One-time coating production method for back paint with a thickness of 14μm~15μm
By adjusting the viscosity and solid content of the back paint, combined with appropriate coating roller parameters and baking treatment, the thickness of the back paint of the cold-rolled color-coated coil plate has been successfully improved, solving the problems of uneven coating and insufficient adhesion. Improves productivity and adhesion.
Patent Information
- Application Number
- CN202411065620.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The thickness of the existing cold-rolled color-coated coiled plate back paint is difficult to reach 14μm~15μm, resulting in uneven coating, insufficient adhesion and low production efficiency.
By adjusting the paint viscosity and solid content of the back paint, combining appropriate diluents and coating roller parameters, a back paint coating machine is used to apply at one time to ensure that the back paint thickness reaches 14μm~15μm, and bake and cure in a curing furnace. .
A uniform coating of the back paint thickness is achieved, which reduces roller consumption and production costs, improves adhesion, and avoids coating peeling and uneven problems.
Smart Images

Figure CN118594895B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coating of cold-rolled color-coated coils and relates to a one-time coating production method for a coating with a back paint thickness of 14 μm to 15 μm. Background Art
[0002] During the production of cold-rolled color-coated coils, the following process steps will be taken: entrance stitching, cleaning, chemical coating, initial coating, initial coating curing, water quenching cooling, fine coating, fine coating curing, water quenching cooling again, coiling, packaging and warehousing.
[0003] The main function of the back paint is to protect the back side. The paint film is required to have good corrosion resistance, scratch resistance, adhesion resistance and processability, but the requirements for decoration and outdoor durability are not high. In addition, the difficulty in thick film coating production will cause defects such as uneven coating, so the conventional back paint film thickness is about 5μm. However, in special applications, customers have higher requirements for the corrosion resistance of color-coated plates, and the thickness of the back paint film needs to be increased. Too thick a paint film will cause the surface of the paint film to solidify while the bottom of the coating is insufficiently solidified, resulting in a phenomenon where the surface layer is dry and the lower layer is soft. And too thick a paint film will also produce internal shrinkage holes, causing paint cracking, peeling, and pinholes.
[0004] Most of the back coating of cold-rolled color-coated coils adopts a single coating, the film layer is thin and there is no support roller during the coating process. The cold-rolled color-coated coils are coated with the back coating by the weight of the coating roller and the rise of the coating roller, so that there is enough pressure between the two to complete the back coating. The conventional thickness of the back coating is 5μm~8μm. When the back coating is thickened, it is generally carried out by secondary coating (the back coating at this stage can only be coated with 5μm~8μm. When it exceeds 5μm~8μm, the paint attached to the plate will drip). The secondary coating has the problems of high roller consumption and high labor intensity of workers adding paint and cleaning paint trays. Moreover, in the secondary coating process, if the control is not proper, it may cause the problem of insufficient adhesion between the two coatings or uneven coating. Summary of the invention
[0005] In order to overcome the defects in the above-mentioned related technologies, the present invention proposes a one-time coating production method for a back paint coating with a thickness of 14μm~15μm, so as to complete the back paint coating operation with a thickness of 14μm~15μm for cold-rolled color-coated coils in one time.
[0006] To achieve the above technical purpose, the present invention provides a one-time coating production method for a back-painted coating with a thickness of 14 μm to 15 μm. The one-time coating production method for a back-painted coating with a thickness of 14 μm to 15 μm is applied to a galvanized or galvanized substrate.
[0007] The one-time coating production method of the back paint with a thickness of 14 μm to 15 μm comprises: obtaining a back paint with a paint viscosity of 118s to 138s and a solid content of 64% to 70%. Adding a diluent to the back paint and stirring, adjusting the paint viscosity of the back paint to 100s. Preparing a substrate to be coated with the back paint. The temperature of the substrate is 200° C. to 250° C.
[0008] A back paint coating operation is performed on the substrate using a back paint coating machine. The diameters of the coating roller and the feed roller of the back paint coating machine are 320 mm. The rotation speed of the coating roller is 1.45 to 1.50 times the running speed of the substrate, and the rotation speed of the feed roller of the back paint coating machine is 0.35 to 0.45 times the running speed of the substrate.
[0009] The substrate coated with the back paint is transported to the curing furnace, and the curing furnace bakes and cures the substrate to keep the temperature of the substrate at 225° C. The curing furnace bakes the substrate for 10 min to 15 min.
[0010] Preferably, the surface cleanliness grade of the substrate is Sa2.5, and the surface roughness of the substrate is Ra0.8~Ra1.2.
[0011] Preferably, the back paint comprises epoxy polyester, and the diluent comprises acetone or toluene.
[0012] Preferably, the feeding roller and the coating roller are both made of polyethylene rubber rollers.
[0013] Preferably, the pressure of the feeding roller and the coating roller is 800Pa~1300Pa.
[0014] The beneficial effects of the present invention are:
[0015] The present invention adjusts the viscosity of the back paint and the coating machine parameters to achieve the purpose of coating the cold-rolled color-coated coil with a thickness of 14 μm to 15 μm at one time, thereby reducing roller consumption, reducing the number of coating machines and employees involved, and reducing production costs.
[0016] The solid content of the back paint in the present invention is 64% to 70%, which is 20% higher than the solid content of the back paint with a thickness of about 5 μm, so as to form a thicker coating. The viscosity of the back paint is 100s, which can increase the thickness of the coating while satisfying the adhesion of the back paint to the substrate and avoiding the problem of the back paint falling off.
[0017] The diameter of the coating roller and the feeding roller of the present invention is 320 mm, and the rotation speed of the coating roller is 1.45 to 1.50 times the running speed of the substrate, which can increase the amount of paint transfer and increase the thickness of the applied coating. In addition, compared with the prior art, the coating roller in the present invention has an increased roller diameter, which can evenly apply pressure to the back paint to form a uniformly distributed coating.
[0018] The present invention can achieve the purpose of successfully coating the back paint of the cold-rolled color-coated coil with a thickness of 14μm to 15μm in one time by adjusting the back paint parameters (solid content of 64% to 70%, paint viscosity of 100s), coordinating the parameters of the back paint coating machine (coating roller diameter of 320mm, the rotation speed of the coating roller is 1.45 to 1.50 times the running speed of the substrate, the pressure of the coating roller is 800Pa to 1300Pa) and maintaining the temperature of the substrate at 200℃ to 250℃. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the drawings required for use in the embodiments or related technical descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0021] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0022] In the description of the present invention, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0023] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0024] Some embodiments of the present invention provide a one-time coating production method for a coating with a back paint thickness of 14 μm to 15 μm. The one-time coating production method for a coating with a back paint thickness of 14 μm to 15 μm is applied to a galvanized or galvanized substrate.
[0025] The one-time coating production method of the back paint coating with a thickness of 14 μm to 15 μm comprises:
[0026] S1. Obtain a back paint with a paint viscosity of 118s~138s and a solid content of 64%~70%.
[0027] S2, adding a diluent to the back paint and stirring, and adjusting the paint viscosity of the back paint to 100s.
[0028] S3, preparing a substrate to be coated with back paint, wherein the temperature of the substrate is 200°C to 250°C.
[0029] S4. Use a back paint coater to coat the substrate with back paint. The diameters of the coating roller and the feed roller of the back paint coater are 320 mm. The rotation speed of the coating roller is 1.45 to 1.50 times the running speed of the substrate. The rotation speed of the feed roller of the back paint coater is 0.35 to 0.45 times the running speed of the substrate.
[0030] S5. The substrate coated with the back paint is transported to the curing furnace. The curing furnace bakes and cures the substrate to keep the temperature of the substrate at 225° C. The curing furnace bakes the substrate for 10 min to 15 min.
[0031] Preferably, the surface cleanliness grade of the substrate is Sa2.5, and the surface roughness of the substrate is Ra0.8~Ra1.2.
[0032] Preferably, the back paint comprises epoxy polyester, and the diluent comprises acetone or toluene.
[0033] Preferably, the feeding roller and the coating roller are both made of polyethylene rubber rollers.
[0034] Preferably, the pressure of the feeding roller and the coating roller is 800Pa~1300Pa.
[0035] In some examples, a back paint having a paint viscosity of 128 s and a solid content of 67% was obtained, and toluene was added to the back paint and stirred to make the viscosity of the back paint 100 s.
[0036] Prepare a substrate, which is a galvanized plate with a surface roughness of Ra0.8 and a cleanliness level of Sa2.5. The temperature of the substrate is 218°C.
[0037] A back paint coating machine is used to coat the substrate with back paint. The diameters of the coating roller and the feeding roller of the back paint coating machine are 320 mm, the rotation speed of the coating roller is 1.45 times the running speed of the substrate, and the rotation speed of the feeding roller of the back paint coating machine is 0.35 times the running speed of the substrate; the pressures of the feeding roller and the coating roller are both 1000 Pa.
[0038] With the above operating parameters, the substrate can be coated with a back paint thickness of 14μm~15μm. After that, the substrate is transported to a curing furnace, and the temperature of the substrate is maintained at 225℃ in the curing furnace.
[0039] After testing, the back paint thickness formed by the above-mentioned back paint thickness 14μm~15μm coating one-time coating production method is 16.57μm, the back paint resistance is greater than 50, the T bending grade is 3T, and when the back paint thickness is 16.57μm, the bending resistance of the cold-rolled color-coated coil is consistent with the bending resistance of the cold-rolled color-coated coil with a back paint thickness of 8μm. Specifically, a 90° bending test was conducted on a cold-rolled color-coated coil with a substrate thickness of less than or equal to 0.75mm and a back paint thickness of 16.57μm, and a T-bending test was conducted on a cold-rolled color-coated coil with a substrate thickness of greater than or equal to 0.75mm and a back paint thickness of 16.57μm. The coating of the cold-rolled color-coated coil did not show cracking or peeling defects, and the paint did not fall off after the 3M tape was adhered.
[0040] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.
[0041] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A one-time coating production method for a back paint coating with a thickness of 14μm to 15μm, applied to a galvanized or galvanized substrate, characterized in that: The one-time coating production method of the back paint coating with a thickness of 14 μm to 15 μm comprises: Obtain a back paint with a paint viscosity of 118s~138s and a solid content of 64%~70%; Adding diluent to the back paint and stirring, adjusting the paint viscosity of the back paint to 100s; Preparing the substrate to be coated with back paint; The temperature of the substrate is 200°C to 250°C; The substrate is coated with back paint by a back paint coating machine, the diameter of the coating roller and the feed roller of the back paint coating machine is 320 mm, the rotation speed of the coating roller is 1.45 to 1.50 times the running speed of the substrate, and the rotation speed of the feed roller of the back paint coating machine is 0.35 to 0.45 times the running speed of the substrate; The substrate coated with the back paint is transported to a curing furnace, and the curing furnace bakes and cures the substrate, so that the temperature of the substrate is maintained at 225° C. The curing furnace bakes the substrate for 10 min to 15 min.
2. The one-time coating production method of a back paint coating with a thickness of 14 μm to 15 μm according to claim 1, characterized in that: The surface cleanliness grade of the substrate is Sa2.5, and the surface roughness of the substrate is Ra0.8~Ra1.
2.
3. The one-time coating production method of a back paint coating with a thickness of 14 μm to 15 μm according to claim 2, characterized in that: The back paint comprises epoxy polyester, and the diluent comprises acetone or toluene.
4. The one-time coating production method of a back paint coating with a thickness of 14 μm to 15 μm according to claim 3, characterized in that: The material raising roller and the coating roller are both polyethylene rubber rollers.
5. The one-time coating production method of a back paint coating with a thickness of 14 μm to 15 μm according to claim 4, characterized in that: The pressure of the feeding roller and the coating roller is 800Pa~1300Pa.