A lithium-sulfur battery positive electrode material and preparation method thereof, positive electrode and lithium-sulfur battery

By using high-entropy selenide-two-dimensional material heterojunction nanomaterials in lithium-sulfur batteries, the problems of slow kinetics and poor conductivity are solved, and the efficient electrochemical performance and long life of lithium-sulfur batteries are achieved, which improves its commercialization .

CN118588918BActive Publication Date: 2024-11-19SONGSHAN LAKE MATERIALS LAB +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411074598.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Lithium sulfur batteries have problems such as shuttle effect, poor electron/ion conductivity, volume expansion caused by slow kinetics, resulting in reduced battery capacity, poor cycle performance and safety risks, limiting their commercial application.

Method used

High-entropy selenide-two-dimensional material heterojunction nanomaterials are used as the cathode material of lithium sulfur batteries, including MXene and/or graphene, and high-entropy selenide-MXene or high-entropy selenide-MXene or high-index Entropy selenide-graphene heterojunction material improves the kinetics and conductivity of lithium polysulfide, buffers volume expansion, and maintains the stability of the electrode structure.

Benefits of technology

It significantly improved the electrochemical performance of lithium-sulfur batteries. The first specific capacity reached more than 1120mAh/g for the first time, and the first Coulomb efficiency was as high as more than 99.1%. The specific capacity was still above 1012mAh/g after 100 turns, extending the battery life and improving capacity stability. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118588918B_ABST
    Figure CN118588918B_ABST
Patent Text Reader

Abstract

The present invention provides a lithium-sulfur battery positive electrode material and a preparation method thereof, a positive electrode and a lithium-sulfur battery, wherein the lithium-sulfur battery positive electrode material comprises a high-entropy selenide-two-dimensional material heterojunction nanomaterial and sulfur; the two-dimensional material in the high-entropy selenide-two-dimensional material heterojunction nanomaterial comprises MXene and / or graphene. The high-entropy selenide in the positive electrode material has 5 or more metal active sites, which can serve as sites in the process of lithium polysulfide adsorption-catalysis-conversion, thereby improving the redox kinetics of sulfur and promoting the effective utilization rate of sulfur. In addition, the high-entropy selenide-two-dimensional material has excellent electronic / ionic conductivity and mechanical properties, and can provide an electronic / ion transmission channel in the redox process of the lithium-sulfur battery. At the same time, the excellent mechanical properties can also effectively buffer the volume expansion of the positive electrode material, thereby improving the capacity stability and the service life of the battery, and improving the electrochemical performance of the lithium-sulfur battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a positive electrode material for a lithium-sulfur battery and a preparation method thereof, a positive electrode and a lithium-sulfur battery. Background Art

[0002] The 16-electron reaction between the elemental sulfur positive electrode and the lithium metal negative electrode can provide a theoretical energy density of 2600Wh / kg, which is much higher than that of traditional lithium-ion batteries. In addition, sulfur has the advantages of abundant reserves, low toxicity and low cost. These competitive advantages make Li-S batteries one of the most promising battery technologies for large-scale application.

[0003] However, lithium-sulfur batteries are still in the research and development stage, and there are still many problems in large-scale application, mainly concentrated in: (1) The shuttling effect of polysulfide. When lithium polysulfide is dissolved in an organic electrolyte, due to its slow conversion kinetics, a large amount of lithium polysulfide accumulates on the positive electrode side. Driven by the concentration gradient, lithium polysulfide shuttles from the positive electrode side through the diaphragm to the negative electrode side. Because the lithium polysulfide shuttled to the negative electrode reacts with the lithium metal at the negative electrode, a layer of electronically insulating low-sulfur lithium (Li2S / Li2S2) is formed on the surface of the lithium negative electrode, which greatly reduces the ion conductivity and causes a large amount of active material loss, resulting in a decrease in battery capacity and shortened life; (2) Elemental sulfur is almost an electronic / ionic insulator, which is one of the main reasons for the slow sulfur redox kinetics and also leads to low utilization of sulfur active materials; (3) During the charge and discharge process, the conversion of elemental sulfur and sulfide will cause the volume of the positive electrode to change, causing the battery capacity to decay and even destroying the battery structure. The above problems lead to battery capacity decay, poor cycle performance, and may even cause safety issues, limiting its commercial application.

[0004] Therefore, in the prior art, lithium-sulfur batteries suffer from the shuttle effect caused by slow kinetics, poor electron / ion conductivity, and volume expansion, which leads to a decrease in sulfur capacity, low effective sulfur utilization, and poor cycle stability. This has become a technical problem that needs to be urgently solved by those skilled in the art. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a lithium-sulfur battery positive electrode material and a preparation method thereof, a positive electrode and a lithium-sulfur battery, which can effectively solve the technical problems of existing lithium-sulfur batteries such as shuttle effect, poor electron / ion conductivity, volume expansion, etc. caused by slow kinetics.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a positive electrode material for a lithium-sulfur battery, wherein the positive electrode material for a lithium-sulfur battery comprises a high entropy selenide-two-dimensional material heterojunction nanomaterial and sulfur;

[0008] The two-dimensional material in the high entropy selenide-two-dimensional material heterojunction nanomaterial includes MXene and / or graphene;

[0009] The high entropy selenide includes at least five other metal elements besides selenium.

[0010] The high entropy selenide of the present invention has more than five metal atoms, and these metal atoms can interact with each other to adjust their electronic structure, thereby generating more active sites. These active sites can adsorb more lithium polysulfide. At the same time, different metal atoms show different catalytic preferences for specific reaction steps between lithium polysulfides. This uniqueness makes high entropy selenide have great advantages in the application of lithium-sulfur batteries with multi-step, multi-electron transfer and multi-phase redox conversion, and can greatly improve the kinetics of lithium polysulfide in the entire redox process. Specifically, during the discharge process, S8 molecules are rapidly converted into lithium polysulfide molecules (Li2S8, Li2S6 and Li2S4), and further rapidly converted into low-sulfide lithium molecules (Li2S and Li2S2); during the charging process, low-sulfide lithium molecules (Li2S and Li2S2) are rapidly converted into lithium polysulfide molecules (Li2S8, Li2S6 and Li2S4), and further rapidly converted into S8 molecules. This ultrafast catalytic conversion kinetics significantly weakens the "shuttle effect" of lithium polysulfide, and even achieves a "no shuttle" effect. In addition, high-entropy selenide-MXene or high-entropy selenide-graphene has excellent electronic / ionic conductivity, which can provide electronic / ion channels for the conversion of lithium polysulfide during the charge and discharge process, thereby further accelerating the kinetics of lithium polysulfide conversion and making efficient use of the active sulfur.

[0011] The high entropy selenide-MXene or high entropy selenide-graphene heterojunction material prepared by the present invention has a large specific surface area and excellent mechanical properties. This enables the high entropy selenide-MXene or high entropy selenide-graphene to effectively buffer the volume expansion of the positive electrode material, thereby maintaining the electrode structure of a good conductive skeleton and active material, improving the capacity stability and service life of the battery, and greatly improving the electrochemical performance of the lithium-sulfur battery.

[0012] Preferably, the high entropy selenide in the high entropy selenide-two-dimensional material heterojunction nanomaterial has a hexagonal crystal structure and / or a cubic crystal structure.

[0013] Preferably, the high entropy selenide-two-dimensional material heterojunction nanomaterial is a nanosheet.

[0014] Preferably, the sheet diameter of the high entropy selenide-two-dimensional material heterojunction nanomaterial is 5nm~1μm, for example, it can be 5nm, 10nm, 15nm, 20nm, 30nm, 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm or 1μm, etc.

[0015] Preferably, the thickness of the high entropy selenide-two-dimensional material heterojunction nanomaterial is 1-10 nm, for example, it can be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm.

[0016] Preferably, the content of high entropy selenide in the high entropy selenide-two-dimensional material heterojunction nanomaterial is 5~60wt%, for example, it can be 5wt%, 6wt%, 10wt%, 12wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt% or 60wt%, etc.

[0017] Preferably, the content of two-dimensional material in the high-entropy selenide-two-dimensional material heterojunction nanomaterial is 40-80wt%, for example, it can be 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt% or 80wt%.

[0018] Preferably, the sulfur content in the lithium-sulfur battery positive electrode material is 60-80wt%, for example, it can be 60wt%, 62wt%, 65wt%, 68wt%, 70wt%, 72wt%, 73wt%, 75wt%, 78wt% or 80wt%.

[0019] Preferably, the other metal elements include at least five of cobalt, molybdenum, nickel, iron, chromium, manganese, tungsten or vanadium, for example, it can be a combination of cobalt, molybdenum, nickel, iron and chromium, a combination of manganese, molybdenum, nickel, iron and chromium, a combination of cobalt, tungsten, nickel, iron and chromium, and a combination of cobalt, tungsten, vanadium, iron and chromium.

[0020] Preferably, the molar ratio of selenium to the sum of other metal elements in the high entropy selenide is (1.8~2.2):1, for example, it can be 1.8:1, 1.85:1, 1.89:1, 1.94:1, 1.98:1, 2.03:1, 2.07:1, 2.12:1, 2.16:1 or 2.2:1, etc.

[0021] The present invention further preferably has the molar ratio of selenium to the sum of other metal elements in the high entropy selenide within the above range, which can better avoid the problem of impurity phase generation.

[0022] Preferably, the molar ratio between any two of the other metal elements is (0.9-1.1):1, for example, it can be 0.9:1, 0.93:1, 0.95:1, 0.97:1, 0.99:1, 1.02:1, 1.04:1, 1.06:1, 1.08:1 or 1.1:1, etc.

[0023] The present invention further prefers that the molar ratio between any two of the other metal elements is relatively close. When the content of a certain element is too high or too low, it is difficult to form a high entropy alloy, which ultimately leads to a poor "cocktail effect".

[0024] In a second aspect, the present invention provides a method for preparing the positive electrode material of a lithium-sulfur battery according to the first aspect, the preparation method comprising the following steps:

[0025] (1) mixing a suspension of a two-dimensional material, a selenium source, other metal element sources, and a reducing agent, and performing in-situ growth by microwave heating to obtain a first nanomaterial; the other metal element sources include at least five other metal elements;

[0026] (2) The first nanomaterial of step (1) is subjected to the step of removing selenium powder and solvent to obtain the high entropy selenide-two-dimensional material heterojunction nanomaterial;

[0027] (3) Mixing elemental sulfur and the high entropy selenide-two-dimensional material heterojunction nanomaterial described in step (2), and melting them in vacuum to obtain the lithium-sulfur battery positive electrode material.

[0028] The synthesis method and mechanism of the present invention are as follows: selenium and sodium borohydride are used to generate selenic acid, which is then mixed with metal acetate to rapidly form high entropy selenide under high temperature and high pressure of a microwave device.

[0029] In the present invention, the MXene or graphene substrate material has a high specific surface area, rich OH - and O 2- Functional groups, which are negatively charged and can attract positively charged metal cations (Mo 4+ ,Co 2+ , W 4+ , Fe 3+ ,Cr 2+ , V 4+ , Ni 2+ , Mn 2+etc.). During microwave heating, when the pressure and temperature reach certain conditions, the high entropy selenides of hexagonal and cubic structures are grown in situ on the surface of MXene or graphene. The high entropy selenides of hexagonal and cubic structures present a two-dimensional nanosheet structure, and the high entropy selenides of hexagonal and cubic structures grow in two-dimensional directions on the surface of MXene or graphene. The high entropy selenides of the nanosheet structure grow crosswise and do not agglomerate. Therefore, the present invention can prepare an in-situ grown high entropy selenide-MXene or high entropy selenide-graphene heterojunction material under microwave hydrothermal conditions.

[0030] Preferably, the molar ratio of selenium in the selenium source to the metal elements in other metal element sources is (1.8-2.2):1, for example, it can be 1.8:1, 1.85:1, 1.89:1, 1.94:1, 1.98:1, 2.03:1, 2.07:1, 2.12:1, 2.16:1 or 2.2:1, etc.

[0031] Preferably, the molar ratio between the metal elements in any two of the other metal element sources is (0.9~1.1):1, for example, it can be 0.9:1, 0.93:1, 0.95:1, 0.97:1, 0.99:1, 1.02:1, 1.04:1, 1.06:1, 1.08:1 or 1.1:1, etc.

[0032] Preferably, the other metal element sources include at least five of a cobalt source, a molybdenum source, a nickel source, an iron source, a chromium source, a manganese source, a tungsten source or a vanadium source.

[0033] Preferably, the other metal element sources include other metal salts, and the other metal salts include at least five of cobalt salts, molybdenum salts, nickel salts, iron salts, chromium salts, manganese salts, tungsten salts or vanadium salts.

[0034] Preferably, the cobalt salt is C4H6CoO4·4H2O and / or Co(NO3)2·6H2O.

[0035] Preferably, the molybdenum salt is NaMoO4·4H2O and / or (NH4)2Mo2O7.

[0036] Preferably, the nickel salt is Ni(CH3COO)2·4H2O and / or Ni(NO3)2·6H2O.

[0037] Preferably, the iron salt is Fe(CO2CH3)2 and / or C4H7FeO5.

[0038] Preferably, the chromium salt is C6H9O6Cr.

[0039] Preferably, the manganese salt is C4H6MnO4 and / or MnC4H6O4·4H2O.

[0040] Preferably, the tungsten salt is Na2WO4·2H2O.

[0041] Preferably, the vanadium salt is NH4VO3.

[0042] Preferably, the selenium source comprises selenium powder.

[0043] Preferably, the reducing agent comprises sodium borohydride and / or hydrazine hydrate.

[0044] Preferably, the molar ratio of the reducing agent to the selenium source is (1.5-3):1, for example, it can be 1.5:1, 1.6:1, 1.8:1, 1.9:1, 2.0:1, 2.2:1, 2.3:1, 2.5:1, 2.8:1, 2.9:1 or 3.0:1, etc.

[0045] Preferably, the concentration of the suspension of the two-dimensional material is 3-10 g / L, for example, it can be 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L, 5 g / L, 5.5 g / L, 6 g / L, 6.5 g / L, 7 g / L, 8 g / L, 9 g / L, 9.5 g / L or 10 g / L, etc.

[0046] Preferably, the ratio of the two-dimensional material to the selenium source in the suspension of the two-dimensional material is (1~5):1, for example, it can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1 or 5:1, etc.

[0047] Preferably, the two-dimensional material comprises graphene and / or MXene.

[0048] Preferably, the MXene comprises any one or a combination of at least two of Ti3C2, V2C, Nb2C and / or Mo2C, wherein typical but non-limiting combinations are a combination of Ti3C2 and V2C, a combination of Nb2C and V2C, a combination of Ti3C2 and Nb2C, a combination of Mo2C and V2C, and a combination of Ti3C2 and Mo2C.

[0049] Preferably, the mass ratio of elemental sulfur to high entropy selenide-two-dimensional material heterojunction nanomaterial is (3~8):2, for example, it can be 3:2, 3.5:2, 4:2, 4.5:2, 5:2, 5.5:2, 6:2, 6.5:2, 7:2, 7.5:2 or 8:2, etc.

[0050] Preferably, the microwave heating comprises microwave solvothermal method and / or microwave hydrothermal method.

[0051] Preferably, the pressure in the autoclave of the microwave solvothermal method is 2-6 MPa, for example, it can be 2 MPa, 2.5 MPa, 2.9 MPa, 3.4 MPa, 3.8 MPa, 4.3 MPa, 4.7 MPa, 5.2 MPa, 5.6 MPa or 6 MPa, etc., the temperature is 180-220°C, for example, it can be 180°C, 185°C, 189°C, 194°C, 198°C, 203°C, 207°C, 212°C, 216°C or 220°C, etc., and the time of the microwave solvothermal method is 0.5-4h, for example, it can be 0.5h, 0.9h, 1.3h, 1.7h, 2.1h, 2.5h, 2.9h, 3.3h, 3.7h or 4h, etc.

[0052] Preferably, the pressure in the kettle of the microwave hydrothermal method is 3-6 MPa, for example, it can be 3 MPa, 3.4 MPa, 3.7 MPa, 4 MPa, 4.4 MPa, 4.7 MPa, 5 MPa, 5.4 MPa, 5.7 MPa or 6 MPa, etc., the temperature is 180-260°C, for example, it can be 180°C, 189°C, 198°C, 207°C, 216°C, 225°C, 234°C, 243°C, 252°C or 260°C, etc., and the time is 0.5-6h, for example, it can be 0.5h, 1.2h, 1.8h, 2.4h, 3h, 3.6h, 4.2h, 4.8h, 5.4h or 6h, etc.

[0053] Preferably, after the microwave heating, a system containing the first nanomaterial is obtained, and the system containing the first nanomaterial is washed, solid-liquid separated and dried to obtain the first nanomaterial.

[0054] Preferably, the washing and solid-liquid separation are performed alternately at least three times.

[0055] Preferably, the washing comprises washing with alcohol and deionized water alternately.

[0056] Preferably, the drying comprises freeze drying.

[0057] Preferably, the method for removing selenium powder and solvent comprises Joule heating.

[0058] Preferably, the temperature of the Joule heating method is 1000-2000°C, for example, it can be 1000°C, 1110°C, 1220°C, 1330°C, 1445°C, 1550°C, 1660°C, 1770°C, 1880°C or 2000°C.

[0059] Preferably, the single Joule heating time is 0.005~15s, for example, it can be 0.005s, 1s, 3s, 5s, 6s, 8s, 9s, 11s, 12s, 14s or 15s.

[0060] Preferably, the pulse number of the Joule heating is 1 to 10 times, for example, it can be 1 time, 2 times, 3 times, 4 times, 5 times, 6 times, 7 times, 8 times, 9 times or 10 times.

[0061] Preferably, the vacuum melting temperature is 150-180°C, for example, it may be 150°C, 154°C, 157°C, 160°C, 164°C, 167°C, 170°C, 174°C, 177°C or 180°C.

[0062] Preferably, the vacuum melting time is 10 to 14 h, for example, it can be 10 h, 10.5 h, 10.9 h, 11.4 h, 11.8 h, 12.3 h, 12.7 h, 13.2 h, 13.6 h or 14 h.

[0063] Preferably, the vacuum degree of the vacuum melting is 0-0.01 kPa, for example, it may be 0 kPa, 0.001 kPa, 0.002 kPa, 0.003 kPa, 0.004 kPa, 0.005 kPa, 0.006 kPa, 0.007 kPa, 0.008 kPa, 0.009 kPa or 0.01 kPa.

[0064] Preferably, the mixture obtained by mixing the elemental sulfur with the high entropy selenide-two-dimensional material heterojunction nanomaterial in step (2) is first ground and then vacuum melted.

[0065] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0066] (1) mixing a suspension of a two-dimensional material, a selenium source, other metal element sources and a reducing agent, and performing in-situ growth by a microwave solvothermal method at a pressure of 2 to 6 MPa and a temperature of 180 to 220° C. in a kettle for 0.5 to 4 h or a microwave hydrothermal method at a pressure of 3 to 6 MPa and a temperature of 180 to 260° C. in a kettle for 0.5 to 6 h to obtain a first nanomaterial; the other metal element sources include at least five other metal elements;

[0067] Wherein, the molar ratio of selenium in the selenium source to the metal elements in other metal element sources is (1.8~2.2):1, the molar ratio between the metal elements in any two of the other metal element sources is 0.9~1.1:1, and the other metal element sources include at least five of a cobalt source, a molybdenum source, a nickel source, an iron source, a chromium source, a manganese source, a tungsten source or a vanadium source; the selenium source includes selenium powder; the reducing agent includes sodium borohydride and / or hydrazine hydrate; the molar ratio of the reducing agent to the selenium source is 1.5~3:1; the concentration of the suspension of the two-dimensional material is 3~10g / L; the ratio of the two-dimensional material to the selenium source in the suspension of the two-dimensional material is 1~5:1; the two-dimensional material includes graphene and / or MXene; the MXene includes any one or a combination of at least two of Ti3C2, V2C, Nb2C and / or Mo2C;

[0068] (2) Step (1) The first nanomaterial is subjected to a Joule heating method at 1000-2000° C., a single time of 0.005-15 s, and a pulse number of 1-10 times to remove selenium powder and solvent, thereby obtaining the high entropy selenide-two-dimensional material heterojunction nanomaterial;

[0069] (3) Mixing elemental sulfur and the high entropy selenide-two-dimensional material heterojunction nanomaterial described in step (2) in a mass ratio of 3-8:2, and vacuum melting them at 0-0.01 kPa and 150-180° C. for 10-14 h to obtain the lithium-sulfur battery positive electrode material.

[0070] In a third aspect, the present invention provides a positive electrode, which comprises the positive electrode material for a lithium-sulfur battery described in the first aspect or the positive electrode material for a lithium-sulfur battery prepared by the method for preparing the positive electrode material for a lithium-sulfur battery described in the second aspect.

[0071] The present invention has no special restrictions on other materials and structures of the positive electrode. Any material and structure that can be used for the positive electrode and is well known to those skilled in the art can be used, and can also be adjusted according to the actual process.

[0072] In a fourth aspect, the present invention provides a lithium-sulfur battery, wherein the lithium-sulfur battery comprises the positive electrode described in the third aspect.

[0073] High entropy selenides are used in lithium-sulfur batteries. The mechanism of action of lithium-sulfur batteries is different from that of sodium-ion batteries. The mechanism of action of sodium-ion batteries is the insertion and extraction of sodium ions. The action of lithium-sulfur batteries is the multi-step catalytic conversion of sulfur species.

[0074] The present invention has no special restrictions on other materials and structures in the above-mentioned lithium-sulfur battery. Any material and structure that can be used for lithium-sulfur batteries known to those skilled in the art can be adopted, and can also be adjusted according to actual processes.

[0075] Compared with the prior art, the present invention has at least the following beneficial effects:

[0076] (1) The lithium-sulfur battery cathode material provided by the present invention is a hexagonal or cubic high-entropy selenide composed of five or more metal elements, which has more metal active sites than mono- or binary metal selenides. These metal active sites are closely related to the S in lithium polysulfide. 2- Combined with other metals, they can adsorb a large amount of lithium polysulfide. At the same time, these different types of metal active sites will selectively adsorb and catalyze different lithium polysulfide species (Li2S8, Li2S6, Li2S4, Li2S2 or Li2S). These preferential catalytic properties can comprehensively improve the catalytic conversion efficiency of lithium polysulfide. Therefore, compared with traditional mono- / binary metal selenides, high entropy selenides can adsorb more lithium polysulfide and improve the kinetics of catalytic conversion at the same time, which can more effectively solve the problem of the "shuttle effect" of lithium-sulfur batteries and improve the utilization rate of sulfur positive electrodes.

[0077] (2) The high entropy selenide-MXene or high entropy selenide-graphene heterojunction material in the lithium-sulfur battery positive electrode material provided by the present invention is more firmly bonded and more evenly dispersed than ordinary composite materials. The high entropy selenide and MXene or graphene are bonded by covalent bonds. The specific bonding method is that the O 2- The ionic functional groups combine with the metal atoms of the high entropy selenide species to form a Ti-OM or COM structure (where M is the metal atom in the high entropy selenide). Therefore, the high entropy selenide-MXene or high entropy selenide-graphene material heterojunction material in the present invention has a more stable structure than the traditional composite material.

[0078] (3) The high entropy selenide-MXene or high entropy selenide-graphene heterojunction material in the lithium-sulfur battery positive electrode material provided by the present invention is used as a host material, which is a good conductive substrate and can effectively solve the problem of poor electronic / ionic conductivity of elemental sulfur and Li2S, thereby realizing the rapid transmission of ions and electrons during the charging and discharging process. In addition, the high entropy selenide-MXene or high entropy selenide-graphene material heterojunction material has a high specific surface area, which can well solve the volume expansion problem of sulfur, so that the electrode structure is relatively intact during the charging and discharging process, thereby improving the capacity stability and service life of the sulfur positive electrode, and improving the electrochemical performance of the lithium-sulfur battery. Specifically, under the preferred conditions, the material is prepared to form a lithium-sulfur battery with a first specific capacity of more than 1120mAh / g, a first coulombic efficiency of more than 99.1%, and a specific capacity of more than 1012mAh / g after 100 cycles. BRIEF DESCRIPTION OF THE DRAWINGS

[0079] Figure 1 This is a scanning electron microscope image of the high entropy selenide-MXene heterojunction material in Example 1 of the present invention;

[0080] Figure 2 XRD diagrams of high entropy selenide-MXene heterojunction materials provided in Example 1, Example 7, and Comparative Examples 1 to 3 of the present invention;

[0081] Figure 3 A graph showing the percentage of each atom in the high entropy selenide provided in Example 1, Comparative Example 1 and Comparative Example 3 of the present invention;

[0082] Figure 4 A visual diagram of the adsorption of lithium polysulfide by the high entropy selenide-MXene heterojunction material provided in an embodiment of the present invention;

[0083] Figure 5 100-cycle curve diagram of the high-entropy selenide-MXene heterojunction material provided in Example 1, Example 5, Comparative Example 1 and Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0084] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0085] Example 1

[0086] This embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery comprises the following steps:

[0087] (1) Preparation of hexagonal high entropy selenide-MXene heterojunction materials:

[0088] The MAXene precursor (Ti3AlC2) (2 mg) was etched in a mixed solution of lithium fluoride (2 mg) and 9 mol / L hydrochloric acid at 36.5 °C for 24 h to obtain a MXene (Ti3C2) suspension with a concentration of 8 g / L;

[0089] According to the molar ratio of sodium borohydride to selenium powder of 2.5:1, sodium borohydride and selenium powder were dissolved in N,N-dimethylformamide solvent (DMF) in a beaker to react and generate a selenium salt precursor; salts such as C4H6CoO4·4H2O, NaMoO4·4H2O, Fe(CO2CH3)2, C6H9O6Cr, Na2WO4·2H2O and NH4VO3 were all dissolved in the MXene suspension at a metal atom molar ratio of 1:1:1:1:1:1, and after magnetic stirring for 10 minutes, the mass ratio of MXene to selenium was 2: 1 is uniformly mixed with a selenium salt precursor solution (and the molar ratio of selenium to other metal elements is 2:1), the mixed solution is stirred for 5 minutes and then transferred into a microwave hydrothermal autoclave, the pressure in the autoclave is 4 MPa, the reaction time is 2 hours, and the reaction temperature is 220°C to obtain a system containing the first nanomaterial; the system containing the first nanomaterial is alternately washed with alcohol and deionized water three times and centrifuged until the solution is neutral (i.e., first washed once with alcohol, centrifuged to obtain a solid phase, then washed once with water and centrifuged to obtain a solid phase, and repeated three times), and the precipitate obtained by centrifugation is freeze-dried to obtain the first nanomaterial.

[0090] (2) The first nanomaterial is subjected to Joule heating treatment at a heating temperature of 1200°C, a pulse time of 10 ms, and a pulse number of 5 times to obtain a hexagonal high entropy selenide-MXene heterojunction nanomaterial with a sheet diameter of 50 nm and a thickness of 2 nm.

[0091] (3) Preparation of positive electrode material for lithium-sulfur battery: sublimated sulfur and the hexagonal high entropy selenide-MXene heterojunction material described in step (2) are mixed in a mass ratio of 4:1, and ground to obtain a mixture, wherein the sulfur content in the mixture reaches 80wt%. The mixture is placed in a sealed tube, the temperature is controlled at 160°C, the insulation time is controlled at 12h, the air in the tube is evacuated to a vacuum degree of 0.001kPa, and vacuum melting is performed to uniformly melt the elemental sulfur into the hexagonal high entropy selenide-MXene heterojunction nanomaterial, and finally a positive electrode material for lithium-sulfur battery (sulfur / hexagonal high entropy selenide-MXene heterojunction nanomaterial) is obtained.

[0092] Figure 1 The SEM image of the hexagonal high entropy selenide-MXene heterojunction material provided in this embodiment. It can be seen from the SEM image that the high entropy selenide nanosheets are uniformly grown in situ on the MXene surface.

[0093] Figure 2 The XRD diagram of the hexagonal high entropy selenide-MXene heterojunction material provided in the embodiment of the present invention. Figure 2It can be seen that there are no impurity peaks caused by phase separation in the hexagonal high-entropy selenide-MXene heterojunction material of the sample obtained in this example. Therefore, the XRD diagram preliminarily proves that a pure phase hexagonal high-entropy selenide-MXene heterojunction material has been successfully synthesized.

[0094] Figure 3 The element content diagram (ICP) of the hexagonal high entropy selenide-MXene heterojunction material provided in Example 1, Comparative Example 1 and Comparative Example 3 of the present invention. Figure 3 It can be seen that the content proportions of each metal atom in the high entropy selenide-MXene heterojunction material in Example 1 are close, and the molar ratio of the sum of the metal atoms to the selenium content is 1:2.

[0095] Figure 4 This is a visual diagram of the adsorption of lithium polysulfide by the hexagonal high entropy selenide-MXene heterojunction material provided in the embodiment of the present invention. Figure 4 It can be seen that the bottle on the left is orange-yellow Li2S4, and the bottle on the right is the liquid after the low-entropy / medium-entropy / high-entropy selenide-MXene heterojunction material adsorbs Li2S4. The high-entropy selenide-MXene heterojunction material provided in the embodiment of the present invention has a strong adsorption effect on Li2S4. It can be seen that the orange-yellow Li2S4 is close to colorless after being adsorbed by the high-entropy selenide-MXene heterojunction material.

[0096] Example 2

[0097] This embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery comprises the following steps:

[0098] (1) Preparation of hexagonal high entropy selenide-graphene heterojunction nanomaterials:

[0099] Sodium borohydride and selenium powder were dissolved in N,N-dimethylformamide solvent (DMF) in a beaker at a molar ratio of 2:1 to generate a selenium salt precursor. C4H6CoO4·4H2O, NaMoO4·4H2O, Fe(CO2CH3)2, C6H9O6Cr, Na2WO4·2H2O and NH4VO3 salts were dissolved in a graphene suspension (concentration of 8 g / L) at a metal atom molar ratio of 1:1:1:1:1:1, and stirred magnetically for 10 min. The graphene suspension was heated at a mass ratio of 2:1 to 2. :1 is uniformly mixed with a selenium salt precursor solution (and the molar ratio of selenium to other metal elements is 2:1), the mixed solution is stirred for 5 minutes and then transferred into a microwave hydrothermal kettle, the pressure in the kettle is 4 MPa, the reaction time is 2 hours, and the reaction temperature is 220°C to obtain a system containing the first nanomaterial; the system containing the first nanomaterial is alternately washed with alcohol and deionized water three times and centrifuged until the solution is neutral (i.e., first washed once with alcohol, centrifuged to obtain a solid phase, then washed once with water and centrifuged to obtain a solid phase, and repeated three times), the precipitate obtained by centrifugation is freeze-dried to obtain the first nanomaterial.

[0100] (2) The first nanomaterial is subjected to Joule heating treatment at a heating temperature of 1200°C, a pulse time of 10 ms, and a pulse number of 5 times to obtain a hexagonal high entropy selenide-graphene heterojunction nanomaterial with a sheet diameter of 100 nm and a thickness of 2 nm.

[0101] (3) Preparing a positive electrode material for a lithium-sulfur battery: mixing sublimated sulfur and the hexagonal high entropy selenide-graphene heterojunction nanomaterial described in step (2) in a mass ratio of 4:1, and grinding to obtain a mixture, wherein the sulfur content in the mixture reaches 80%, placing the mixture into a sealed tube, controlling the temperature at 155° C., and holding the mixture for 12 h. The air in the tube is evacuated until the vacuum degree is 0.001 kPa, and vacuum melting is performed to uniformly melt the elemental sulfur into the hexagonal high entropy selenide-graphene heterojunction nanomaterial, thereby finally obtaining a positive electrode material for a lithium-sulfur battery (sulfur / hexagonal high entropy selenide-graphene heterojunction nanomaterial).

[0102] Example 3

[0103] This embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery comprises the following steps:

[0104] (1) Preparation of hexagonal high entropy selenide-MXene heterojunction materials:

[0105] The MAXene precursor (Ti3AlC2) was etched in a mixed solution of lithium fluoride (2 mg) and 10 mol / L hydrochloric acid at 38 °C for 20 h to obtain a MXene (Ti3C2) suspension with a concentration of 8 g / L.

[0106] Sodium borohydride and selenium powder were dissolved in N,N-dimethylformamide solvent (DMF) in a beaker at a molar ratio of 2:1 to generate a selenium salt precursor. C4H6CoO4·4H2O, Ni(CH3COO)2·4H2O, C6H9O6Cr, MnC4H6O4·4H2O and NH4VO3 salts were all dissolved in the MXene suspension at a metal atom molar ratio of 0.9:1:1:0.9:1. After magnetic stirring for 15 minutes, the suspension was mixed with selenium salt at a mass ratio of MXene to selenium of 2:1. The precursor solutions are uniformly mixed (and the molar ratio of selenium to other metal elements is 2:1), the mixed solution is stirred for 10 minutes and then transferred into a microwave hydrothermal autoclave with a pressure of 3 MPa, a reaction time of 6 hours, and a reaction temperature of 180°C to obtain a system containing the first nanomaterial; the system containing the first nanomaterial is alternately washed four times with alcohol and deionized water and centrifuged until the solution is neutral (i.e., washed once with alcohol, centrifuged to obtain a solid phase, then washed once with water and centrifuged to obtain a solid phase, and repeated four times), the precipitate obtained by centrifugation is freeze-dried to obtain the first nanomaterial.

[0107] (2) The first nanomaterial is subjected to Joule heating treatment at a heating temperature of 2000°C, a pulse time of 5 ms, and a pulse number of 6 times to obtain a cubic high-entropy selenide-MXene heterojunction nanomaterial with a sheet diameter of 75 nm and a thickness of 6.5 nm.

[0108] (3) Preparation of positive electrode material for lithium-sulfur battery: sublimated sulfur and the cubic high entropy selenide-MXene heterojunction material described in step (2) are mixed in a mass ratio of 3:1, and ground to make the sulfur content in the mixture reach 75%, and the mixture is placed in a sealed tube, the temperature is controlled at 180°C, the insulation time is controlled at 10 h, the air in the tube is evacuated to a vacuum degree of 0.001 kPa, and vacuum melting is performed to make the elemental sulfur evenly melt into the cubic high entropy selenide-MXene heterojunction nanomaterial, and finally a positive electrode material for lithium-sulfur battery (sulfur / cubic high entropy selenide-MXene heterojunction nanomaterial) is obtained.

[0109] Example 4

[0110] This embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery comprises the following steps:

[0111] (1) Preparation of hexagonal high entropy selenide-graphene heterojunction nanomaterials:

[0112] Sodium borohydride and selenium powder were dissolved in N,N-dimethylformamide solvent (DMF) in a beaker at a molar ratio of 2:1 to generate a selenium salt precursor. C4H6CoO4·4H2O, Ni(CH3COO)2·4H2O, C6H9O6Cr, MnC4H6O4·4H2O and NH4VO3 salts were dissolved in a graphene suspension (concentration of 8 g / L) at a metal atom molar ratio of 1:1.1:1:1.1:1, and stirred magnetically for 8 min. The graphene and selenium were mixed at a mass ratio of 2:1. The selenium salt precursor solution is uniformly mixed (and the molar ratio of selenium to other metal elements is 2:1), the mixed solution is stirred for 12 minutes and then transferred into a microwave hydrothermal autoclave, the pressure in the autoclave is 3 MPa, the reaction time is 1 hour, and the reaction temperature is 260°C to obtain a system containing the first nanomaterial; the system containing the first nanomaterial is alternately washed with alcohol and deionized water five times and centrifuged until the solution is neutral (i.e., first washed once with alcohol, centrifuged to obtain a solid phase, then washed once with water and centrifuged to obtain a solid phase, and repeated five times), the precipitate obtained by centrifugation is freeze-dried to obtain the first nanomaterial.

[0113] (2) The first nanomaterial is subjected to Joule heating treatment at a heating temperature of 1000°C, a pulse time of 50 ms, and a pulse number of 10 times to obtain a cubic high entropy selenide-graphene heterojunction nanomaterial with a sheet diameter of 200 nm and a thickness of 3 nm.

[0114] (3) Preparing a positive electrode material for a lithium-sulfur battery: mixing sublimated sulfur and the cubic high-entropy selenide-graphene heterojunction nanomaterial described in step (2) in a mass ratio of 3:1, and grinding to obtain a mixture, wherein the sulfur content in the mixture reaches 75%, placing the mixture into a sealed tube, controlling the temperature at 150° C., and holding the mixture for 14 h. The air in the tube is evacuated to a vacuum degree of 0.001 kPa, and vacuum melting is performed to uniformly melt the elemental sulfur into the cubic high-entropy selenide-graphene heterojunction nanomaterial, thereby finally obtaining a positive electrode material for a lithium-sulfur battery (sulfur / cubic high-entropy selenide-graphene heterojunction nanomaterial).

[0115] Example 5

[0116] The present embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery is the same as that of Embodiment 1, except that other metal salts are not added to C6H9O6Cr and the molar ratio of selenium to other metal elements is maintained at 2:1, and will not be described in detail here.

[0117] Example 6

[0118] The present embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery is the same as that of Embodiment 1, except that Fe(CO2CH3)2 is not added to other metal salts and the molar ratio of selenium to other metal elements is maintained at 2:1, and will not be repeated here.

[0119] Example 7

[0120] This embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery is the same as that of Embodiment 1, except that other metal salts are not added with NH4VO3 and the molar ratio of selenium to other metal elements is maintained at 2:1, and will not be repeated here.

[0121] Example 8

[0122] This embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery is the same as that of Embodiment 1 except that the molar ratio of selenium to other metal elements is 2.5:1, and will not be described in detail herein.

[0123] Example 9

[0124] This embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery is the same as that of Embodiment 1 except that the molar ratio of selenium to other metal elements is 1.5:1, and will not be described in detail herein.

[0125] Example 10

[0126] This embodiment provides a positive electrode material for a lithium-sulfur battery. The preparation method of the positive electrode material for a lithium-sulfur battery is the same as that of Embodiment 1, except that vacuum melting is not performed after grinding in step (3), and will not be described in detail here.

[0127] Embodiment 11

[0128] The present embodiment provides a lithium-sulfur battery positive electrode material. The preparation method of the lithium-sulfur battery positive electrode material is the same as that of Embodiment 1, except that in step (3), the metal atomic molar ratio of C4H6CoO4·4H2O, NaMoO4·4H2O, Fe(CO2CH3)2, C6H9O6Cr, Na2WO4·2H2O and NH4VO3 salt is 1.5:1:1:1:1:1, and the details are not repeated here.

[0129] Example 12

[0130] This embodiment provides a lithium-sulfur battery positive electrode material. The preparation method of the lithium-sulfur battery positive electrode material is the same as that of Example 1, except that the MXene (Ti3C2) suspension is replaced by a MoC solution of equal concentration, and will not be repeated here.

[0131] Comparative Example 1

[0132] This comparative example provides a lithium-sulfur battery positive electrode material. The preparation method of the lithium-sulfur battery positive electrode material is the same as that of Example 1, except that only Na2WO4·2H2O is added as other metal salts and the molar ratio of selenium to other metal elements is maintained at 2:1, and will not be repeated here.

[0133] Comparative Example 2

[0134] This comparative example provides a lithium-sulfur battery positive electrode material. The preparation method of the lithium-sulfur battery positive electrode material is the same as that of Example 1, except that only Na2WO4·2H2O and NaMoO4·4H2O are added as other metal salts, and the molar ratio of selenium to other metal elements is maintained at 2:1, and will not be repeated here.

[0135] Comparative Example 3

[0136] This comparative example provides a lithium-sulfur battery positive electrode material. The preparation method of the lithium-sulfur battery positive electrode material is the same as that of Example 1, except that other metal salts are only added with C4H6CoO4·4H2O, Na2WO4·2H2O and NaMoO4·4H2O, and the molar ratio of selenium to other metal elements is maintained at 2:1, and no further details are given here.

[0137] Comparative Example 4

[0138] This comparative example provides a lithium-sulfur battery positive electrode material. The preparation method of the lithium-sulfur battery positive electrode material is the same as that of Example 1, except that other metal salts are only added with C4H6CoO4·4H2O, NH4VO3, Na2WO4·2H2O and NaMoO4·4H2O, and the molar ratio of selenium to other metal elements is maintained at 2:1, and no further details are given here.

[0139] Comparative Example 5

[0140] This comparative example provides a lithium-sulfur battery positive electrode material. The preparation method of the lithium-sulfur battery positive electrode material is the same as that of Example 1, except that the MXene (Ti3C2) suspension is not added, and will not be repeated here.

[0141] The positive electrode material of lithium-sulfur battery is prepared according to the conventional method, and the specific steps are as follows: sulfur / hexagonal high entropy selenide-graphene heterojunction nanomaterial, Ketjen black and PVDF are mixed in NMP solvent in a ratio of 8:1:1 to prepare slurry, the slurry is coated on carbon-coated aluminum foil, and dried in a vacuum oven at 60°C for 10 hours. After drying, it is cut into a circular pole piece with a diameter of 12 mm. The above-prepared sulfur / hexagonal high entropy selenide-MXene heterojunction material circular pole piece is used as the positive electrode, metallic lithium is used as the negative electrode, and the electrolyte is 1 molL -1LITFSI / DOL / DME with 2% LiNO3 and the performance was tested at a current density of 1C.

[0142] The 100-cycle curve diagram of the high entropy selenide-MXene heterojunction material provided in Example 1, Example 5, Comparative Example 1 and Comparative Example 3 is shown in Figure 5 ,from Figure 5 It can be seen that the high entropy selenide heterojunction materials prepared in Example 1 and Example 5 have better cycle performance, higher material structure stability, and higher coulombic efficiency and mass specific capacity.

[0143] The test results of the above embodiments and comparative examples are shown in Table 1.

[0144] Table 1

[0145]

[0146] From Table 1, we can see the following points:

[0147] (1) It can be seen from Examples 1 to 5 that the lithium-sulfur battery cathode material provided by the present invention can improve the stability of the material by compounding the high entropy selenide with MXene or graphene material, and improve the capacity stability and service life of the sulfur cathode, thereby improving the electrochemical performance of the lithium-sulfur battery. Specifically, the initial specific capacity is as high as 1120 mAh / g or more, the initial coulombic efficiency is as high as 99.1% or more, and the specific capacity after 100 cycles is above 1012 mAh / g;

[0148] (2) Combining Example 1 and Examples 8 to 9, it can be seen that the molar ratio of selenium to other metal elements in Example 1 is 2:1, compared with 2.5:1 and 1.5:1 in Examples 8 to 9, respectively. In Example 1, the initial specific capacity is 1205 mAh / g, the initial coulombic efficiency is as high as 99.6%, and the specific capacity after 100 cycles is 1048 mAh / g, while in Examples 8 to 9, the specific capacities after 100 cycles are only 710 mAh / g and 650 mAh / g, respectively. In addition, a small amount of V2Se5 peaks will appear in Example 8, and a small amount of Fe2Se3 peaks will appear in Example 9. This shows that the present invention controls the molar ratio of selenium to other metal elements within a specific range, which can better improve the structural stability of the positive electrode material;

[0149] (3) It can be seen from Example 1 and Example 10 that vacuum melting is performed after grinding in Example 1. Compared with Example 10 in which vacuum melting is not performed after grinding, the first specific capacity in Example 1 is 1205 mAh / g, the first coulombic efficiency is as high as 99.6%, and the specific capacity after 100 cycles is 1048 mAh / g, while the specific capacity after 100 cycles in Example 10 is only 620 mAh / g. In addition, the dispersibility of sulfur in the host material in Example 10 is reduced, resulting in a low effective utilization rate of sulfur and a lower cycle performance than that in Example 1. This shows that vacuum melting after grinding in the present invention can better improve the structural stability of the positive electrode material and can improve the specific capacity of the material;

[0150] (4) Combining Examples 1 and 11, it can be seen that in Example 1, the metal salts are mixed at a metal atomic molar ratio of 1:1:1:1:1:1, compared with the metal atomic molar ratio of 1.5:1:1:1:1:1:1 among C4H6CoO4·4H2O, NaMoO4·4H2O, Fe(CO2CH3)2, C6H9O6Cr, Na2WO4·2H2O and NH4VO3 salts in Example 11, the initial specific capacity in Example 1 is 1205 mAh / g, and the initial specific capacity is 1205 mAh / g. The catalytic efficiency is as high as 99.6%, and the specific capacity after 100 cycles is 1048 mAh / g, while the specific capacity after 100 cycles in Example 10 is only 620 mAh / g, and the synergistic effect in Example 11 is weakened, and the catalytic activity is weakened, resulting in the mass initial specific capacity of only 950 mAh / g, and the specific capacity after 100 cycles is only 608 mAh / g, which shows that the present invention controls the molar ratio between the elements within a specific range, which can better improve the specific capacity and cycle stability of the material;

[0151] (5) In Example 12, MoC is used. MoC is more easily oxidized to form MoO2 material during the synthesis of heterojunction materials, and its thermal stability is worse, resulting in a decrease in electrochemical performance compared with Example 1;

[0152] (6) In Comparative Examples 1 to 4, no high entropy alloy was formed, and the electrochemical performance was significantly worse than that of Example 1. In Comparative Example 5, no MXene (Ti3C2) suspension was added, which would cause serious agglomeration of high entropy selenide, resulting in a sharp decrease in the number of active sites and a significant decrease in electrochemical performance. This shows that the present invention significantly improves the electrochemical performance of the material by combining a high entropy alloy with a two-dimensional material.

[0153] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A lithium-sulfur battery positive electrode material, characterized in that: The lithium-sulfur battery positive electrode material comprises a high entropy selenide-two-dimensional material heterojunction nanomaterial and S; The two-dimensional material in the high entropy selenide-two-dimensional material heterojunction nanomaterial includes MXene and / or graphene; The high entropy selenide includes at least five other metal elements besides selenium; The molar ratio between any two of the other metal elements is 0.9-1.1:1; The other metal elements are a combination of Co, Mo, Fe, Cr, W and V, a combination of Co, Ni, Cr, Mn and Fe, a combination of Co, Mo, Fe, W and V or a combination of Co, Mo, Cr, W and V; The molar ratio of selenium to the sum of other metal elements in the high entropy selenide is (1.8-2.2):

1.

2. The lithium-sulfur battery positive electrode material according to claim 1, characterized in that The high entropy selenide in the high entropy selenide-two-dimensional material heterojunction nanomaterial is a hexagonal crystal structure and / or a cubic crystal structure; The high entropy selenide-two-dimensional material heterojunction nanomaterial is a nanosheet.

3. The lithium-sulfur battery positive electrode material according to claim 1 or 2, characterized in that: The content of high entropy selenide in the high entropy selenide-two-dimensional material heterojunction nanomaterial is 5-60wt%.

4. A method for preparing a lithium-sulfur battery positive electrode material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) mixing a suspension of a two-dimensional material, a selenium source, other metal element sources, and a reducing agent, and performing in-situ growth by microwave heating to obtain a first nanomaterial; the other metal element sources include at least five other metal elements; (2) The first nanomaterial of step (1) is subjected to the step of removing selenium powder and solvent to obtain the high entropy selenide-two-dimensional material heterojunction nanomaterial; (3) Mixing elemental sulfur and the high entropy selenide-two-dimensional material heterojunction nanomaterial described in step (2), and melting them in vacuum to obtain the lithium-sulfur battery positive electrode material.

5. The preparation method according to claim 4, characterized in that: The other metal element sources include at least five of a cobalt source, a molybdenum source, a nickel source, an iron source, a chromium source, a manganese source, a tungsten source or a vanadium source; The other metal element sources include other metal salts, and the other metal salts include at least five of cobalt salts, molybdenum salts, nickel salts, iron salts, chromium salts, manganese salts, tungsten salts or vanadium salts.

6. The preparation method according to claim 4, characterized in that: The reducing agent includes sodium borohydride and / or hydrazine hydrate; The molar ratio of the reducing agent to the selenium source is (1.5-3):1; The concentration of the suspension of the two-dimensional material is 3-10 g / L; The ratio of the two-dimensional material to the selenium source in the suspension of the two-dimensional material is (1-5):1; The two-dimensional material includes graphene and / or MXene; The MXene includes any one of Ti3C2, V2C, Nb2C or Mo2C or a combination of at least two thereof; The mass ratio of the elemental sulfur and the high entropy selenide-two-dimensional material heterojunction nanomaterial is (3-8):

2.

7. The preparation method according to claim 4, characterized in that: The microwave heating includes microwave solvothermal method and / or microwave hydrothermal method; The temperature of the vacuum melting is 150-180°C; The vacuum melting time is 10 to 14 hours.

8. A positive electrode, characterized in that The positive electrode comprises the lithium-sulfur battery positive electrode material according to any one of claims 1 to 3 or the lithium-sulfur battery positive electrode material prepared by the preparation method of the lithium-sulfur battery positive electrode material according to any one of claims 4 to 7.

9. A lithium-sulfur battery, characterized in that: The lithium-sulfur battery comprises the positive electrode according to claim 8.