH aqueous solution and analytical grade methanol is used, wherein the mass content of methanol in the first mixed solution is preferably 95%; for PI, the first etching solution is preferably a mixture of sodium hydroxide (NaOH) aqueous solution and sodium hypochlorite, the sodium hydroxide (NaOH) aqueous solution is recorded as the second sodium hydroxide aqueous solution, and the mixed solution is recorded as the second mixed solution, wherein the concentration of the second sodium hydroxide aqueous solution is preferably 2.5-9 mol / L Sodium hypochlorite (NaClO) of analytical grade from any commercial manufacturer can be used. The second sodium hydroxide aqueous solution and sodium hypochlorite can be mixed in any proportion, wherein the content of one of the second sodium hydroxide aqueous solution and sodium hypochlorite can be zero, preferably not zero; more preferably, a second mixed solution of 5 mol / L NaOH aqueous solution and analytically pure NaClO can be used, wherein the mass content of NaClO in the second mixed solution is 90%.

[0060] In some embodiments, in step S110, etching is performed in a water bath heating environment, the etching temperature is between 25°C and 70°C, the etching time can be determined according to the etching solution ratio and the etching temperature, and the etching time is preferably between 1h and 10h.

[0061] Metal deposition step S120: depositing a metal layer on the surface of the ion track template using a coating technology to form a metal substrate.

[0062] The metal nanocone plasmon resonant cavity is prepared on the basis of the ion track template. This step is the core of the present application. A layer of metal is deposited on the surface of the ion track template by using a coating technology to form a metal substrate.

[0063] The following is a brief description of the coating process, please refer to Figure 3 , Figure 3The left figure in FIG. 1 shows two irregular polymer cones, and a cone hole is formed between the two irregular polymer cones, that is, the cone hole of the micro-nano structure on the ion track template implemented in step S110, which has a very large aspect ratio. Due to the shadow effect of the coating method such as magnetron sputtering, the thickness of the metal layer deposited on the side wall of the structure is distributed in a gradient from top to bottom. As the sputtering time increases, the tip of the irregular polymer cone forms a "match head" structure (such as Figure 3 The left picture and Figure 4 As shown in the figure, each match head structure adheres to each other, and after adhesion, multiple match heads form a "closed surface", which is the metal substrate. The metal substrate prevents the metal from continuing to deposit into the cone hole. At this time, a metal nanocone tube with a large aspect ratio has been formed in the cone hole (please refer to Figure 3 At this point, you can stop sputtering, but the metal substrate formed at this point is relatively "thin". If you want to achieve self-support, you usually need to add a support layer. If you want a thicker metal substrate, continue sputtering deposition until a dense metal substrate is formed, and then stop sputtering. This kind of metal substrate can achieve self-support, and usually no support layer is needed.

[0064] In some embodiments of the present application, in the metal deposition step, the coating technology is preferably a magnetron sputtering method or an evaporation method, preferably a magnetron sputtering method.

[0065] The coating method may be magnetron sputtering or evaporation with a shadow effect, preferably magnetron sputtering. It should be noted that highly conformal methods such as atomic layer deposition and electroless chemical deposition are not recommended for use in this application.

[0066] In the present application, the material of the metal nanocone tube can be gold, silver, copper, aluminum, palladium, cobalt, chromium, iron, indium, molybdenum, niobium, nickel, lead, platinum, tin, tantalum, vanadium, tungsten, zinc, manganese, antimony, bismuth, germanium, etc., or nickel-chromium, nickel-iron, titanium-aluminum, etc. In some embodiments, the metal nanocone tube exciton resonant cavity and its preparation method of the present application can also be extended to SiO 2 、Al 2 O 3 , HfO 2 , TiN, AlN and TaN and other oxides or nitrides.

[0067] Therefore, the present application can be implemented without relying on electrochemical deposition and is applicable to a variety of materials, including oxides and nitrides.

[0068] In some embodiments of the present application, before the template dissolving step, the method further comprises: a support enhancing step: adding a support layer on the surface of the metal substrate, wherein the support layer is a polymer support layer or a metal support layer.

[0069] Adding a support layer is an optional step. To increase the stability of the structure, an additional support layer may be added to the metal substrate. The support layer may be a polymer support layer or a metal support layer. This application does not limit this and the support layer may be selected as needed.

[0070] Template dissolving step S130: using a second etching solution to dissolve the ion track template to obtain a metal nanocone plasmon resonant cavity.

[0071] Finally, the ion track template is dissolved. The ion track template is slowly dissolved with a certain ratio of etching solution. The cone holes between the irregular polymer cones form a cone pit structure, thereby obtaining a metal nanocone tube plasmon resonant cavity with a large aspect ratio. Please also refer to Figure 3~Figure 7 ,go through Figure 3 After the sputtering process shown, multiple match head structures formed on the top of multiple irregular polymer cones of the ion track template adhere together to form a metal substrate, as shown in FIG. Figure 4 After the ion track template is dissolved, the match head side of the metal substrate is marked as the top, and it is turned over. The other side of the metal substrate is "grown" with hollow metal nanocones with a large aspect ratio. These hollow metal nanocones form a metal nanocone plasmon resonant cavity, and its microstructure is shown in the figure. Figure 5-Figure 7 shown.

[0072] The second etching solution in this step is similar to the first etching solution in step S110, except that the proportion of the NaOH aqueous solution in the mixed solution is greater than 50%. That is, in the template dissolving step, for polyethylene terephthalate or polycarbonate, the second etching solution is preferably a mixture of sodium hydroxide (NaOH) aqueous solution and methanol, the sodium hydroxide (NaOH) aqueous solution is recorded as the third sodium hydroxide aqueous solution, and the mixed solution is recorded as the third mixed solution, wherein the concentration of the third sodium hydroxide aqueous solution is preferably 2.5-9 mol / L, methanol can be of analytical grade from any commercial manufacturer, and the mass content of the third sodium hydroxide aqueous solution in the third mixed solution is greater than 50%; for PI, the second etching solution is preferably a mixture of sodium hydroxide (NaOH) aqueous solution and sodium hypochlorite, the sodium hydroxide (NaOH) aqueous solution is recorded as the fourth sodium hydroxide aqueous solution, and the mixed solution is recorded as the fourth mixed solution, wherein the concentration of the fourth sodium hydroxide aqueous solution is preferably 2.5-9 mol / L, sodium hypochlorite (NaClO) can be of analytical grade from any commercial manufacturer, and the mass content of the fourth sodium hydroxide aqueous solution in the fourth mixed solution is greater than 50%.

[0073] The aspect ratio of the hollow metal cone tube of the metal nanocone tube plasmon resonance cavity prepared by any of the above-mentioned preparation methods of the metal nanocone tube plasmon resonance cavity is greater than 20, and the thinnest tube wall of the hollow metal cone tube is less than or equal to 10 nm; and it supports multiple resonance modes; the cone tube structure is adjustable, the tube wall is smooth, and it can be prepared on a large area; the metal nanocone tube plasmon resonance cavity can be an all-metal structure, and has broad potential application value in the fields of photocatalysis, sensing and detection.

[0074] Example 1

[0075] Step (1): PC (polymer substrate) with a thickness of 175 µm was irradiated by the TR5 irradiation terminal of the Heavy Ion Research Facility Lanzhou (HIRFL) of the Institute of Modern Physics, Chinese Academy of Sciences. The irradiation ions were Xe, the ion energy was 2500 MeV, and the irradiation dose was 2×10 8 ions / cm 2 The irradiated polymer substrate is placed in a first etching solution to ensure that the surface of the polymer substrate is fully in contact with the first etching solution. The first etching solution is a first mixed solution of a first NaOH aqueous solution and methanol. The concentration of the first NaOH aqueous solution is 9 mol / L. Methanol is of commercially available analytical grade. The mass content of methanol in the first mixed solution is 95%. The temperature is maintained at 25°C in a water bath and etching is performed for 4 hours.

[0076] Then, the polymer substrate is taken out from the first etching solution, rinsed twice with deionized water to remove the first etching solution and adsorbed particles on the surface, rinsed once with anhydrous ethanol, and finally rinsed again with deionized water and hung to dry naturally. The obtained polymer substrate with micro-nano structure, i.e., ion track template, is Figure 2 As shown, from Figure 2 It can be seen that the micro-nanostructure on the ion track template is composed of two types of structural units: conical holes with large aspect ratios and irregular polymer cones with large length-to-diameter ratios.

[0077] Step (2): Place the ion track template in a magnetron sputtering coating apparatus, with the micro-nano structure facing the sputtering target, select Pd as the target material, set the sputtering current to 10 mA, and the coating time to 2 h. After the sputtering is completed, take out the ion track template substrate with the metal substrate. The surface of the ion track template after sputtering is as follows: Figure 4 During the sputtering process, due to the shadow effect and the large aspect ratio of the cone hole and the large length-diameter ratio of the polymer cone, the thickness of the metal layer is distributed in a gradient from top to bottom on the side wall of the polymer cone and the hole wall of the cone hole. As the deposition continues, the tip of the polymer cone gradually forms a "match head" structure, making the shadow effect of the deposition more significant, and finally closing the opening of the cone hole to form a metal substrate, as shown in Figure 1. Figure 4At this time, the cone tube structure in the cone hole no longer changes, and a nanocone tube with a large aspect ratio is formed in the cone hole; deposition continues, and a denser metal substrate is gradually formed at the closed cone hole, and the sufficient thickness can make the final nanocone tube plasmon resonant cavity self-supporting.

[0078] Step (3): Coat a layer of high temperature resistant sealant (purchased from: Meisgoton, model: Gao Mowen 500) on the surface of the metal substrate on the above-mentioned ion track template, and place it naturally for 24 hours to wait for the high temperature resistant sealant to be completely cured as a support layer for the metal substrate.

[0079] Step (4): placing the ion track template with a metal substrate to which a support layer is added in a second etching solution, wherein the second etching solution is a third mixed solution of a third NaOH aqueous solution and methanol, wherein the concentration of the third NaOH aqueous solution is 9 mol / L, the methanol is of analytical grade, and the mass content of the third NaOH aqueous solution in the third mixed solution is 60%. The water bath temperature is set to 50°C, and the reaction is carried out for 10 hours. The ion track template is completely dissolved, and the remaining structure is rinsed twice with deionized water to remove the second etching solution remaining on the surface of the remaining structure, and then rinsed once with anhydrous ethanol, and finally rinsed again with deionized water and dried naturally, and finally a metal nanocone tube plasmon resonance cavity made of Pd material is obtained. The metal substrate is placed downward and the metal nanocone tube is placed upward for electron microscope scanning, and the following is obtained: Figure 5-Figure 7 The image shown. Figure 5-Figure 7 It can be seen that the Pd metal nanocone tube plasmon resonant cavity is indeed a cone tube array structure with a large aspect ratio, each cone tube has a uniform size, is vertically and evenly distributed, and has an extremely thin and smooth tube wall. It should be noted that this step cannot use fast dissolving agents such as dichloromethane, which will destroy the metal nanocone tube structure due to the shrinkage of the polymer.

[0080] Figure 8 This is the absorption spectrum of the metal nanocone plasmon resonant cavity prepared in Example 1. The absorption rate is obtained by 1-hemispherical reflectivity-transmittance (the curves in the figure correspond to 0°, 30°, and 60° from top to bottom). The hemispherical reflectivity and transmittance are measured by a UV-visible near-infrared spectrophotometer. The instrument model is LAMBDA 900 from PerkinElmer, USA. A hemispherical total reflection test unit is used. The test wavelength range is 300 nm-2300 nm, the wavelength interval is 2 nm, and a Spectralon 99% standard reflector with a calibration value is used as a reference standard. Figure 8From the absorption spectrum shown, it can be seen that at vertical incidence and an incident angle of 30°, the average absorption rate of the metal nanocone tube plasmon resonant cavity made of Pd material in the range of 300 nm-2300 nm is greater than 99.5%; when the incident angle is 50°, the average absorption rate in this band is greater than 99.3%, indicating that the metal nanocone tube plasmon resonant cavity made of Pd material has excellent wide-angle, wide-spectrum and high absorption rate characteristics.

[0081] Example 2

[0082] Step (1): Same as step (1) in Example 1.

[0083] Step (2): Place the ion track template into a magnetron sputtering coating apparatus, with the micro-nano structure facing the sputtering target. Select Cu as the target material, set the sputtering current to 20 mA, the coating time to 20 h, and the surface coating thickness to about 30 µm. After the sputtering is completed, take out the ion track template with the metal substrate.

[0084] Step (3): Omit the addition of an additional support layer and directly dissolve the ion track template in the same manner as step (4) of Example 1. Since the metal substrate has sufficient thickness, the remaining metal structure can be self-supporting, thereby obtaining a Cu-made metal nanocone plasmon resonant cavity.

[0085] Example 3

[0086] Step (1): PI (polymer substrate) with a thickness of 150 µm was irradiated by the TR5 irradiation terminal of the Heavy Ion Research Facility (HIRFL) of the Institute of Modern Physics, Chinese Academy of Sciences. The irradiation ions were Ta, the ion energy was 2900 MeV, and the irradiation dose was 5×10 8 ions / cm 2 . The irradiated polymer substrate is placed in the first etching solution to ensure that the surface of the polymer substrate is fully in contact with the first etching solution. The first etching solution is a second mixed solution of a second NaOH aqueous solution and NaClO, wherein the concentration of the second NaOH aqueous solution is 5 mol / L, NaClO is of analytical grade, and the mass content of NaClO is 90%. Etching is performed for 3 hours in a water bath at 50°C. Then the polymer substrate is taken out of the first etching solution, rinsed twice with deionized water to remove the first etching solution remaining on the surface, rinsed once with anhydrous ethanol, and finally rinsed again with deionized water and suspended to dry naturally to obtain a polymer substrate with a micro-nano structure, namely, an ion track template.

[0087] Step (2): Place the ion track template in a magnetron sputtering coating apparatus with its micro-nano structure facing the sputtering target. Select Ti as the target material, introduce nitrogen gas, and sputter 100 nm thick TiN on the ion track template. After sputtering, take out the ion track template with the metal substrate.

[0088] Step (3): Same as step (3) of Example 1.

[0089] Step (4): placing the ion track template with a metal substrate to which a support layer is added in a second etching solution, wherein the second etching solution is a fourth mixed solution of a fourth NaOH aqueous solution and NaClO, wherein the NaClO is of analytical grade, wherein the concentration of the fourth NaOH aqueous solution is 5 mol / L, the NaClO is of analytical grade, and the NaClO content is 49%. The water bath temperature is set to 50° C. and the reaction is carried out for 10 hours. The ion track template is completely dissolved, and the remaining structure is rinsed twice with deionized water to remove the second etching solution remaining on the surface, and then rinsed once with anhydrous ethanol, and finally rinsed again with deionized water and naturally dried to obtain a metal nanocone tube plasmon resonance cavity made of TiN material.

[0090] Example 4

[0091] Step (1): PC (polymer substrate) with a thickness of 150 µm was irradiated by the TR5 irradiation terminal of the Heavy Ion Research Facility Lanzhou (HIRFL) of the Institute of Modern Physics, Chinese Academy of Sciences. The irradiation ions were Bi, the ion energy was 1980 MeV, and the irradiation dose was 1×10 7 ions / cm 2 . The irradiated polymer substrate is placed in the first etching solution to ensure that the surface of the polymer substrate is in full contact with the first etching solution. The first etching solution is a first mixed solution of a first NaOH aqueous solution and methanol, wherein the concentration of the first NaOH aqueous solution is 9 mol / L, the methanol is of analytical grade, and the mass content of methanol in the first mixed solution is 90%. The etching is carried out in a water bath at 50°C for 2 hours. Then the polymer substrate is taken out from the etching solution, rinsed twice with deionized water to remove the first etching solution remaining on the surface, rinsed once with anhydrous ethanol, and finally rinsed again with deionized water and suspended to dry naturally to obtain a polymer substrate with a micro-nano structure, namely, an ion track template.

[0092] Step (2): Place the ion track template into a magnetron sputtering coating apparatus with its micro-nano structure facing the sputtering target. Select Ni as the target material, set the sputtering current to 10 mA, and the coating time to 2 h. After the sputtering is completed, take out the ion track template with the metal substrate.

[0093] Step (3): Deposit an additional Cu support layer on the surface of the metal substrate by electrochemical deposition, with the Cu electrolyte composition being 75 g / L Cu 2 SO 4 •5H 2 O+30 g / LH 2 SO 4 , the deposition voltage is 0.5V, and the deposition time is 1h.

[0094] Step (4): placing the ion track template with a metal substrate to which a support layer is added in a second etching solution, wherein the second etching solution is a third mixed solution of a third NaOH aqueous solution and methanol, wherein the concentration of the third NaOH aqueous solution is 5 mol / L, and the methanol is of analytical grade, wherein the mass content of methanol in the third mixed solution is 20%, setting the water bath temperature to 50°C, and reacting for 10 hours. After the ion track template is completely dissolved, the remaining structure is rinsed twice with deionized water to remove the second etching solution remaining on the surface, and then rinsed once with anhydrous ethanol, and finally rinsed again with deionized water and dried naturally to obtain a nanocone plasmon resonance cavity made of Ni.

[0095] Example 5

[0096] Step (1): 150 µm thick PET (polymer substrate) was irradiated by the TR5 irradiation terminal of the Heavy Ion Research Facility Lanzhou (HIRFL) of the Institute of Modern Physics, Chinese Academy of Sciences. The irradiation ion was Kr, the ion energy was 1500 MeV, and the irradiation dose was 1×10 9 ions / cm 2 . The irradiated polymer substrate is placed in the first etching solution to ensure that the surface of the polymer substrate is fully in contact with the first etching solution. The first etching solution is a first mixed solution of a first NaOH aqueous solution and methanol. The concentration of the first NaOH aqueous solution is 5 mol / L. The methanol is analytically pure. The mass content of methanol in the first mixed solution is 50%. Etching is performed in a water bath at 50°C for 2 hours. Then the polymer substrate is taken out of the etching solution, rinsed twice with deionized water to remove the first etching solution remaining on the surface, rinsed once with anhydrous ethanol, and finally rinsed again with deionized water and suspended to dry naturally. The obtained polymer substrate with micro-nano structure is the ion track template.

[0097] Step (2): Place the ion track template into a magnetron sputtering coating apparatus with its micro-nano structure facing the sputtering target, select the target material as W, set the sputtering current to 20 mA, and the coating time to 2 h. After the sputtering is completed, take out the ion track template with the metal substrate.

[0098] Step (3): Same as step (3) of Example 4.

[0099] Step (4): placing the ion track template with a metal substrate to which a support layer is added in a second etching solution, wherein the second etching solution is a third mixed solution of a third NaOH aqueous solution and methanol, wherein the concentration of the third NaOH aqueous solution is 5 mol / L, the methanol is analytical grade, and the mass content of methanol in the third mixed solution is 10%. The water bath temperature is set to 70°C, and the reaction is carried out for 5 hours. After the ion track template is completely dissolved, the remaining structure is rinsed twice with deionized water to remove the second etching solution remaining on the surface, and then rinsed once with anhydrous ethanol, and finally rinsed again with deionized water and dried naturally to obtain a nanocone tube plasmon resonance cavity made of W material.

[0100] The embodiments described above are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included in the protection scope of the present invention.

Claims

1. A method for preparing a metal nanocone plasmon resonant cavity, characterized in that: The metal nano-cone tube plasmon resonant cavity comprises a nano-scale hollow metal cone tube array structure, wherein the hollow metal cone tube array structure comprises irregular hollow metal cone tubes and irregular conical pit structures formed between the hollow metal cone tubes; The aspect ratio of the hollow metal conical tube is greater than 20, and the thinnest tube wall of the hollow metal conical tube is less than or equal to 10 nm; The preparation method of the metal nanocone tube plasmon resonant cavity comprises: The template preparation step comprises: irradiating a polymer substrate with a high-energy heavy ion beam to cause track damage on the surface of the polymer substrate; and placing the irradiated polymer substrate in a first etching solution for etching to form irregular polymer cones and cone holes between the irregular polymer cones to obtain an ion track template; Metal deposition step: depositing a metal layer on the surface of the ion track template by using a coating technology to form a metal substrate; Template dissolving step: using a second etching solution to dissolve the ion track template to obtain a metal nanocone plasmon resonant cavity; Wherein, in the template preparation step, the polymer substrate is selected from one of polyethylene terephthalate, polyimide and polycarbonate; The thickness of the polymer substrate is greater than 50 μm; in the template preparation step, if the polymer substrate is polyethylene terephthalate or polycarbonate, the first etching solution is a first mixed solution of a first sodium hydroxide aqueous solution and methanol in any proportion, wherein the concentration of the first sodium hydroxide aqueous solution is 2.5-9 mol / L, and the methanol is of analytical grade; If the polymer substrate is polyimide, the first etching solution is a second mixed solution of a second sodium hydroxide aqueous solution and sodium hypochlorite in any ratio, wherein the concentration of the second sodium hydroxide aqueous solution is 2.5-9 mol / L, and the sodium hypochlorite is of analytical grade; In the template dissolving step, if the polymer substrate is polyethylene terephthalate or polycarbonate, the second etching solution is a third mixed solution of a third sodium hydroxide aqueous solution and methanol in any proportion, wherein the concentration of the third sodium hydroxide aqueous solution is 2.5-9 mol / L, and the methanol is of analytical grade; If the polymer substrate is polyimide, the second etching solution is a fourth mixed solution of a fourth sodium hydroxide aqueous solution and sodium hypochlorite in any ratio, wherein the concentration of the fourth sodium hydroxide aqueous solution is 2.5-9 mol / L, and the sodium hypochlorite is of analytical grade; The mass content of the third aqueous sodium hydroxide solution in the third mixed solution is greater than 50%; the mass content of the fourth aqueous sodium hydroxide solution in the fourth mixed solution is greater than 50%.

2. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 1, characterized in that: When the material of the hollow metal cone tube is palladium, the absorption rate of the metal nanocone tube plasmon resonance cavity to light in the wavelength band of 300 nm-2300 nm is greater than 99.5%.

3. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 1, characterized in that: Before the template dissolving step, the method further comprises: Support enhancement step: adding a support layer on the surface of the metal substrate, wherein the support layer is a polymer support layer or a metal support layer.

4. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 1, characterized in that: The concentration of the first sodium hydroxide aqueous solution is 9 mol / L, and the mass content of methanol in the first mixed solution is 95%; The concentration of the second sodium hydroxide aqueous solution is 5 mol / L, and the mass content of the sodium hypochlorite in the second mixed solution is 90%.

5. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 1, characterized in that: The high energy heavy ions are selected from 86 Kr, 129 Xe, 183 Ta and 209 At least one of Bi; and the ion energy of the high-energy heavy ions is greater than 1500 MeV.

6. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 5, characterized in that: The irradiation dose of the high energy heavy ions is 1×10 7 ions / cm 2 -1×10 9 ions / cm 2 .

7. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 6, characterized in that: The irradiation dose of the high energy heavy ions is 1×10 7 ions / cm 2 , 2×10 7 ions / cm 2 , 3×10 7 ions / cm 2 , 4×10 7 ions / cm 2 , 5×10 7 ions / cm 2 , 6×10 7 ions / cm 2 ,7×10 7 ions / cm 2 , 8×10 7 ions / cm 2 ,9×10 7 ions / cm 2 , 1×10 8 ions / cm 2 , 2×10 8 ions / cm 2 , 3×10 8 ions / cm 2 , 4×10 8 ions / cm 2 , 5×10 8 ions / cm 2 , 6×10 8 ions / cm 2 ,7×10 8 ions / cm 2 , 8×10 8 ions / cm 2 ,9×10 8 ions / cm 2 and 1×10 9 ions / cm 2 Any one of .

8. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 7, characterized in that: The irradiation dose is 2×10 8 ions / cm 2 .

9. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 1, characterized in that: In the template preparation step, the etching is performed in a water bath heating environment, the water bath temperature is 25° C.-70° C., and the etching time is 1 h-10 h.

10. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 1, characterized in that: In the metal deposition step, the coating technology is magnetron sputtering or evaporation.

11. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 10, characterized in that: The coating technology is magnetron sputtering.

12. The method for preparing a metal nanocone tube plasmon resonant cavity according to claim 1, characterized in that: In the metal deposition step, the material of the metal layer is selected from one or an alloy formed by several of gold, silver, copper, aluminum, palladium, cobalt, chromium, iron, indium, molybdenum, niobium, nickel, lead, platinum, tin, tantalum, vanadium, tungsten, zinc, manganese, antimony, bismuth and germanium, or is selected from any one of SiO2, Al2O3, HfO2, TiN, AlN and TaN.

13. The method for preparing the metal nanocone tube plasmon resonant cavity according to claim 1, characterized in that: The template dissolving step is carried out in a water bath environment, the water bath temperature is 50° C.-70° C., and the dissolving time is 5 h-10 h.

14. Application of the metal nanocone tube plasmon resonant cavity prepared by the method for preparing the metal nanocone tube plasmon resonant cavity according to any one of claims 1 to 13 in photocatalysis, sensing technology and detection technology.