Plate and preparation method thereof
By using specific composition inorganic boards and multi-layer structural design in the board, the problem of insufficient moisture-proof and waterproof performance of existing boards is solved, and efficient moisture-proof and waterproof effect and cost reduction are achieved.
Patent Information
- Application Number
- CN202411080869.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The moisture-proof and waterproof performance of existing boards is low, making it difficult to meet the requirements of various application scenarios.
Inorganic sheets, which include plant fibers and inorganic materials, are specifically composed of magnesium sulfate, magnesium oxide, magnesium chloride and citric acid. Through a specific mass ratio design and process, a plate with a low water absorption thickness expansion rate is formed and on the surface. Multiple adhesive and toughening layers are provided to improve mechanical strength and flatness.
The high moisture-proof and waterproof performance of the board is achieved, which reduces the preparation cost and reduces the total cost of the board while ensuring performance.
Smart Images

Figure CN118598631B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of decoration materials, and in particular to a board material and a preparation method thereof. Background Art
[0002] Existing household or commercial floors have increasingly higher requirements for moisture-proof and waterproof properties of the panels, but the moisture-proof and waterproof properties of existing panels are still relatively low, making it difficult to meet the requirements of a variety of application scenarios. Summary of the invention
[0003] The embodiment of the present application provides a board material, which has good moisture-proof and waterproof properties and a low water absorption thickness expansion rate.
[0004] In a first aspect, an embodiment of the present application provides a plate, the plate comprising:
[0005] An inorganic board, the inorganic board includes plant fiber and inorganic material, in which the mass ratio of the inorganic material to the plant fiber ranges from 1.2 to 1.5, the raw material components of the inorganic material include magnesium sulfate and magnesium oxide, the mass ratio of the magnesium sulfate to the magnesium oxide ranges from 0.4 to 0.5; the raw material components of the inorganic material also include magnesium chloride and a modifier, the mass ratio of magnesium chloride to magnesium oxide ranges from 0.05 to 0.15; the modifier is citric acid; in the raw material components of the inorganic material, the mass ratio of the modifier to the magnesium chloride ranges from 0.025 to 0.045; the 24h water absorption thickness expansion rate of the inorganic board is less than or equal to 3%.
[0006] In some embodiments, the raw material components of the inorganic material include, by mass fraction, 2% to 6% of magnesium chloride, 17% to 23% of magnesium sulfate, and 40% to 48% of magnesium oxide.
[0007] In some embodiments, before the citric acid is added, the citric acid is first mixed with a portion of the magnesium sulfate to form a mixed solution, so that the mass ratio of the citric acid to the magnesium sulfate in the mixed solution is in the range of 20 to 66.
[0008] In some embodiments, the raw material components of the inorganic material include the following components in parts by weight:
[0009] 12 to 16 parts of magnesium chloride;
[0010] 68 to 75 parts of magnesium sulfate;
[0011] 150 to 170 parts of magnesium oxide;
[0012] 0.3 to 1.2 parts of a modifier; and
[0013] 110 to 120 parts of water.
[0014] In some embodiments, the density p of the inorganic plate is in the range of 1 mg / cm 3 ≤ρ≤1.5mg / cm 3 ; The 2h water absorption thickness expansion rate of the inorganic board is less than or equal to 2%; The fire protection level of the inorganic board is A2.
[0015] In some embodiments, the sheet further comprises:
[0016] a first adhesive layer, the first adhesive layer being disposed on a surface of the inorganic board;
[0017] A clamping plate, the clamping plate is arranged on a surface of the first adhesive layer away from the inorganic plate;
[0018] a second adhesive layer, the second adhesive layer being disposed on a surface of the splint facing away from the first adhesive layer; and
[0019] A back plate is arranged on a surface of the second adhesive layer facing away from the inorganic plate.
[0020] In some embodiments, the plywood includes multiple adhesive layers and multiple veneers, the adhesive layers and the veneers are alternately stacked in sequence, the fibers of one of two adjacent veneers extend along a first direction, and the fibers of the other extend along a second direction, wherein the first direction intersects with the second direction.
[0021] In some embodiments, the number of the inorganic boards is multiple layers, and the board also includes at least one toughening layer. The multiple inorganic boards and the toughening layers are alternately stacked in sequence to form an inorganic composite board, and the toughening layer is thin wood or non-woven fabric.
[0022] In some embodiments, the sheet further comprises:
[0023] a decorative layer, the decorative layer being disposed on one side of the inorganic board; and
[0024] A balancing layer is disposed on the other side of the inorganic board.
[0025] In a second aspect, an embodiment of the present application provides a method for preparing a plate, the method comprising:
[0026] Provide an inorganic gel and plant fiber, wherein the raw material components of the inorganic gel include magnesium chloride, magnesium sulfate and magnesium oxide;
[0027] Stirring and mixing the inorganic gel and the plant fiber to obtain a mixture; and
[0028] The mixture is laid, cold-pressed and dried in sequence to solidify the inorganic gel to form an inorganic material, and the inorganic board is obtained, wherein the board includes an inorganic board, in which the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, and the 24h water absorption thickness expansion rate of the inorganic board is less than or equal to 3%; the raw material components of the inorganic gel also include magnesium chloride and a modifier, and the mass ratio of magnesium chloride to magnesium oxide is in the range of 0.05 to 0.15; the modifier is citric acid; in the raw material components of the inorganic gel, the mass ratio of the modifier to the magnesium chloride is in the range of 0.025 to 0.045.
[0029] In some embodiments, the raw material components of the inorganic gel further include magnesium chloride and a modifier, and the providing of the inorganic gel includes:
[0030] Dissolving the magnesium chloride in water at room temperature;
[0031] Add magnesium sulfate, and stir at room temperature until the magnesium sulfate is completely dissolved; and
[0032] adding magnesium oxide and a modifier, and stirring at room temperature to allow magnesium chloride, magnesium sulfate and magnesium oxide to react to obtain the inorganic gel;
[0033] The providing of plant fiber comprises:
[0034] The plant fiber raw material is crushed to obtain plant fibers, wherein the plant fibers have a size ranging from 1.5 mm to 2.0 mm.
[0035] In some embodiments, the mixture is sequentially paved, cold-pressed and molded, and dried to solidify the inorganic gel to form an inorganic material, and the inorganic board is obtained, including:
[0036] The mixed material is laid on a pad to obtain a green body, and a plurality of the green bodies are stacked in sequence;
[0037] Cold-pressing and mold-locking the stacked green bodies to obtain a green body stack; and
[0038] The green body stack is dried at a temperature of 125° C. to 145° C. to obtain the inorganic board.
[0039] In some embodiments, the step of drying the green body stack at a temperature of 125° C. to 145° C. to obtain the inorganic board comprises:
[0040] Set the mold temperature controller so that the preset outlet temperature of the mold temperature controller is 160°C to 180°C and the preset reflow temperature is 125°C to 145°C;
[0041] When the reflux temperature of the mold temperature controller reaches the preset reflux temperature, placing the green body stack in the mold temperature controller;
[0042] In a first time period, the mold temperature controller is turned on every first time period, wherein the first time period includes a plurality of the first time periods;
[0043] In a second time period, the mold temperature controller is turned on every second sub-time period, wherein the second time period includes a plurality of second time lengths, the second time length is greater than the first time length, and the second time period is after the first time period; and
[0044] When the reflux temperature is 2° C. to 5° C. higher than the preset reflux temperature, the mold temperature controller is turned on to obtain the inorganic board.
[0045] In some embodiments, the preparation method further comprises:
[0046] Providing a clamping plate and a back plate, and forming a first adhesive layer and a second adhesive layer on two opposite surfaces of the clamping plate respectively;
[0047] Laying the inorganic plate on the surface of the first adhesive layer away from the clamping plate, and laying the back plate on the surface of the second adhesive layer away from the clamping plate;
[0048] Performing a first cold pressing at a pressure of 5kg / cm² to 7kg / cm²; and
[0049] The first hot pressing is performed at a pressure of 8kg / cm² to 13kg / cm² and a temperature of 115°C to 125°C, so that the first adhesive layer forms a first bonding layer and the second adhesive layer forms a second bonding layer; wherein, before the first hot pressing, the moisture content of the backplane is greater than the moisture content of the inorganic board.
[0050] In some embodiments, before the first hot pressing, the moisture content of the back panel is greater than that of the plywood, and the moisture content of the plywood is greater than that of the inorganic panel; the moisture content of the back panel ranges from 12% to 20%; the moisture content of the plywood ranges from 10% to 12%; the moisture content of the inorganic panel ranges from 4% to 7%.
[0051] In some embodiments, providing a splint comprises:
[0052] Provide adhesives and multi-layer veneers;
[0053] Applying adhesive on the surface of some of the multi-layer veneers, and stacking the multi-layer veneers in sequence;
[0054] At a pressure of 5kg / cm 2 Up to 7kg / cm 2 Performing a second cold pressing; and
[0055] At a pressure of 8kg / cm 2 Up to 13kg / cm 2 , a second hot pressing is performed at a temperature of 115°C to 125°C to solidify the adhesive to form an adhesive layer, and the plywood is obtained, wherein the plywood includes multiple layers of adhesive layers and multiple layers of veneers, the adhesive layers and the veneers are alternately stacked in sequence, the fibers of one of the two adjacent layers of veneers extend along a first direction, and the fibers of the other extend along a second direction, wherein the first direction intersects with the second direction.
[0056] The plate of the embodiment of the present application includes an inorganic plate, the inorganic plate includes plant fiber and inorganic material, in the inorganic plate, the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, the raw material components of the inorganic material include magnesium chloride, magnesium sulfate and magnesium oxide, and the 24h water absorption thickness expansion rate of the inorganic plate is less than or equal to 3%. In the embodiment of the present application, inorganic material is added to the inorganic plate, and the inorganic plate has a lower 24h water absorption thickness expansion rate through the design of the inorganic material component and the ratio of the inorganic material to the plant fiber; in addition, the plate of the present application includes an inorganic plate, the inorganic plate is made by pressing, and has a higher flatness, so that when the decorative layer is attached to the surface of the inorganic plate, it has a higher yield, improves the preparation yield of the plate, and reduces the preparation cost of the plate; furthermore, the inorganic plate can be used as the surface plate of the plate, and when the inorganic plate is used as the surface plate, the defect requirements for the single plate under the surface plate are reduced, and the cost of the plate can be better reduced while ensuring that the performance of the plate remains unchanged. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0058] Figure 1 It is a plan view of a plate according to an embodiment of the present application.
[0059] Figure 2 The plate of the first embodiment of the present application is along Figure 1 Schematic diagram of the cross-sectional structure in the AA direction.
[0060] Figure 3 The plate of the second embodiment of the present application is along Figure 1 Schematic diagram of the cross-sectional structure in the AA direction.
[0061] Figure 4 The splint edge of an embodiment of the present application Figure 1 Schematic diagram of the cross-sectional structure in the AA direction.
[0062] Figure 5 The plate of the third embodiment of the present application is along Figure 1 Schematic diagram of the cross-sectional structure in the AA direction.
[0063] Figure 6 The plate of the fourth embodiment of the present application is along Figure 1 Schematic diagram of the cross-sectional structure in the AA direction.
[0064] Figure 7 The plate of the fifth embodiment of the present application is along Figure 1 Schematic diagram of the cross-sectional structure in the AA direction.
[0065] Figure 8 The plate of the sixth embodiment of the present application is along Figure 1 Schematic diagram of the cross-sectional structure in the AA direction.
[0066] Fig. 9 The plate of the seventh embodiment of the present application is along Figure 1 Schematic diagram of the cross-sectional structure in the AA direction.
[0067] Fig.10 It is a schematic flow chart of a first method for preparing a plate according to an embodiment of the present application.
[0068] Fig.11 It is a schematic flow chart of a method for preparing an inorganic gel according to an embodiment of the present application.
[0069] Fig.12 It is a schematic flow chart of a second method for preparing the plate of an embodiment of the present application.
[0070] Fig.13 It is a schematic diagram of the drying process in the method for preparing a board material according to an embodiment of the present application.
[0071] Fig.14 It is a schematic flow chart of the third method for preparing the plate material of the embodiment of the present application.
[0072] Fig.15 It is a schematic flow chart of a method for preparing a splint according to an embodiment of the present application.
[0073] Fig.16 It is a schematic flow chart of the fourth method for preparing the plate material of the embodiment of the present application.
[0074] Fig.17 It is a schematic flow chart of the fifth method for preparing the plate material of the embodiment of the present application.
[0075] Fig.18 It is a schematic flow chart of the sixth method for preparing the plate material of the embodiment of the present application.
[0076] Description of reference numerals:
[0077] 100-plate material, 10-inorganic plate, 20-first adhesive layer, 30-plywood, 31-adhesive layer, 32-veneer, 40-second adhesive layer, 50-back plate, 60-toughening layer, 70-third adhesive layer, 80-decorative layer, 90-balancing layer, 91-fourth adhesive layer, 92-fifth adhesive layer. DETAILED DESCRIPTION
[0078] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0079] The terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices.
[0080] The technical solutions in the embodiments of the present application will be described below in conjunction with the accompanying drawings.
[0081] It should be noted that, for the convenience of explanation, in the embodiments of the present application, the same figure marks represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments.
[0082] Existing household or commercial floors have increasingly higher requirements for moisture-proof and waterproof properties of the panels, but the moisture-proof and waterproof properties of existing panels are still relatively low, making it difficult to meet the requirements of a variety of application scenarios.
[0083] The base material of relevant solid wood composite floor is usually multi-layer plywood, and the main raw materials are eucalyptus veneer, poplar veneer or miscellaneous wood veneer. When pasting 0.6mm veneer, the quality requirements for the surface veneer (referred to as the surface board) and the two layers of veneer under the surface board are relatively high. The surface board is generally required to be a whole beech veneer, without dead knots, cracks, no repairs, and a smooth surface. The two layers of veneer under the surface board are required to have no overlapping cores, no cracks, and repairs are smooth. Otherwise, after pasting the decorative layer, due to the quality defects of the veneer under the surface board, the floor board surface (such as the surface or decorative layer or balance layer) will show some quality problems, such as bulging, bubbling, stripe printing, etc.
[0084] See also Figure 1 and Figure 2 The embodiment of the present application provides a plate 100, which includes an inorganic plate 10, and the inorganic plate 10 includes plant fiber and inorganic material. In the inorganic plate 10, the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, and the raw material components of the inorganic material include magnesium sulfate (MgSO4) and magnesium oxide (MgO), and the mass ratio of the magnesium sulfate to the magnesium oxide is in the range of 0.4 to 0.5; the 24h (hour) water absorption thickness expansion rate of the inorganic plate 10 is less than or equal to 3%.
[0085] The board 100 of the embodiment of the present application can be applied to home or commercial floor, wall panel, furniture panel and other decoration board 100.
[0086] It should be noted that the board 100 of the present application may only include the inorganic board 10. In addition to the inorganic board 10, the board 100 of the present application may also include other wood veneers.
[0087] Optionally, the plant fiber may be, but is not limited to, at least one of wood fiber (such as wood powder), straw fiber (such as straw powder), etc. The straw fiber may include, but is not limited to, plant straws such as rice straw, wheat straw, and reed straw.
[0088] Specifically, the mass ratio of the inorganic material to the plant fiber may be, but is not limited to, 1.2, 1.23, 1.25, 1.28, 1.3, 1.33, 1.35, 1.38, 1.4, 1.44, 1.45, 1.48, 1.5, etc. If the mass ratio of the inorganic material to the plant fiber is too small, the amount of inorganic gel added is insufficient during the preparation of the inorganic board 10, and the plant fiber cannot be well bonded, resulting in insufficient internal bonding strength of the inorganic board 10, easy delamination, and reduced mechanical strength of the inorganic board 10; if the mass ratio of the inorganic material to the plant fiber is too large, the amount of inorganic material in the inorganic board 10 is too much, and the amount of plant fiber is too little, which increases the brittleness of the inorganic board 10 and reduces the impact strength of the inorganic board 10. When the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, the inorganic board 10 can have good internal bonding strength, is not prone to delamination, and has high toughness, thereby having good rigidity and impact resistance.
[0089] It should be noted that the inorganic material is formed by solidifying an inorganic gel, which is made of components such as magnesium sulfate (MgSO4) and magnesium oxide (MgO).
[0090] Among the raw material components of the inorganic material, magnesium sulfate can improve the water resistance and compressive strength of the inorganic gel. Magnesium oxide can improve the mechanical strength of the inorganic board 10. Through the compounding of magnesium sulfate and magnesium oxide, the inorganic gel can be better bonded with the plant fiber, and the inorganic board 10 has better water resistance and mechanical strength such as compressive strength and impact strength.
[0091] It can be understood that, in the raw material components of the inorganic gel, the mass ratio of the magnesium sulfate to the magnesium oxide is in the range of 0.4 to 0.5.
[0092] Specifically, in the raw material components of the inorganic material, the mass ratio of the magnesium sulfate to the magnesium oxide may be, but is not limited to, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, etc. If the mass ratio of the magnesium sulfate to the magnesium oxide is too low, the content of the magnesium sulfate is too little and the content of the magnesium oxide is too much; if the content of the magnesium sulfate is too little, the water resistance and compressive strength of the inorganic board 10 are reduced; if the content of the magnesium oxide is too much, when the magnesium oxide is hydrated, more magnesium hydroxide (Mg(OH)2 colloid) colloid is formed in a short time, which increases the alkalinity of the inorganic gel and aggravates the moisture absorption and halogen return of the inorganic board 10. If the mass ratio of the magnesium sulfate to the magnesium oxide is too high, the content of magnesium sulfate is too high and the content of magnesium oxide is too low; if the content of magnesium sulfate is too high, the strength of the inorganic board 10 is reduced, the inorganic board 10 becomes brittle, and the impact strength is reduced, which is not conducive to the application of the inorganic board 10; if the content of magnesium oxide is too low, the magnesium oxychloride formed in the inorganic gel is less gelled, and in addition, magnesium chloride will be excessive, and chloride ions will exist in the inorganic board 10 in a free form, making the inorganic board 10 easy to absorb moisture and return to brine or water, thereby reducing the moisture-proof performance of the inorganic board 10.
[0093] Specifically, the 24h water absorption thickness expansion rate of the inorganic board 10 may be, but is not limited to, less than or equal to 3%, less than or equal to 2.8%, less than or equal to 2.6%, less than or equal to 2.4%, less than or equal to 2.2%, less than or equal to 2.0%, less than or equal to 1.8%, etc. For example, the 24h water absorption thickness expansion rate of the inorganic board 10 may be, but is not limited to, 3%, 2.8%, 2.6%, 2.4%, 2.2%, 2.0%, 1.8%, 1.5%, etc. The inorganic board 10 of the embodiment of the present application has a lower 24h water absorption thickness expansion rate and has better moisture-proof and waterproof properties.
[0094] The plate 100 of the embodiment of the present application includes an inorganic plate 10, which includes plant fibers and inorganic materials. In the inorganic plate 10, the mass ratio of the inorganic material to the plant fibers is in the range of 1.2 to 1.5, and the raw material components of the inorganic material include magnesium sulfate and magnesium oxide. The 24h water absorption thickness expansion rate of the inorganic plate 10 is less than or equal to 3%. In an embodiment of the present application, inorganic materials are added to the inorganic board 10, and the inorganic material components are designed as well as the ratio of the inorganic material to the plant fiber, so that the inorganic board 10 has a lower 24h water absorption thickness expansion rate; in addition, the board 100 of the present application includes the inorganic board 10, and the inorganic board 10 is made by pressing and has a higher flatness, so that when a decorative layer is affixed to the surface of the inorganic board 10, it has a higher yield, thereby improving the preparation yield of the board 100 and reducing the preparation cost of the board 100; furthermore, the inorganic board 10 can be used as the surface board of the board 100, and when the inorganic board 10 is used as the surface board, the defect requirements for the single board under the surface board are reduced, and the cost of the board 100 can be better reduced while ensuring that the performance of the board 100 remains unchanged.
[0095] In some embodiments, the raw material components of the inorganic material also include magnesium chloride (MgCl2). Magnesium chloride can increase the adhesion of the inorganic gel, thereby improving the bonding strength between the inorganic gel and the plant fiber; in addition, magnesium chloride can make the inorganic board 10 more water-resistant and less prone to deformation or decay; furthermore, adding magnesium chloride to the inorganic gel can promote the curing speed of the inorganic gel, thereby improving the surface hardness of the inorganic board 10.
[0096] In some embodiments, the mass ratio of magnesium chloride to magnesium oxide in the raw material components of the inorganic material is in the range of 0.05 to 0.15. In other words, the mass ratio of magnesium chloride to magnesium oxide in the raw material components of the inorganic gel is in the range of 0.05 to 0.15.
[0097] Specifically, in the raw material components of the inorganic material, the mass ratio of magnesium chloride to magnesium oxide can be, but is not limited to, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, etc. In the raw material components of the inorganic material, if the mass ratio of magnesium chloride to magnesium oxide is too small, the content of magnesium chloride in the raw material components of the inorganic material is too little, and the content of magnesium oxide is too much; if the content of magnesium chloride is too low, the bonding strength of the inorganic gel will be reduced, thereby reducing the bonding strength between the inorganic gel and the plant fiber, which is not conducive to improving the hardness and mechanical strength of the inorganic board 10; if the content of magnesium oxide is too high, when magnesium oxide is hydrated, more magnesium hydroxide (Mg(OH)2 colloid) colloid is formed in a short time, which increases the alkalinity of the inorganic gel, prevents the normal progress of the magnesium oxychloride gelling material, and makes magnesium chloride exist in the form of MgCl2•6H2O, which will also aggravate the moisture absorption and halogen return of the inorganic board 10. If the mass ratio of magnesium chloride to magnesium oxide in the raw material components of the inorganic material is too large, the content of magnesium chloride in the raw material components of the inorganic material will be too high and the content of magnesium oxide will be too low; if the content of magnesium chloride is too high, the inorganic board 10 will be prone to deformation and cracking; if the content of magnesium oxide is too low, the magnesium oxychloride formed in the inorganic gel will be less gelled, and in addition, magnesium chloride will be excessive, and chloride ions will exist in the inorganic board 10 in a free form, making the inorganic board 10 prone to moisture absorption and halogen absorption or water absorption, thereby reducing the moisture-proof performance of the inorganic board 10.
[0098] In some embodiments, the raw material components of the inorganic material include, by mass fraction, 2% to 6% magnesium chloride, 17% to 23% magnesium sulfate, and 40% to 48% magnesium oxide, with the remainder being water. In other words, the raw material components of the inorganic gel include, by mass fraction, 2% to 6% magnesium chloride, 17% to 23% magnesium sulfate, and 40% to 48% magnesium oxide, with the remainder being water.
[0099] Specifically, in the raw material components of the inorganic material, the mass fraction of the magnesium chloride may be, but is not limited to, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, etc. In the raw material components of the inorganic material, if the mass fraction of the magnesium chloride is too low, the bonding strength of the inorganic gel is reduced, thereby reducing the bonding force between the inorganic gel and the plant fiber, which is not conducive to improving the hardness and mechanical strength of the inorganic board 10; in the raw material components of the inorganic material, if the mass fraction of the magnesium chloride is too high, the inorganic board 10 is prone to deformation and cracking, thereby reducing the preparation yield of the inorganic board 10. When the mass fraction of the magnesium chloride in the raw material components of the inorganic material is in the range of 2% to 6%, the inorganic board 10 can have higher hardness and mechanical strength, and is not prone to cracking.
[0100] Furthermore, in the raw material components of the inorganic material, the mass fraction of the magnesium chloride is in the range of 2% to 4%. This allows the inorganic plate 10 to have higher hardness and mechanical strength and is less prone to cracking.
[0101] Specifically, in the raw material components of the inorganic material, the mass fraction of the magnesium sulfate may be, but is not limited to, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, etc. In the raw material components of the inorganic material, if the mass fraction of the magnesium sulfate is too low, the water resistance and compressive strength of the inorganic board 10 are reduced; in the raw material components of the inorganic material, if the mass fraction of the magnesium sulfate is too high, the strength of the inorganic board 10 is reduced, the inorganic board 10 becomes brittle, and the impact strength is reduced, which is not conducive to the application of the inorganic board 10. When the mass fraction of the magnesium sulfate in the raw material components of the inorganic material is 17% to 23%, the inorganic board 10 can have better water resistance, compressive strength and impact strength.
[0102] Furthermore, in the raw material components of the inorganic material, the mass fraction of the magnesium sulfate is 18% to 20%. This can make the inorganic board 10 have better water resistance, compressive strength and impact strength.
[0103] Specifically, in the raw material components of the inorganic material, the mass fraction of the magnesium oxide may be, but is not limited to, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, etc. In the raw material components of the inorganic material, if the content of magnesium oxide is too low, the magnesium oxychloride formed in the inorganic gel will be less gelled, and in addition, the magnesium chloride will be excessive, and the chloride ions will exist in the inorganic board 10 in a free form, making the inorganic board 10 easy to absorb moisture and return to halogen or absorb water and return to moisture, thereby reducing the moisture-proof performance of the inorganic board 10; in the raw material components of the inorganic material; if the content of magnesium oxide is too high, when magnesium oxide is hydrated, more magnesium hydroxide (Mg(OH)2 colloid) colloid will be formed in a short time, which will increase the alkalinity of the inorganic gel, prevent the normal progress of the magnesium oxychloride gelling material, and make the magnesium chloride exist in the form of MgCl2•6H2O, which will also aggravate the moisture absorption and return to halogen of the inorganic board 10. When the mass fraction of the magnesium oxide in the raw material components of the inorganic material is 40% to 48%, the inorganic board 10 can have better moisture-proof and waterproof properties, and can better prevent the inorganic board 10 from absorbing moisture and returning to halogen.
[0104] Furthermore, in the raw material components of the inorganic material, the mass fraction of the magnesium oxide is 42% to 44%. This can make the inorganic board 10 have better moisture-proof and waterproof properties, and can better prevent the inorganic board 10 from absorbing moisture and returning to halogen.
[0105] In a specific embodiment, the raw material components of the inorganic material include, by mass fraction, 2% to 4% magnesium chloride, 18% to 20% magnesium sulfate, and 42% to 44% magnesium oxide. In this way, the inorganic board 10 can have good moisture and water resistance, high water resistance, compressive strength, and impact resistance.
[0106] In some embodiments, the raw material component of the inorganic material further includes a modifier, and the modifier is citric acid; in the raw material component of the inorganic material, the mass ratio of the modifier to the magnesium chloride ranges from 0.025 to 0.045.
[0107] Specifically, in the raw material components of the inorganic material, the mass ratio of the modifier to the magnesium chloride can be, but is not limited to, 0.025, 0.028, 0.030, 0.033, 0.035, 0.038, 0.040, 0.043, 0.045, etc. In the raw material components of the inorganic material, if the mass ratio of the modifier to the magnesium chloride is too small, the content of the modifier is too little, the degree of the reaction of the magnesium chloride is limited, and the performance of the inorganic board 10 in reducing moisture absorption and halogen return is reduced; if the mass ratio of the modifier to the magnesium chloride is too large, the content of the modifier is too high, and the thermal stability of the formed inorganic gel is reduced.
[0108] In this embodiment, by adding a modifier to the raw material components of the inorganic material, the modifier can increase the reaction degree of magnesium chloride in the raw material components of the inorganic material, allowing the magnesium chloride to react more fully with magnesium sulfate and magnesium oxide, reducing the content of free chloride ions, and better reducing the probability of the inorganic board 10 absorbing moisture and returning to halogen.
[0109] In some embodiments, before the citric acid is added, the citric acid is first mixed with a portion of the magnesium sulfate to form a mixed solution, so that the mass ratio of the citric acid to the magnesium sulfate in the mixed solution is in the range of 20 to 66.
[0110] Specifically, the mass ratio of the citric acid to the magnesium sulfate in the mixed solution may be, but is not limited to, 20, 25, 30, 35, 40, 45, 50, 55, 60, 63, 66, etc. If the mass ratio of the citric acid to the magnesium sulfate is too high, the content of the citric acid is too high, which will reduce the reaction rate of the modifier; if the mass ratio of the citric acid to the magnesium sulfate is too low, the content of the magnesium sulfate is too high, which will reduce the strength of the inorganic board 10.
[0111] In some embodiments, the mixed solution includes, by mass fraction, 30% to 33% citric acid, 0.5% to 1.5% magnesium sulfate, and the remainder water. Specifically, the mass fraction of citric acid in the mixed solution may be, but not limited to, 30%, 31%, 32%, 33%, etc.; the mass fraction of magnesium sulfate may be, but not limited to, 0.5%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.5%, etc.
[0112] In some embodiments, the raw material components of the inorganic material include the following components in parts by weight:
[0113] 12 to 16 parts of magnesium chloride;
[0114] 68 to 75 parts of magnesium sulfate;
[0115] 150 to 170 parts of magnesium oxide;
[0116] 0.3 to 1.2 parts of a modifier; and
[0117] 110 to 120 parts of water.
[0118] In this embodiment, when the raw material components of the inorganic material include 12 to 16 parts of magnesium chloride; 68 to 75 parts of magnesium sulfate; 150 to 170 parts of magnesium oxide; 0.3 to 1.2 parts of a modifier; and 110 to 120 parts of water, the formed inorganic gel has better bonding properties with the plant fiber, which can better improve the internal bonding strength of the inorganic board 10, making the inorganic board 10 less prone to stratification; in addition, the toughness and mechanical strength of the inorganic board 10 can be better improved, so that the inorganic board 10 has good rigidity and good impact strength.
[0119] In a specific embodiment, the raw material components of the inorganic material include, by weight: 14 parts of magnesium chloride, 71.8 parts of magnesium sulfate, 160 parts of magnesium oxide, 0.5 parts of a modifier, and 116.8 parts of water. When the inorganic gel prepared by this raw material component is used to prepare the inorganic board 10, the inorganic gel and the plant fiber can have better bonding properties, and the internal bonding strength of the inorganic board 10 can be better improved, making the inorganic board 10 less prone to stratification; in addition, the toughness and mechanical strength of the inorganic board 10 can be better improved, so that the inorganic board 10 has good rigidity and good impact strength. In addition, the inorganic board 10 prepared by the ratio of the inorganic filler is less likely to have moisture regurgitation, condensation of water droplets, etc. in a high temperature and high humidity environment, and has a lower 24h water absorption thickness expansion rate.
[0120] In some embodiments, the density ρ of the inorganic plate 10 is in the range of 1 mg / cm 3 ≤ρ≤1.5mg / cm3 Specifically, the density ρ of the inorganic plate 10 may be, but is not limited to, 1.1 mg / cm 3 , 1.2mg / cm 3 , 1.3mg / cm 3 , 1.4mg / cm 3 , 1.5mg / cm 3 The inorganic board 10 of the present application has a relatively small density, and can be applied to the board 100 to make the board 100 have a relatively light weight.
[0121] Optionally, the fireproof grade of the inorganic board 10 is A2. The inorganic board 10 of the present application has a higher fireproof grade, so that the board 100 has a higher fireproof property.
[0122] Optionally, the 2h water absorption thickness expansion rate of the inorganic board 10 is less than or equal to 2%. Specifically, the 2h water absorption thickness expansion rate of the inorganic board 10 can be, but not limited to, 2%, 1.8%, 1.6%, 1.4%, 1.2%, 1.0%, 0.8%, 0.5%, 0.3%, etc. The inorganic board 10 of the embodiment of the present application has a lower 2h water absorption thickness expansion rate and has better moisture-proof and waterproof properties.
[0123] Optionally, the moisture content of the inorganic board 10 is 4% to 7%. Specifically, the moisture content of the inorganic board 10 may be, but is not limited to, 4%, 4.2%, 4.4%, 4.6%, 4.8%, 5%, 5.2%, 5.4%, 5.6%, 5.8%, 6%, 6.2%, 6.4%, 6.6%, 6.8%, 7%, etc. The inorganic board 10 of the present application has a lower moisture content, and when used as a surface board and hot-pressed with other single boards or composite boards, it is less prone to water loss and shrinkage, so that the obtained board 100 is more likely to warp to one side.
[0124] Optionally, the internal bonding strength of the inorganic board 10 is 1.25 MPa to 1.5 MPa. Specifically, the internal bonding strength of the inorganic board 10 may be, but is not limited to, 1.25 MPa, 1.28 MPa, 1.3 MPa, 1.32 MPa, 1.35 MPa, 1.38 MPa, 1.4 MPa, 1.42 MPa, 1.45 MPa, 1.48 MPa, 1.5 MPa, etc. The inorganic board 10 of the embodiment of the present application has a higher internal bonding strength, thereby having higher mechanical strength and hardness, and having a longer service life.
[0125] Optionally, the surface bonding strength of the inorganic board 10 is 1.08 MPa to 1.2 MPa. Specifically, the surface bonding strength of the inorganic board 10 may be, but is not limited to, 1.08 MPa, 1.1 MPa, 1.12 MPa, 1.15 MPa, 1.18 MPa, 1.2 MPa, etc. The inorganic board 10 of the embodiment of the present application has a higher surface bonding strength, thereby having higher mechanical strength and hardness, and having a longer service life.
[0126] See also Figure 3 In some embodiments, the plate material 100 further includes a first adhesive layer 20, which is disposed on the surface of the inorganic board 10; a plywood 30, which is disposed on the surface of the first adhesive layer 20 facing away from the inorganic board 10; a second adhesive layer 40, which is disposed on the surface of the plywood 30 facing away from the first adhesive layer 20; and a back panel 50, which is disposed on the surface of the second adhesive layer 40 facing away from the inorganic board 10.
[0127] It can be understood that in this embodiment, the board 100 includes a back board 50 , a second adhesive layer 40 , a sandwich board 30 , a first adhesive layer 20 and an inorganic board 10 which are stacked in sequence.
[0128] Optionally, the material of the first adhesive layer 20 is formed by curing a first adhesive, and the first adhesive includes melamine-modified urea glue and flour.
[0129] Optionally, the mass fraction of the flour in the first adhesive ranges from 40% to 50%. Specifically, the mass fraction of the flour in the first adhesive may be, but is not limited to, 40%, 42%, 44%, 46%, 48%, 50%, etc. If the mass fraction of the flour in the first adhesive is too low, the leveling property of the first adhesive is insufficient, which reduces the roller coating processing performance of the first adhesive; if the mass fraction of the flour in the first adhesive is too high, the first adhesive is too viscous, which is not easy to apply, and the adhesion of the first adhesive is reduced.
[0130] Optionally, the mass fraction of the melamine-modified urea glue in the first adhesive ranges from 50% to 60%. Specifically, the mass fraction of the melamine-modified urea glue in the first adhesive may be, but is not limited to, 50%, 52%, 55%, 56%, 58%, 60%, etc. If the mass fraction of the melamine-modified urea glue in the first adhesive is too small, the first adhesive is too viscous, not easy to apply, and the adhesion of the first adhesive is reduced; if the mass fraction of the melamine-modified urea glue in the first adhesive is too large, the leveling property of the first adhesive is insufficient, and the roller coating processing performance of the first adhesive is reduced.
[0131] Optionally, the material of the second adhesive layer 40 is formed by curing a second adhesive, and the second adhesive includes melamine-modified urea glue and flour.
[0132] Optionally, the mass fraction of the flour in the second adhesive is in the range of 40% to 50%. Specifically, the mass fraction of the flour in the second adhesive may be, but is not limited to, 40%, 42%, 44%, 46%, 48%, 50%, etc. If the mass fraction of the flour in the second adhesive is too low, the leveling property of the second adhesive is insufficient, which reduces the roller coating processing performance of the second adhesive; if the mass fraction of the flour in the second adhesive is too high, the second adhesive is too viscous, which is not easy to apply, and the adhesive force of the second adhesive is reduced.
[0133] Optionally, the mass fraction of the melamine-modified urea glue in the second adhesive is in the range of 50% to 60%. Specifically, the mass fraction of the melamine-modified urea glue in the second adhesive may be, but is not limited to, 50%, 52%, 55%, 56%, 58%, 60%, etc. If the mass fraction of the melamine-modified urea glue in the second adhesive is too small, the second adhesive is too viscous, not easy to apply, and the adhesion of the second adhesive is reduced; if the mass fraction of the melamine-modified urea glue in the second adhesive is too large, the leveling property of the second adhesive is insufficient, and the roller coating processing performance of the second adhesive is reduced.
[0134] Optionally, the backboard 50 may be, but is not limited to, a eucalyptus veneer. In a specific embodiment, the backboard 50 is a eucalyptus veneer with a thickness of 1.7 mm.
[0135] When preparing the plate 100 of the present embodiment, the inorganic plate 10, the first adhesive layer forming the first adhesive layer 20, the plywood 30, the second adhesive layer forming the second adhesive layer 40, and the back plate 50 are stacked in sequence, and after hot pressing, the plate 100 having the back plate 50, the second adhesive layer 40, the plywood 30, the first adhesive layer 20, and the inorganic plate 10 stacked in sequence is obtained. When the inorganic plate 10, the first adhesive layer forming the first adhesive layer 20, the plywood 30, the second adhesive layer forming the second adhesive layer 40, and the back plate 50 are compounded by hot pressing, the inorganic plate 10 has the phenomenon of water loss and shrinkage. Due to the high density of the inorganic plate 10, after the inorganic plate 10 shrinks, the plate 100 is easy to warp or bend to one side of the inorganic plate 10. The back plate 50 is arranged on the side of the plywood 30 away from the inorganic plate 10, which can balance the tension generated by the shrinkage of the inorganic plate 10, thereby making the plate 100 more straight.
[0136] See also Figure 4In some embodiments, the splint 30 includes multiple adhesive layers 31 and multiple single sheets 32, wherein the adhesive layers 31 and the single sheets 32 are alternately stacked in sequence, and the fibers of one of the two adjacent single sheets 32 extend along a first direction, and the fibers of the other extend along a second direction, wherein the first direction intersects the second direction. In this embodiment, by arranging the fiber directions of any two adjacent single sheets 32 in a crisscross pattern, the splint 30 is less prone to deformation and bending after hot pressing, and has a higher flatness.
[0137] Optionally, the number of the adhesive layers 31 may be two, three, four, five, six, etc. The number of the single boards 32 may be two, three, four, five, six, etc. The number of the adhesive layers 31 and the single boards 32 is not specifically limited in this application.
[0138] Optionally, the number of the adhesive layers 31 is one layer less than the number of the single boards 32 .
[0139] Optionally, the veneer 32 may be, but is not limited to, at least one of a eucalyptus veneer, a poplar veneer, or a miscellaneous wood veneer, etc. In a specific example, the veneer 32 is a 1.7 mm thick eucalyptus veneer.
[0140] In one embodiment, the first direction is perpendicular to the second direction.
[0141] Optionally, the material of the bonding layer 31 is formed by curing an adhesive, and the adhesive includes melamine-modified urea glue and flour.
[0142] Optionally, the mass fraction of the flour in the adhesive is in the range of 40% to 50%. Specifically, the mass fraction of the flour in the adhesive may be, but is not limited to, 40%, 42%, 44%, 46%, 48%, 50%, etc. If the mass fraction of the flour in the adhesive is too low, the leveling property of the adhesive is insufficient, which reduces the roller coating processing performance of the adhesive; if the mass fraction of the flour in the adhesive is too high, the adhesive is too viscous, which is not easy to construct, and the adhesive force of the adhesive is reduced.
[0143] Optionally, the mass fraction of the melamine-modified urea glue in the adhesive is in the range of 50% to 60%. Specifically, the mass fraction of the melamine-modified urea glue in the adhesive may be, but is not limited to, 50%, 52%, 55%, 56%, 58%, 60%, etc. If the mass fraction of the melamine-modified urea glue in the adhesive is too small, the adhesive is too viscous, not easy to apply, and the adhesive force of the adhesive is reduced; if the mass fraction of the melamine-modified urea glue in the adhesive is too large, the leveling property of the adhesive is insufficient, and the roller coating processing performance of the adhesive is reduced.
[0144] Optionally, the splint 30 includes three adhesive layers 31 and four single boards 32 , the single boards 32 and the adhesive layers 31 are alternately stacked in sequence, and the four single boards 32 are connected as a whole through the three adhesive layers 31 .
[0145] See also Figure 5 In some embodiments, the number of the inorganic boards 10 is multiple layers, and the board 100 further includes at least one toughening layer 60. The multiple inorganic boards 10 and the toughening layers 60 are alternately stacked in sequence to form an inorganic composite board 10a, and the toughening layer 60 is thin wood (such as Okoume) or non-woven fabric. In this embodiment, the inorganic composite board 10a is formed by stacking multiple inorganic boards 10, which can better improve the mechanical strength of the board 100. At the same time, the toughening layer 60 is arranged between two adjacent inorganic boards 10, which can reduce the brittleness of the board 100 and improve the toughness of the board 100.
[0146] Optionally, the thickness of the toughening layer 60 may be 0.3 mm to 0.5 mm. Specifically, the thickness of the toughening layer 60 may be, but is not limited to, 0.3 mm, 0.4 mm, 0.5 mm, etc.
[0147] Optionally, the plate 100 further includes a third adhesive layer 70, which is disposed between the inorganic plate 10 and the toughening layer 60, and is used to bond the inorganic plate 10 to the toughening layer 60. In a specific embodiment, the number of inorganic plates 10 in the inorganic composite plate 10a is two, the number of toughening layers 60 is one, and the number of third adhesive layers 70 is two. The inorganic composite plate 10a includes the inorganic plate 10, the third adhesive layer 70, the toughening layer 60, the third adhesive layer 70, and the inorganic plate 10, which are sequentially stacked.
[0148] Optionally, the material of the third adhesive layer 70 is formed by curing a third adhesive, wherein the third adhesive includes phenolic resin glue and flour.
[0149] Optionally, the mass fraction of the flour in the third adhesive is in the range of 20% to 28%. Specifically, the mass fraction of the flour in the third adhesive may be, but not limited to, 20%, 22%, 24%, 26%, 28%, etc. If the mass fraction of the flour in the third adhesive is too low, the leveling property of the third adhesive is insufficient, which reduces the roller coating processing performance of the third adhesive; if the mass fraction of the flour in the third adhesive is too high, the third adhesive is too viscous, which is not easy to apply, and reduces the adhesion of the third adhesive. Optionally, the mass fraction of the phenolic resin glue in the third adhesive is in the range of 72% to 80%. Specifically, the mass fraction of the phenolic resin glue in the third adhesive may be, but not limited to, 72%, 74%, 76%, 78%, etc. If the mass fraction of the phenolic resin glue in the third adhesive is too small, the third adhesive will be too viscous and difficult to apply, and the adhesion of the third adhesive will be reduced; if the mass fraction of the phenolic resin glue in the third adhesive is too large, the leveling property of the third adhesive will be insufficient, and the roller coating processing performance of the third adhesive will be reduced.
[0150] See also Figure 6 and Figure 7 In some embodiments, the board 100 further includes: a decorative layer 80, which is disposed on one side of the inorganic board 10; and a balancing layer 90, which is disposed on the other side of the inorganic board 10. In this embodiment, by disposing the decorative layer 80 on one side of the inorganic board 10 and the balancing layer 90 on the other side of the inorganic board 10, the board 100 can have a better appearance.
[0151] It should be noted that, “disposed on one side of a certain film layer” in the present application can be disposed on the surface of the film layer; or it can be disposed opposite to and spaced from the film layer, with other film layers disposed between the film layer.
[0152] It can be understood that the decoration layer 80 and the balance layer 90 are disposed on two opposite sides of the inorganic board 10. The decoration layer 80 and the balance layer 90 are respectively used as the outermost layers on two opposite sides of the board 100.
[0153] Optionally, the decorative layer 80 may be, but is not limited to, at least one of natural veneer, impregnated paper, luxury vinyl tile (LVT) or terephthalic acid and ethylene glycol layer (PET).
[0154] Optionally, the balancing layer 90 may be, but is not limited to, at least one of veneer, balancing paper, LVT, PET, etc. Optionally, the veneer may be, but is not limited to, natural veneer or technical wood, etc.
[0155] In one embodiment, when the decoration layer 80 is impregnated paper and the balancing layer 90 is balancing paper, the decoration layer 80 and the balancing layer 90 are directly bonded together by a hot pressing process without using an adhesive.
[0156] See also Figure 8 and Fig. 9 In other embodiments, when the decorative layer 80 is at least one of natural veneer, LVT, and PET, and the balancing layer 90 is at least one of veneer, LVT, or PET, the board 100 also includes a fourth adhesive layer 91 and a fifth adhesive layer 92, the fourth adhesive layer 91 is used to adhere the decorative layer 80 to one side of the inorganic board 10 or the inorganic composite board 10a, and the fifth adhesive layer 92 is used to adhere the balancing layer 90 to the other side of the inorganic board 10 or the inorganic composite board 10a.
[0157] It can be understood that in some embodiments, the plate 100 includes a balancing layer 90, a fifth adhesive layer 92, an inorganic plate 10, a fourth adhesive layer 91 and a decorative layer 80 which are stacked in sequence. Figure 8 In some other embodiments, the board 100 includes a balancing layer 90, a fifth adhesive layer 92, a back plate 50, a second adhesive layer 40, a plywood 30, a first adhesive layer 20, an inorganic board 10, a fourth adhesive layer 91 and a decorative layer 80 stacked in sequence. In some other embodiments, the board 100 includes a balancing layer 90, a fifth adhesive layer 92, an inorganic composite board 10a, a fourth adhesive layer 91 and a decorative layer 80 stacked in sequence, as shown. Fig. 9 In some other embodiments, the board 100 includes a balancing layer 90, a fifth adhesive layer 92, a back plate 50, a second adhesive layer 40, a sandwich plate 30, a first adhesive layer 20, an inorganic composite board 10a, a fourth adhesive layer 91 and a decorative layer 80 which are stacked in sequence.
[0158] Optionally, the fourth adhesive layer 91 is made of a material formed by curing a fourth adhesive.
[0159] Optionally, when the decorative layer 80 is natural veneer, the fourth adhesive includes melamine-modified urea glue and flour. Optionally, the mass fraction of the flour in the fourth adhesive ranges from 20% to 28%. Specifically, the mass fraction of the flour in the fourth adhesive may be, but not limited to, 20%, 22%, 24%, 26%, 28%, etc. If the mass fraction of the flour in the fourth adhesive is too low, the leveling property of the fourth adhesive is insufficient, which reduces the roller coating processing performance of the fourth adhesive; if the mass fraction of the flour in the fourth adhesive is too high, the fourth adhesive is too viscous, not easy to apply, and the adhesion of the fourth adhesive is reduced. Optionally, the mass fraction of the melamine-modified urea glue in the fourth adhesive ranges from 72% to 80%. Specifically, the mass fraction of the melamine-modified urea glue in the fourth adhesive may be, but not limited to, 72%, 74%, 76%, 78%, etc. If the mass fraction of the melamine-modified urea glue in the fourth adhesive is too small, the fourth adhesive will be too viscous and difficult to construct, and the adhesion of the fourth adhesive will be reduced; if the mass fraction of the melamine-modified urea glue in the fourth adhesive is too large, the leveling property of the fourth adhesive will be insufficient, and the roller coating processing performance of the fourth adhesive will be reduced.
[0160] Optionally, when the decorative layer 80 is LVT or PET, the fourth adhesive is a moisture-curing reactive polyurethane hot melt adhesive (Polyurethane Reactive, PUR adhesive for short).
[0161] Optionally, the material of the fifth adhesive layer 92 is formed by curing a fifth adhesive.
[0162] Optionally, when the balancing layer 90 is veneer, the fifth adhesive includes melamine-modified urea glue and flour. Optionally, the mass fraction of the flour in the fifth adhesive is in the range of 20% to 28%. Specifically, the mass fraction of the flour in the fifth adhesive may be, but not limited to, 20%, 22%, 24%, 26%, 28%, etc. If the mass fraction of the flour in the fifth adhesive is too low, the leveling property of the fifth adhesive is insufficient, which reduces the roller coating processing performance of the fifth adhesive; if the mass fraction of the flour in the fifth adhesive is too high, the fifth adhesive is too viscous, not easy to apply, and the adhesion of the fifth adhesive is reduced. Optionally, the mass fraction of the melamine-modified urea glue in the fifth adhesive is in the range of 72% to 80%. Specifically, the mass fraction of the melamine-modified urea glue in the fifth adhesive may be, but not limited to, 72%, 74%, 76%, 78%, etc. If the mass fraction of the melamine-modified urea glue in the fifth adhesive is too small, the fifth adhesive will be too viscous and difficult to apply, and the adhesion of the fifth adhesive will be reduced; if the mass fraction of the melamine-modified urea glue in the fifth adhesive is too large, the leveling property of the fifth adhesive will be insufficient, and the roller coating processing performance of the fifth adhesive will be reduced.
[0163] Optionally, when the balancing layer 90 is LVT or PET, the fifth adhesive is a moisture-curing reactive polyurethane hot melt adhesive (PolyurethaneReactive, referred to as PUR adhesive) or a two-component adhesive such as acrylic, epoxy, or polyurethane (referred to as AB adhesive).
[0164] The plate 100 of the embodiment of the present application can be prepared by the method described in the following embodiments of the present application. In addition, it can also be prepared by other methods. The preparation method of the embodiment of the present application is only one or more preparation methods of the plate 100 of the present application and should not be understood as a limitation on the plate 100 provided in the embodiment of the present application.
[0165] See also Fig.10 The present application also provides a method for preparing a plate 100, the method comprising:
[0166] S21, providing an inorganic gel and plant fiber, wherein the raw material components of the inorganic gel include magnesium sulfate and magnesium oxide, and the mass ratio of the magnesium sulfate to the magnesium oxide is in a range of 0.4 to 0.5;
[0167] S22, stirring and mixing the inorganic gel and the plant fiber to obtain a mixture;
[0168] Optionally, the weights of the inorganic gel and the plant fibers are measured according to a preset mass ratio, the crushed plant fibers are conveyed to a blender by a belt, the inorganic gel is evenly sprayed on the plant fibers through a nozzle of the blender, and a 3.5-meter-long spiral mixing and stirring method is used to obtain a mixture.
[0169] S23, laying, cold pressing and drying the mixture in sequence to solidify the inorganic gel to form an inorganic material, and obtain an inorganic board 10, wherein the board 100 includes an inorganic board 10, in which the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, and the 24h water absorption thickness expansion rate of the inorganic board 10 is less than or equal to 3%.
[0170] For detailed descriptions of other aspects of the inorganic board 10 , inorganic materials, and plant fibers, please refer to the descriptions of the corresponding parts of the above embodiments, which will not be repeated here.
[0171] The plate 100 of the embodiment of the present application includes an inorganic plate 10, which includes plant fibers and inorganic materials. In the inorganic plate 10, the mass ratio of the inorganic material to the plant fibers is in the range of 1.2 to 1.5, and the raw material components of the inorganic material include magnesium sulfate and magnesium oxide. The 24h water absorption thickness expansion rate of the inorganic plate 10 is less than or equal to 3%. In an embodiment of the present application, inorganic materials are added to the inorganic board 10, and the inorganic material components are designed as well as the ratio of the inorganic material to the plant fiber, so that the inorganic board 10 has a lower 24h water absorption thickness expansion rate; in addition, the board 100 of the present application includes the inorganic board 10, and the inorganic board 10 is made by pressing and has a higher flatness, so that when the decorative layer 80 is affixed to the surface of the inorganic board 10, it has a higher yield, improves the preparation yield of the board 100, and reduces the preparation cost of the board 100; furthermore, the inorganic board 10 can be used as the surface board of the board 100, and when the inorganic board 10 is used as the surface board, the defect requirements for the single board 32 under the surface board are reduced, and the cost of the board 100 can be better reduced while ensuring that the performance of the board 100 remains unchanged.
[0172] Optionally, the raw material components of the inorganic gel also include magnesium chloride, and the mass ratio of magnesium chloride to magnesium oxide in the raw material components of the inorganic gel is in the range of 0.05 to 0.15. If the mass ratio of magnesium chloride to magnesium oxide in the raw material components of the inorganic gel is too small, the content of magnesium chloride in the raw material components of the inorganic gel is too little, and the content of magnesium oxide is too much; if the content of magnesium chloride is too low, the bonding strength of the inorganic gel will be reduced, thereby reducing the bonding force between the inorganic gel and the plant fiber, which is not conducive to improving the hardness and mechanical strength of the inorganic board 10; if the content of magnesium oxide is too high, when the magnesium oxide is hydrated, more magnesium hydroxide (Mg(OH)2 colloid) colloid is formed in a short time, which increases the alkalinity of the inorganic gel, prevents the normal progress of the magnesium oxychloride gelling material, and makes the magnesium chloride exist in the form of MgCl2•6H2O, which will also aggravate the moisture absorption and halogen return of the inorganic board 10. If the mass ratio of magnesium chloride to magnesium oxide in the raw material components of the inorganic gel is too large, the content of magnesium chloride in the raw material components of the inorganic gel will be too high and the content of magnesium oxide will be too low; if the content of magnesium chloride is too high, the inorganic board 10 will be prone to deformation and cracking; if the content of magnesium oxide is too low, the magnesium oxychloride formed in the inorganic gel will be less gelled, and in addition, the magnesium chloride will be excessive, and chloride ions will exist in the inorganic board 10 in a free form, making it easy for the inorganic board 10 to absorb moisture and return to halogen or water, thereby reducing the moisture-proof performance of the inorganic board 10.
[0173] Optionally, in the raw material components of the inorganic gel, the mass ratio of the magnesium sulfate to the magnesium oxide is in the range of 0.4 to 0.5. Specifically, in the raw material components of the inorganic gel, the mass ratio of the magnesium sulfate to the magnesium oxide may be, but is not limited to, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, etc. If the mass ratio of the magnesium sulfate to the magnesium oxide is too low, the content of the magnesium sulfate is too little and the content of the magnesium oxide is too much; if the content of the magnesium sulfate is too little, the water resistance and compressive strength of the inorganic board 10 are reduced; if the content of the magnesium oxide is too much, when the magnesium oxide is hydrated, more magnesium hydroxide (Mg(OH)2 colloid) colloid is formed in a short time, which increases the alkalinity of the inorganic gel, prevents the normal progress of the magnesium oxychloride gelling material, and makes the magnesium chloride exist in the form of MgCl2•6H2O, which will also aggravate the moisture absorption and halogen return of the inorganic board 10. If the mass ratio of the magnesium sulfate to the magnesium oxide is too high, the content of magnesium sulfate is too high and the content of magnesium oxide is too low; if the content of magnesium sulfate is too high, the strength of the inorganic board 10 is reduced, the inorganic board 10 becomes brittle, and the impact strength is reduced, which is not conducive to the application of the inorganic board 10; if the content of magnesium oxide is too low, the magnesium oxychloride formed in the inorganic gel is less gelled, and in addition, magnesium chloride will be excessive, and chloride ions will exist in the inorganic board 10 in a free form, making the inorganic board 10 easy to absorb moisture and return to brine or water, thereby reducing the moisture-proof performance of the inorganic board 10.
[0174] Optionally, the raw material components of the inorganic gel also include a modifier, and the modifier is citric acid; in the raw material components of the inorganic gel, the mass ratio of the modifier to the magnesium chloride ranges from 0.025 to 0.045. Specifically, in the raw material components of the inorganic gel, the mass ratio of the modifier to the magnesium chloride can be, but is not limited to, 0.025, 0.028, 0.030, 0.033, 0.035, 0.038, 0.040, 0.043, 0.045, etc. In the raw material components of the inorganic gel, if the mass ratio of the modifier to the magnesium chloride is too small, the content of the modifier is too small, the degree of reaction of the magnesium chloride is limited, and the performance of the inorganic board 10 in reducing moisture absorption and halogen return is reduced; if the mass ratio of the modifier to the magnesium chloride is too large, the content of the modifier is too high, which reduces the thermal stability of the formed inorganic gel.
[0175] In some embodiments, the raw material components of the inorganic gel include the following components in parts by weight: 12 to 16 parts of magnesium chloride, 68 to 75 parts of magnesium sulfate, 150 to 170 parts of magnesium oxide, 0.3 to 1.2 parts of a modifier, and 110 to 120 parts of water. In this embodiment, when the raw material components of the inorganic gel include: 12 to 16 parts of magnesium chloride; 68 to 75 parts of magnesium sulfate; 150 to 170 parts of magnesium oxide; 0.3 to 1.2 parts of a modifier; and 110 to 120 parts of water, the formed inorganic gel has better bonding properties with the plant fiber, can better improve the internal bonding strength of the inorganic board 10, so that the inorganic board 10 is less prone to delamination; in addition, the toughness and mechanical strength of the inorganic board 10 can be better improved, so that the inorganic board 10 has better rigidity and better impact resistance.
[0176] In a specific embodiment, the raw material components of the inorganic gel include, by weight: 14 parts of magnesium chloride, 71.8 parts of magnesium sulfate, 160 parts of magnesium oxide, 0.5 parts of a modifier, and 116.8 parts of water. When the inorganic gel prepared by this raw material component is used to prepare the inorganic board 10, the inorganic gel and the plant fiber can have better bonding properties, and the internal bonding strength of the inorganic board 10 can be better improved, making the inorganic board 10 less prone to stratification; in addition, the toughness and mechanical strength of the inorganic board 10 can be better improved, so that the inorganic board 10 has good rigidity and good impact strength. In addition, the inorganic board 10 prepared by the ratio of the inorganic filler is less likely to have moisture regurgitation, condensation of water droplets, etc. in a high temperature and high humidity environment, and has a lower 24h water absorption thickness expansion rate.
[0177] For detailed descriptions of magnesium chloride, magnesium oxide, magnesium sulfate, citric acid and other aspects, please refer to the descriptions of the corresponding parts of the above embodiments, which will not be repeated here.
[0178] See also Fig.11 In some embodiments, the raw material components of the inorganic gel further include magnesium chloride and a modifier. In S21, providing the inorganic gel includes:
[0179] S211, dissolving the magnesium chloride in water at room temperature;
[0180] Optionally, a certain amount of deionized water or tap water is put into the preparation tank and stirred at room temperature to gradually dissolve the magnesium chloride.
[0181] S212, adding magnesium sulfate, and stirring at room temperature until the magnesium sulfate is completely dissolved;
[0182] Optionally, magnesium sulfate is added to the preparation tank and stirred until the magnesium sulfate is completely dissolved to obtain a magnesium salt solution.
[0183] S213, adding magnesium oxide and a modifier, and stirring at room temperature to allow magnesium chloride, magnesium sulfate and magnesium oxide to react to obtain the inorganic gel.
[0184] After adding magnesium oxide, magnesium oxide and magnesium salt solution (magnesium chloride and magnesium sulfate solution) react to form xMg(OH)2•yMgCI2•zH2O and xMg(OH)2•yMgSO4•zH2O to obtain inorganic gel. At room temperature, the main components of inorganic gel include 3Mg(OH)2•MgCI2•8H2O, 3Mg(OH)2•MgSO4•8H2O, and 5Mg(OH)2•MgCI2•8H2O.
[0185] Optionally, the pH value of the inorganic gel ranges from 8.0 to 9.5. Specifically, the pH value of the inorganic gel can be, but is not limited to, 8.0, 8.3, 8.5, 8.8, 9.0, 9.3, 9.5, and the like.
[0186] The inorganic gel prepared by the method of this embodiment has better bonding properties with plant fibers. When the inorganic gel and plant fibers are composited to prepare the inorganic board 10, the prepared inorganic board 10 can have higher hardness, compressive strength and impact strength, etc. In addition, the inorganic board 10 can also have a lower 24h water absorption thickness expansion rate, higher waterproof and moisture-proof properties, better fire resistance, etc.
[0187] In some embodiments, in S21, providing plant fibers includes: crushing the plant fiber raw materials to obtain plant fibers, wherein the size of the plant fibers ranges from 1.5 mm to 2.0 mm.
[0188] Optionally, the wood or plant straw is cleaned from impurities, dried, and then crushed; then sieved with a sieve to obtain plant fibers with a size of 1.5 mm to 2.0 mm. It can be understood that the aperture of the sieve is 1.5 mm to 2.0 mm.
[0189] Specifically, the size of the plant fiber may be, but is not limited to, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2.0 mm, etc. If the size of the plant fiber is too small, the crushing requirement is high, which increases the preparation cost of the inorganic board 10. If the size of the plant fiber is too large, the surface roughness of the inorganic board 10 is increased, and the strength of the inorganic board 10 is reduced. In this embodiment, by making the size of the plant fiber range from 1.5 mm to 2.0 mm, the surface roughness of the inorganic board 10 can be made smaller, smoother, and have higher strength.
[0190] Optionally, S22, stirring and mixing the inorganic gel and the plant fiber to obtain a mixture, including: measuring the weight of the inorganic gel and the plant fiber according to a preset mass ratio, conveying the crushed plant fiber to a mixer by a belt, spraying the inorganic gel evenly on the plant fiber through the nozzle of the mixer, and using a 3.5-meter-long spiral mixing and stirring to obtain a mixture.
[0191] See also Fig.12 In some embodiments, in S23, the mixture is sequentially paved, cold-pressed and molded, and dried to solidify the inorganic gel to form an inorganic material, and the inorganic board 10 is obtained, including:
[0192] S231, paving the mixed material on a pad to obtain a green body, and stacking a plurality of the green bodies in sequence;
[0193] Optionally, provide a pad and apply a release agent on two opposite surfaces of the pad, set the pad in a paving machine, use a material receiving and dividing device to pave the mixture, spread the mixture on the surface of the pad to form a blank of preset size, and stack multiple blanks in sequence through automatic stacking.
[0194] S232, cold pressing and locking the stacked multiple green bodies to obtain a green body stack;
[0195] Optionally, a mold is used to clamp multiple stacked green bodies, and after cold pressing to a preset thickness, the mold is locked to prevent the green bodies from rebounding and changing their dimensions (such as length, width, thickness, etc.). After being protected in a curing room for a period of time, the mold is automatically removed and naturally cured to obtain a green body stack.
[0196] S233 , drying the green body stack at a temperature of 125° C. to 145° C. to obtain the inorganic plate 10 .
[0197] Specifically, the drying temperature may be, but is not limited to, 125°C, 128°C, 130°C, 133°C, 135°C, 138°C, 140°C, 143°C, 145°C, etc.
[0198] The inorganic board 10 manufactured by this embodiment has high mechanical strength and hardness, and has low water absorption thickness expansion rate, water resistance and fire resistance.
[0199] See also Fig.13 In some embodiments, the green body stack is dried at a temperature of 125° C. to 145° C. to obtain the inorganic plate 10, comprising:
[0200] S2331, setting the mold temperature controller so that the preset outlet temperature of the mold temperature controller is 160° C. to 180° C. and the preset reflux temperature is 125° C. to 145° C.;
[0201] Specifically, the preset outlet temperature of the mold temperature controller may be, but is not limited to, 160°C, 163°C, 165°C, 168°C, 170°C, 173°C, 175°C, 178°C, 180°C, etc.
[0202] Specifically, the preset reflux temperature may be, but is not limited to, 125°C, 128°C, 130°C, 133°C, 135°C, 138°C, 140°C, 143°C, 145°C, etc.
[0203] S2332, when the reflux temperature of the mold temperature controller reaches the preset reflux temperature, placing the green body stack in the mold temperature controller;
[0204] Exemplarily, for example, the preset reflux temperature of the mold temperature controller is 138° C., and when the reflux temperature of the mold temperature controller reaches 138° C., the green body stack is placed in the mold temperature controller (ie, fed into the board).
[0205] S2333, in a first time period, turning on the mold temperature controller every first time period, wherein the first time period includes a plurality of the first time periods;
[0206] Optionally, the first time period may be, but is not limited to, within 50 to 70 minutes after entering the board; specifically, it may be, but is not limited to, 50 minutes, 55 minutes, 60 minutes, 66 minutes, 70 minutes, etc.
[0207] Optionally, the first duration may be, but is not limited to, 3 min to 6 min; specifically, it may be, but is not limited to, 3 min, 3.5 min, 4 min, 4.5 min, 5 min, 5.5 min, 6 min, etc.
[0208] In a specific example, within one hour after the board is loaded (the first period is 1 hour), the mold temperature controller is turned on every 5 minutes (the first period is 5 minutes). It can be understood that the mold temperature controller is turned on for a preset time (for example, 3s to 6s) each time and then turned off again.
[0209] S2334, in a second time period, turning on the mold temperature controller every second time period, wherein the second time period includes a plurality of second time periods, the second time period is greater than the first time period, and the second time period is after the first time period;
[0210] Optionally, the second time period can be but is not limited to a time period from 50 minutes to 70 minutes after entering the board; specifically, it can be but is not limited to a time period after 50 minutes, a time period after 55 minutes, a time period after 60 minutes, a time period after 66 minutes, a time period after 70 minutes, etc.
[0211] Optionally, the second duration may be but is not limited to 4 min to 10 min; specifically, it may be but is not limited to 4 min, 5 min, 6 min, 6.5 min, 7 min, 7.5 min, 8 min, 8.5 min, 9 min, 9.5 min, 10 min, etc.
[0212] In a specific example, after one hour after the board is loaded (the second period is 1 hour later), the mold temperature controller is turned on every 8 minutes (the second period is 8 minutes). It can be understood that the mold temperature controller is turned on for a preset time (for example, 3s to 6s) each time and then turned off again.
[0213] S2335 , when the reflow temperature is 2° C. to 5° C. higher than the preset reflow temperature, turn on the mold temperature controller to obtain the inorganic board 10 .
[0214] Optionally, when the reflow temperature of the mold temperature controller is stabilized at 2° C. to 5° C. higher than the preset reflow temperature, the inorganic board 10 has been prepared, and the mold temperature controller can be turned on.
[0215] Specifically, when the reflux temperature of the mold temperature controller is 2° C., 2° C., 4° C., or 5° C. higher than the preset reflux temperature, the baking is stopped and the mold temperature controller is turned on to obtain the inorganic board 10 .
[0216] In a specific embodiment, the thickness of each blank is greater than or equal to 10 mm. When the blanks are baked, the preset outlet temperature of the mold temperature controller is set to 170°C, and the preset reflux temperature is set to 135°C; when the reflux temperature of the mold temperature controller reaches 135°C, the blank stack is placed in the mold temperature controller (into the board); within the first hour, the mold temperature controller is opened and closed every 5 minutes, and the reflux temperature of the mold temperature controller is approximately 127°C after each opening and closing; after one hour, the mold temperature controller is opened and closed every 8 minutes until the reflux temperature of the mold temperature controller stabilizes at 138°C, and then the board is discharged.
[0217] In another specific embodiment, the thickness of each blank is less than 10 mm. When the blanks are baked, the preset outlet temperature of the mold temperature controller is set to 161°C, and the preset reflux temperature is set to 135°C; when the reflux temperature of the mold temperature controller reaches 135°C, the blank stack is placed in the mold temperature controller (into the board); within the first hour, the mold temperature controller is opened and closed every 3 minutes, and the reflux temperature of the mold temperature controller is approximately 127°C after each opening and closing; after one hour, the mold temperature controller is opened and closed every 5 minutes until the reflux temperature of the mold temperature controller stabilizes at 137°C, and then the board is discharged.
[0218] In this embodiment, the mold temperature controller is opened and closed once every a first time period in a first time period, and is opened and closed once every a second time period in a second time period, and the second time period is made greater than the first time period. In this way, during the reaction and curing process of the inorganic gel and the plant fiber, the water vapor in the blank can be removed in time, thereby improving the preparation efficiency of the inorganic board 10; in addition, the water content of the prepared inorganic board 10 can also be reduced; furthermore, it can also avoid that the water vapor in the blank is not removed in time and remains in the skin to form pores, so that the prepared inorganic board 10 has too many pores, thereby reducing the mechanical strength and the reasons of the inorganic board 10.
[0219] See also Fig.14 The present application also provides a method for preparing a plate 100, the method comprising:
[0220] S31, providing an inorganic gel and plant fibers, wherein the raw material components of the inorganic gel include magnesium chloride, magnesium sulfate and magnesium oxide;
[0221] S32, stirring and mixing the inorganic gel and the plant fiber to obtain a mixture;
[0222] S33, laying, cold-pressing and drying the mixture in sequence, so that the inorganic gel is solidified to form an inorganic material, and the inorganic board 10 is obtained, wherein the board 100 includes the inorganic board 10, in which the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, and the 24h water absorption thickness expansion rate of the inorganic board 10 is less than or equal to 3%;
[0223] For a detailed description of S31 to S33, please refer to the corresponding parts of the above embodiments S21 to S23, which will not be repeated here.
[0224] S34, providing a clamping plate 30 and a back plate 50, and forming a first adhesive layer and a second adhesive layer on two opposite surfaces of the clamping plate 30 respectively;
[0225] Optionally, a first adhesive is coated on one surface of the splint 30 to form a first adhesive layer, and a second adhesive is coated on the other surface of the splint 30 to form a second adhesive layer.
[0226] Optionally, the first adhesive includes melamine-modified urea adhesive and flour.
[0227] Optionally, the mass fraction of the flour in the first adhesive ranges from 40% to 50%. Specifically, the mass fraction of the flour in the first adhesive may be, but is not limited to, 40%, 42%, 44%, 46%, 48%, 50%, etc. If the mass fraction of the flour in the first adhesive is too low, the leveling property of the first adhesive is insufficient, which reduces the roller coating processing performance of the first adhesive; if the mass fraction of the flour in the first adhesive is too high, the first adhesive is too viscous, which is not easy to apply, and the adhesion of the first adhesive is reduced.
[0228] Optionally, the mass fraction of the melamine-modified urea glue in the first adhesive ranges from 50% to 60%. Specifically, the mass fraction of the melamine-modified urea glue in the first adhesive may be, but is not limited to, 50%, 52%, 55%, 56%, 58%, 60%, etc. If the mass fraction of the melamine-modified urea glue in the first adhesive is too small, the first adhesive is too viscous, not easy to apply, and the adhesion of the first adhesive is reduced; if the mass fraction of the melamine-modified urea glue in the first adhesive is too large, the leveling property of the first adhesive is insufficient, and the roller coating processing performance of the first adhesive is reduced.
[0229] Optionally, the coating amount of the first adhesive is in the range of 400 g / m 2 Up to 460g / m 2 Specifically, the coating amount of the first adhesive may be, but is not limited to, 400 g / m 2 , 410g / m2 , 420g / m 2 , 430g / m 2 , 450g / m 2 , 450g / m 2 , 460g / m 2 If the coating amount of the first adhesive is too small, the bonding force between the inorganic board 10 and the sandwich board 30 is reduced; if the coating amount of the first adhesive is too large, the mechanical strength of the prepared board 100 is reduced.
[0230] Optionally, the second adhesive includes melamine-modified urea adhesive and flour.
[0231] Optionally, the mass fraction of the flour in the second adhesive is in the range of 40% to 50%. Specifically, the mass fraction of the flour in the second adhesive may be, but is not limited to, 40%, 42%, 44%, 46%, 48%, 50%, etc. If the mass fraction of the flour in the second adhesive is too low, the leveling property of the second adhesive is insufficient, which reduces the roller coating processing performance of the second adhesive; if the mass fraction of the flour in the second adhesive is too high, the second adhesive is too viscous, which is not easy to apply, and the adhesive force of the second adhesive is reduced.
[0232] Optionally, the mass fraction of the melamine-modified urea glue in the second adhesive is in the range of 50% to 60%. Specifically, the mass fraction of the melamine-modified urea glue in the second adhesive may be, but is not limited to, 50%, 52%, 55%, 56%, 58%, 60%, etc. If the mass fraction of the melamine-modified urea glue in the second adhesive is too small, the second adhesive is too viscous, not easy to apply, and the adhesion of the second adhesive is reduced; if the mass fraction of the melamine-modified urea glue in the second adhesive is too large, the leveling property of the second adhesive is insufficient, and the roller coating processing performance of the second adhesive is reduced.
[0233] Optionally, the coating amount of the second adhesive is in the range of 400 g / m 2 Up to 460g / m 2 Specifically, the coating amount of the second adhesive may be, but is not limited to, 400 g / m 2 , 410g / m 2 , 420g / m 2 , 430g / m 2 , 450g / m 2 , 450g / m 2 , 460g / m 2 If the coating amount of the second adhesive is too small, the bonding force between the sandwich panel 30 and the back panel 50 is reduced; if the coating amount of the second adhesive is too large, the mechanical strength of the prepared board 100 is reduced.
[0234] S35, stacking the inorganic plate 10 on the surface of the first adhesive layer away from the clamping plate 30, and stacking the back plate 50 on the surface of the second adhesive layer away from the clamping plate 30;
[0235] It can be understood that the inorganic board 10 is attached to the first adhesive layer, and the backboard 50 is attached to the second adhesive layer, forming a stack in which the backboard 50, the second adhesive layer, the sandwich panel 30, the first adhesive layer and the inorganic board 10 are stacked in sequence.
[0236] S36, at a pressure of 5kg / cm 2 Up to 7kg / cm 2 Carry out the first cold pressing;
[0237] Optionally, the laminate is first subjected to a pressure of 5 kg / cm 2 Up to 7kg / cm 2 The first cold pressing is performed under the condition of 30 minutes to 120 minutes. The first cold pressing is performed before the first hot pressing, so that the first adhesive layer and the second adhesive layer can better form a continuous adhesive film, so that the first adhesive layer can better contact with the inorganic board 10 and the splint 30, and the contact area between the inorganic board 10 and the splint 30 and the first adhesive layer can be increased. At the same time, the second adhesive layer can better contact with the backboard 50 and the splint 30, and the contact area between the backboard 50 and the splint 30 and the first adhesive layer can be increased, so that the various layers of the plate 100 prepared have better bonding force, are less prone to delamination after long-term use, and have better mechanical strength.
[0238] Specifically, the pressure of the first cold pressing may be, but is not limited to, 5 kg / cm 2 , 5.5kg / cm 2 , 6kg / cm 2 、6.5kg / cm 2 , 7kg / cm 2 If the pressure of the first cold pressing is too small, it is difficult for the first adhesive layer and the second adhesive layer to form a continuous adhesive film, and the contact area between the first adhesive layer and the inorganic board 10 and the clamping plate 30 and the contact area between the second adhesive layer and the back plate 50 and the clamping plate 30 are still small; if the pressure of the first cold pressing is too large, it is easy to damage the inorganic board 10, the clamping plate 30 or the back plate 50.
[0239] Specifically, the time of the first cold pressing may be, but is not limited to, 30 min, 40 min, 50 min, 60 min, 80 min, 100 min, 120 min, etc. If the time of the first cold pressing is too short, it is difficult for the first adhesive layer and the second adhesive layer to form a continuous adhesive film, and the contact area between the first adhesive layer and the inorganic board 10 and the clamping plate 30 and the contact area between the second adhesive layer and the backboard 50 and the clamping plate 30 are still small; if the time of the first cold pressing is too long, the preparation cost of the board 100 is increased.
[0240] S37, at a pressure of 8kg / cm 2 Up to 13kg / cm 2 , a first hot pressing is performed at a temperature of 115°C to 125°C, so that the first adhesive layer forms a first adhesive layer 20, and the second adhesive layer forms a second adhesive layer 40, to obtain the board 100; wherein, before the first hot pressing, the moisture content of the backboard 50 is greater than the moisture content of the inorganic board 10.
[0241] Optionally, at a pressure of 8 kg / cm 2 Up to 13kg / cm 2 The first hot pressing is performed at a temperature of 115° C. to 125° C. for 8 min to 15 min, so that the first adhesive layer is cured to form a first adhesive layer 20 , and the second adhesive layer is cured to form a second adhesive layer 40 , thereby obtaining a plate 100 .
[0242] Optionally, the preparation method further comprises: curing the plate 100 for 7 days, sanding to determine thickness, trimming, and then packaging and storing.
[0243] Specifically, the pressure of the first hot pressing may be, but is not limited to, 8 kg / cm 2 , 9kg / cm 2 , 10kg / cm 2 , 11kg / cm 2 , 12kg / cm 2 , 13kg / cm 2 If the pressure of the first hot pressing is too small, the bonding of the inorganic board 10 , the clamping plate 30 and the back plate 50 is reduced; if the pressure of the first hot pressing is too large, the inorganic board 10 , the clamping plate 30 or the back plate 50 is easily damaged.
[0244] Specifically, the first hot pressing time may be, but is not limited to, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, etc. If the first hot pressing time is too short, the first adhesive layer and the second adhesive layer are not completely cured, so that the bonding force of the inorganic board 10, the clamping board 30 and the back board 50 is reduced, and the water resistance and mechanical strength of the prepared board 100 are reduced; if the first hot pressing time is too long, the preparation cost of the board 100 is increased.
[0245] Specifically, the temperature of the first hot pressing may be, but is not limited to, 115°C, 116°C, 117°C, 118°C, 119°C, 120°C, 121°C, 122°C, 123°C, 124°C, 125°C, etc. If the temperature of the first hot pressing is too low, the first adhesive layer and the second adhesive layer are not completely cured, so that the bonding force of the inorganic board 10, the splint 30 and the backboard 50 is reduced, and the water resistance and mechanical strength of the prepared board 100 are reduced; if the temperature of the first hot pressing is too high, the curing speed of the first adhesive layer and the second adhesive layer is too fast, and bubbles are easily present in the formed first adhesive layer 20 and the second adhesive layer 40, which will also reduce the bonding force of the inorganic board 10, the splint 30 and the backboard 50, and reduce the water resistance and mechanical strength of the prepared board 100.
[0246] In this embodiment, when the inorganic board 10 is compounded with the splint 30 and the back plate 50, the first cold pressing is performed first, and then the first hot pressing is performed, so that the inorganic board 10, the splint 30 and the back plate 50 of the prepared board 100 have better bonding force, thereby having higher mechanical strength. In addition, during the first hot pressing process, although the inorganic board 10, the back plate 50 and the splint 30 will shrink due to water loss, due to the high density of the inorganic board 10, when the moisture content of the inorganic board 10 is equivalent to that of the back plate 50, the first hot pressing is performed, and after the inorganic board 10 shrinks, the board 100 is more likely to warp or bend toward one side of the inorganic board 10. In this embodiment, by making the moisture content of the back panel 50 greater than the moisture content of the inorganic panel 10 before the first hot pressing, the internal stress or tension generated by the shrinkage of the back panel 50 after the first hot pressing can better balance the internal stress or tension generated by the shrinkage of the inorganic panel 10, thereby making the obtained panel 100 straighter and having a higher flatness.
[0247] In some embodiments, before the first hot pressing, the moisture content of the back panel 50 is greater than the moisture content of the splint 30, and the moisture content of the splint 30 is greater than the moisture content of the inorganic panel 10; the moisture content of the back panel 50 ranges from 12% to 20%; the moisture content of the splint 30 ranges from 10% to 12%; the moisture content of the inorganic panel 10 ranges from 4% to 7%.
[0248] Specifically, the moisture content of the back plate 50 may be in the range of, but not limited to, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20%. If the moisture content of the back plate 50 is too low, it is difficult to balance the internal stress generated by the shrinkage of the inorganic plate 10 during the hot pressing process, causing the prepared plate 100 to warp or bend toward one side of the inorganic plate 10; if the moisture content of the back plate 50 is too high, the internal stress generated by the water loss shrinkage of the back plate 50 during the hot pressing process is greater than the internal stress generated by the water loss shrinkage of the inorganic plate 10, causing the prepared plate 100 to warp or bend toward one side of the back plate 50.
[0249] Specifically, the moisture content of the splint 30 may be, but is not limited to, 10%, 10.3%, 10.5%, 10.8%, 11%, 11.3%, 11.5%, 11.8%, 12%, etc. If the moisture content of the splint 30 is too low, the splint 30 in the prepared sheet 100 is prone to expansion and deformation after absorbing moisture. In addition, the splint 30 is prone to brittleness, reduced toughness, and difficult to cut. It is prone to breakage, edge collapse, and other damage during processing; if the moisture content of the splint 30 is too high, it is prone to warping, deformation, and splitting after hot pressing.
[0250] Specifically, the moisture content of the inorganic board 10 may be, but is not limited to, 4%, 4.2%, 4.4%, 4.6%, 4.8%, 5%, 5.2%, 5.4%, 5.6%, 5.8%, 6%, 6.2%, 6.4%, 6.6%, 6.8%, 7%, etc. If the moisture content of the inorganic board 10 is too low, it is difficult to balance the internal stress generated by the shrinkage of the back plate 50 during the hot pressing process, so that the prepared board 100 is warped or bent toward one side of the back plate 50; if the moisture content of the inorganic board 10 is too high, the internal stress generated by the water loss shrinkage of the inorganic board 10 during the hot pressing process is greater than the internal stress generated by the water loss shrinkage of the back plate 50, so that the prepared board 100 is warped or bent toward one side of the inorganic board 10.
[0251] In this embodiment, before the first hot pressing, the moisture content of the back plate 50 is greater than the moisture content of the splint 30, and the moisture content of the splint 30 is greater than the moisture content of the inorganic plate 10. By designing the moisture content of the back plate 50, the splint 30 and the inorganic plate 10, the obtained plate 100 is less prone to deformation, bending, warping, etc., and the obtained plate 100 is straighter.
[0252] See also Fig.15 In some embodiments, in S34, providing the splint 30 includes:
[0253] S341, providing an adhesive and a multi-layer veneer 32;
[0254] Optionally, the adhesive includes melamine-modified urea glue and flour.
[0255] Optionally, the mass fraction of the flour in the adhesive is in the range of 40% to 50%. Specifically, the mass fraction of the flour in the adhesive may be, but is not limited to, 40%, 42%, 44%, 46%, 48%, 50%, etc. If the mass fraction of the flour in the adhesive is too low, the leveling property of the adhesive is insufficient, which reduces the roller coating processing performance of the adhesive; if the mass fraction of the flour in the adhesive is too high, the adhesive is too viscous, which is not easy to construct, and the adhesive force of the adhesive is reduced.
[0256] Optionally, the mass fraction of the melamine-modified urea glue in the adhesive is in the range of 50% to 60%. Specifically, the mass fraction of the melamine-modified urea glue in the adhesive may be, but is not limited to, 50%, 52%, 55%, 56%, 58%, 60%, etc. If the mass fraction of the melamine-modified urea glue in the adhesive is too small, the adhesive is too viscous, not easy to apply, and the adhesive force of the adhesive is reduced; if the mass fraction of the melamine-modified urea glue in the adhesive is too large, the leveling property of the adhesive is insufficient, and the roller coating processing performance of the adhesive is reduced.
[0257] Optionally, the veneer 32 may be, but is not limited to, at least one of a eucalyptus veneer, a poplar veneer, or a miscellaneous wood veneer, etc. In a specific example, the veneer 32 is a 1.7 mm thick eucalyptus veneer.
[0258] S342, coating the surface of a part of the multi-layer single board 32 with adhesive, and stacking the multi-layer single boards 32 in sequence;
[0259] Optionally, one layer of the multi-layer veneer 32 is not coated with adhesive, and the others are coated with adhesive on one surface to form an adhesive layer, and the multi-layer veneer 32 is stacked in sequence to form a stack in which the multi-layer veneer 32 and multiple layers of adhesive are alternately stacked in sequence.
[0260] Optionally, the coating amount of the adhesive of each adhesive layer is in the range of 360 g / m 2 Up to 400g / m 2 Specifically, the coating amount of the adhesive may be, but is not limited to, 360 g / m 2 , 370g / m 2 , 380g / m 2 , 390g / m 2 , 400g / m 2 If the amount of the adhesive applied is too little, the bonding force between the single plates 32 is reduced; if the amount of the adhesive applied is too much, the mechanical strength of the prepared plate 100 is reduced.
[0261] S343, at a pressure of 5kg / cm 2Up to 7kg / cm 2 The second cold pressing is carried out;
[0262] Optionally, the stack is first placed under a pressure of 5 kg / cm 2 Up to 7kg / cm 2 The second cold pressing is performed before the first hot pressing, and the time of the second cold pressing is 30 minutes to 120 minutes. The second cold pressing is performed before the first hot pressing, so that the adhesive layer can better form a continuous adhesive film, so that the adhesive layer and the single board 32 are in better contact, and the contact area between the adhesive layer and the single board 32 is increased, so that the single boards 32 of the prepared plywood 30 have better bonding force, and are less likely to be delaminated after long-term use, and have better mechanical strength.
[0263] Specifically, the pressure of the second cold pressing may be, but is not limited to, 5 kg / cm 2 , 5.5kg / cm 2 , 6kg / cm 2 、6.5kg / cm 2 , 7kg / cm 2 If the pressure of the second cold pressing is too small, it is difficult for the adhesive layer to form a continuous film, and the contact area between the adhesive layer and the single board 32 is still small; if the pressure of the second cold pressing is too large, the single board 32 is easily crushed.
[0264] Specifically, the second cold pressing time may be, but is not limited to, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 80 minutes, 100 minutes, 120 minutes, etc. If the second cold pressing time is too short, it is difficult for the adhesive layer to form a continuous adhesive film, and the contact area between the adhesive layer and the single board 32 is still small; if the second cold pressing time is too long, the preparation cost of the plywood 30 is increased.
[0265] S344, at a pressure of 8kg / cm 2 Up to 13kg / cm 2 , a second hot pressing is performed at a temperature of 115°C to 125°C to solidify the adhesive to form an adhesive layer 31, and the plywood 30 is obtained, wherein the plywood 30 includes a plurality of adhesive layers 31 and a plurality of single boards 32, the adhesive layers 31 and the single boards 32 are alternately stacked in sequence, the fibers of one of the two adjacent single boards 32 extend along a first direction, and the fibers of the other extend along a second direction, wherein the first direction intersects with the second direction.
[0266] Optionally, at a pressure of 8 kg / cm 2 Up to 13kg / cm 2 The second hot pressing is performed at a temperature of 115° C. to 125° C. The time of the second hot pressing is 8 min to 15 min, so that the adhesive layer is cured to form an adhesive layer 31 .
[0267] Specifically, the pressure of the second hot pressing may be, but is not limited to, 8 kg / cm 2 , 9kg / cm 2 , 10kg / cm 2 , 11kg / cm 2 , 12kg / cm 2 , 13kg / cm 2 If the pressure of the second hot pressing is too small, the bonding between the multi-layer single plates 32 will be reduced; if the pressure of the second hot pressing is too large, the splint 30 will be easily crushed.
[0268] Specifically, the second hot pressing time may be, but is not limited to, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, etc. If the second hot pressing time is too short, the adhesive is not completely cured, so that the bonding force of the multi-layer single board 32 is reduced, and the water resistance and mechanical strength of the prepared splint 30 are reduced; if the second hot pressing time is too long, the preparation cost of the splint 30 is increased.
[0269] Specifically, the temperature of the second hot pressing may be, but is not limited to, 115°C, 116°C, 117°C, 118°C, 119°C, 120°C, 121°C, 122°C, 123°C, 124°C, 125°C, etc. If the temperature of the second hot pressing is too low, the adhesive is not completely cured, which reduces the bonding strength of the multi-layer veneer 32, and reduces the water resistance and mechanical strength of the obtained splint 30; if the temperature of the second hot pressing is too high, the curing speed of the adhesive is too fast, and bubbles are easily present in the formed adhesive layer 31, which also reduces the bonding strength of the multi-layer veneer 32, and reduces the water resistance and mechanical strength of the obtained splint 30.
[0270] See also Fig.16 The present application also provides a method for preparing a plate 100, the method comprising:
[0271] S41, providing an inorganic gel and plant fibers, wherein the raw material components of the inorganic gel include magnesium chloride, magnesium sulfate and magnesium oxide;
[0272] S42, stirring and mixing the inorganic gel and the plant fiber to obtain a mixture;
[0273] S43, laying, cold pressing and locking the mold, and drying the mixture in sequence, so that the inorganic gel is solidified to form an inorganic material, and the inorganic board 10 is obtained, wherein the board 100 includes the inorganic board 10, in which the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, and the 24h water absorption thickness expansion rate of the inorganic board 10 is less than or equal to 3%;
[0274] For a detailed description of S41 to S43, please refer to the corresponding parts of the above embodiments S21 to S23, which will not be repeated here.
[0275] S44, coating the third adhesive on the surface of the multilayer inorganic board 10 to form a third adhesive layer;
[0276] Optionally, the third adhesive comprises phenolic resin glue and flour. Optionally, the mass fraction of the flour in the third adhesive ranges from 20% to 28%, and the mass fraction of the phenolic resin glue ranges from 72% to 80%.
[0277] Optionally, the coating amount of each layer of the third adhesive is in the range of 120 g / m 2 Up to 180g / m 2 Specifically, the coating amount of the third adhesive may be, but is not limited to, 120 g / m 2 , 130g / m 2 , 140g / m 2 , 150g / m 2 , 160g / m 2 , 170g / m 2 , 180g / m 2 If the coating amount of the third adhesive is too small, the bonding force between the two inorganic boards 10 is reduced; if the coating amount of the third adhesive is too large, the mechanical strength of the prepared inorganic composite board 10a is reduced.
[0278] For detailed description of other aspects of the third adhesive, please refer to the description of the corresponding parts of the above embodiments, which will not be repeated here.
[0279] S45, providing at least one toughening layer 60, disposing each toughening layer 60 between two inorganic plates 10, and making each third adhesive layer located between the toughening layer 60 and the inorganic plate 10;
[0280] It can be understood that the inorganic plates 10 and the toughening layers 60 are alternately stacked in sequence, and the adjacent inorganic plates 10 and toughening layers 60 are bonded by the third adhesive layer.
[0281] S46, at a pressure of 5kg / cm 2 Up to 7kg / cm 2 Under the condition of being cold pressed for the third time, the time of the third cold pressed time is 30min to 120min;
[0282] Specifically, the pressure of the third cold pressing may be, but is not limited to, 5 kg / cm 2 , 5.5kg / cm 2 , 6kg / cm 2 、6.5kg / cm 2, 7kg / cm 2 If the pressure of the third cold press is too small, it is difficult for the third adhesive layer to form a continuous adhesive film, and the contact area between the third adhesive layer and the inorganic board 10 is still small; if the pressure of the third cold press is too large, the inorganic board 10 is easily crushed.
[0283] Specifically, the third cold pressing time may be, but is not limited to, 30 min, 40 min, 50 min, 60 min, 80 min, 100 min, 120 min, etc. If the third cold pressing time is too short, it is difficult for the third adhesive layer to form a continuous adhesive film, and the contact area between the third adhesive layer and the inorganic board 10 is still small; if the third cold pressing time is too long, the preparation cost of the inorganic composite board 10a is increased.
[0284] S47, at a pressure of 8kg / cm 2 Up to 13kg / cm 2 The third hot pressing is performed at a temperature of 115° C. to 125° C. for a time of 8 min to 15 min, so that the third adhesive layer is cured to form a third bonding layer 70 , thereby obtaining the inorganic composite board 10 a .
[0285] Specifically, the pressure of the third hot pressing may be, but is not limited to, 8 kg / cm 2 , 9kg / cm 2 , 10kg / cm 2 , 11kg / cm 2 , 12kg / cm 2 , 13kg / cm 2 If the pressure of the third hot pressing is too small, the bonding between the inorganic plate 10 and the toughening layer 60 will be reduced; if the pressure of the third hot pressing is too large, the inorganic plate 10 will be easily damaged.
[0286] Specifically, the time of the third hot pressing may be, but is not limited to, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, etc. If the time of the third hot pressing is too short, the third adhesive layer is not completely cured, so that the bonding force between the inorganic board 10 and the toughening layer 60 is reduced, and the water resistance and mechanical strength of the prepared inorganic composite board 10a are reduced; if the time of the third hot pressing is too long, the preparation cost of the inorganic composite board 10a is increased.
[0287] Specifically, the temperature of the third hot pressing may be, but is not limited to, 115°C, 116°C, 117°C, 118°C, 119°C, 120°C, 121°C, 122°C, 123°C, 124°C, 125°C, etc. If the temperature of the third hot pressing is too low, the third adhesive layer is not completely cured, so that the bonding force between the inorganic board 10 and the toughening layer 60 is reduced, and the water resistance and mechanical strength of the inorganic composite board 10a are reduced; if the temperature of the third hot pressing is too high, the curing speed of the third adhesive layer is too fast, and bubbles are easily present in the formed third adhesive layer 70, which also reduces the bonding force between the inorganic board 10 and the toughening layer 60, and reduces the water resistance and mechanical strength of the inorganic composite board 10a.
[0288] See also Fig.17 The present application also provides a method for preparing a plate 100, the method comprising:
[0289] S51, providing an inorganic gel and plant fiber, wherein the raw material components of the inorganic gel include magnesium chloride, magnesium sulfate and magnesium oxide;
[0290] S52, stirring and mixing the inorganic gel and the plant fiber to obtain a mixture;
[0291] S53, laying, cold pressing and locking the mold, and drying the mixture in sequence, so that the inorganic gel is solidified to form an inorganic material, and the inorganic board 10 is obtained, wherein the board 100 includes the inorganic board 10, in which the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, and the 24h water absorption thickness expansion rate of the inorganic board 10 is less than or equal to 3%;
[0292] S54, coating a third adhesive on the surface of the inorganic board 10 to form a third adhesive layer;
[0293] S55, providing at least one toughening layer 60, disposing each toughening layer 60 between two inorganic plates 10, and making each third adhesive layer located between the toughening layer 60 and the inorganic plate 10;
[0294] S56, at a pressure of 5kg / cm 2 Up to 7kg / cm 2 Under the condition of being cold pressed for the third time, the time of the third cold pressed time is 30min to 120min;
[0295] S57, at a pressure of 8kg / cm 2 Up to 13kg / cm 2 , performing a third hot pressing at a temperature of 115° C. to 125° C., and the time of the third hot pressing is 8 min to 15 min, so as to obtain an inorganic composite plate 10a;
[0296] For a detailed description of S51 to S57, please refer to the corresponding parts of the above embodiments S41 to S47, which will not be repeated here.
[0297] S58, coating a fourth adhesive on one surface of the inorganic composite board 10a to form a fourth adhesive layer, and coating a fifth adhesive on the other surface to form a fifth adhesive layer;
[0298] Optionally, when the fourth adhesive and the fifth adhesive both include melamine-modified urea adhesive and flour, the coating amount of the fourth adhesive is in the range of 80 g / m 2 Up to 100g / m 2 The coating amount of the fourth adhesive is in the range of 100g / m 2 Up to 120g / m 2 .
[0299] When the fourth adhesive and the fifth adhesive are both PUR adhesives, the coating amount of the fourth adhesive and the fifth adhesive is 60g / m 2 Up to 80g / m 2 .
[0300] For detailed description of other aspects of the fourth adhesive and the fifth adhesive, please refer to the description of the corresponding parts of the above embodiments, which will not be repeated here.
[0301] S59, disposing a decorative layer 80 on the surface of the fourth adhesive layer, and disposing a balancing layer 90 on the surface of the fifth adhesive layer;
[0302] For detailed description of other aspects of the decoration layer 80 and the balancing layer 90 , please refer to the description of the corresponding parts of the above embodiment, which will not be repeated here.
[0303] S510 , performing lamination to solidify the fourth adhesive layer to form a fourth adhesive layer 91 , and solidify the fifth adhesive layer to form a fifth adhesive layer 92 , so as to obtain the plate 100 .
[0304] When the decorative layer 80 is natural veneer and the balancing layer 90 is thin wood, the pressing step includes: 2 Up to 7kg / cm 2 The fourth cold pressing is performed at a pressure of 6 kg / cm 2 Up to 10kg / cm 2 The fourth hot pressing is performed at a temperature of 105° C. to 115° C., and the time of the fourth hot pressing is 4 min to 8 min.
[0305] When the decorative layer 80 is LVT or PET and the balancing layer 90 is LVT or PET, the lamination comprises: firstly rolling at a pressure of 7 kg / cm 2Up to 9kg / cm 2 The fourth cold pressing is carried out for 18 to 30 hours.
[0306] See also Fig.18 The present application also provides a method for preparing a plate 100, the method comprising:
[0307] S61, providing an inorganic gel and plant fiber, wherein the raw material components of the inorganic gel include magnesium chloride, magnesium sulfate and magnesium oxide;
[0308] S62, stirring and mixing the inorganic gel and the plant fiber to obtain a mixture;
[0309] S63, laying, cold pressing and locking the mold, and drying the mixture in sequence, so that the inorganic gel is solidified to form an inorganic material, and the inorganic board 10 is obtained, wherein the board 100 includes the inorganic board 10, in which the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, and the 24h water absorption thickness expansion rate of the inorganic board 10 is less than or equal to 3%;
[0310] For a detailed description of S61 to S63, please refer to the corresponding parts of the above embodiments S21 to S23, which will not be repeated here.
[0311] S64, disposing a decorative layer 80 on one side of the inorganic board 10, and disposing a balancing layer 90 on the other side of the inorganic board 10, wherein the decorative layer 80 is impregnated paper, and the balancing layer 90 is balancing paper;
[0312] S65, at a pressure of 70kg / cm 2 Up to 80kg / cm 2 , a fifth hot pressing is performed at a temperature of 190° C. to 200° C. The time of the fifth hot pressing is 25 seconds to 40 seconds to obtain a plate 100.
[0313] The board 100 of the embodiment of the present application is further described below through specific examples.
[0314] Example 1 and Example 2
[0315] The plate 100 of each embodiment is prepared by the following steps:
[0316] (1) Prepare an inorganic gel, which comprises, by mass fraction, 4% magnesium chloride, 20% magnesium sulfate, 44% magnesium oxide, and the remainder water.
[0317] (2) Providing reed stalk fibers having a size of 1.5 mm to 2.0 mm;
[0318] (3) stirring and mixing the inorganic gel and the reed stalk fiber to obtain a mixture, wherein the mass ratio of the inorganic gel to the reed stalk fiber is 2:1;
[0319] (4) laying out the mixed materials in sequence, cold pressing and locking the mold, and obtaining a green body stack;
[0320] (5) The preset outlet temperature of the mold temperature controller is set to 161°C, and the preset reflux temperature is set to 135°C; when the reflux temperature of the mold temperature controller reaches 135°C, the blank stack is placed in the mold temperature controller (board feeding); within the first hour, the mold temperature controller is opened and closed every 3 minutes, and the reflux temperature of the mold temperature controller is approximately 127°C after each opening and closing; after one hour, the mold temperature controller is opened and closed every 5 minutes until the reflux temperature of the mold temperature controller is stabilized at 137°C, and then the board is discharged.
[0321] The thickness of the inorganic plate 10 prepared in Example 1 is 3.5 mm; the thickness of the inorganic plate 10 prepared in Example 2 is 8.0 mm.
[0322] Comparative Example 1
[0323] The board 100 of this comparative example is a commercially available 3.5 mm straw board.
[0324] Comparative Example 2
[0325] The board 100 of this comparative example is a commercially available 3.5 mm wood powder board.
[0326] Comparative Example 3
[0327] The board 100 of this comparative example is a commercially available 8.0 mm wood powder board.
[0328] Comparative Example 4
[0329] The board 100 of this comparative example is a commercially available 8.0 mm thick wood powder board (wood powder).
[0330] Comparative Example 5
[0331] The board 100 of this comparative example is a commercially available 8.0 mm rock board (wood powder).
[0332] Comparative Example 6
[0333] The board 100 of this comparative example is a commercially available 8.0 mm high-density fiberboard (HDF).
[0334] The following performance tests were performed on the board 100 of Examples 1 to 2 and Comparative Examples 1 to 6.
[0335] (1) Formaldehyde detection: According to GB / T 17657-2022, the desiccant method is used for detection.
[0336] (2) 24h water absorption thickness expansion rate and 2h water absorption thickness expansion rate: measured in accordance with GB / T 18102-2020.
[0337] (3) Moisture content (%), density (g / cm³), internal bonding strength (MPa), surface bonding strength (MPa): tested in accordance with LY / T1611-2011.
[0338] (4) Fire resistance performance (level): tested in accordance with GB 8624.
[0339] (5) Anti-halogen reversion: Tested according to JC 688.
[0340] Various performance tests were performed on the plates 100 of Examples 1 to 2 and Comparative Examples 1 to 6, and the test results are shown in Table 1 below:
[0341] Table 1 Test data of the board 100 of Examples 1 to 2 and Comparative Examples 1 to 6
[0342]
[0343] From the test results of Examples 1 to 2 and Comparative Examples 1 to 6, it can be seen that, under the condition of the same thickness, the plate 100 (i.e., the inorganic plate 10) of the embodiment of the present application has a lower formaldehyde content, a lower 2h water absorption thickness expansion rate, a lower 24h water absorption thickness expansion rate, and a lower moisture content. In addition, the plate 100 (i.e., the inorganic plate 10) of the embodiment of the present application also has higher fire resistance and better water resistance.
[0344] Example 3 to Example 11
[0345] The difference between each embodiment and embodiment 1 is that the composition of the inorganic gel is different, and the modifier of each embodiment includes 32% citric acid, 1% magnesium sulfate and the balance water. The composition of the inorganic gel of each embodiment is shown in Table 2 below:
[0346] Table 2 Composition of the inorganic gels of Examples 3 to 11
[0347]
[0348] Various performance tests were performed on the plates 100 of Examples 3 to 11, and the test results are shown in Table 3 below:
[0349] Table 3 Test data of the plate 100 of Examples 3 to 11
[0350]
[0351] It can be seen from the test results of Examples 1 to 9 that the inorganic board 10 made of the inorganic gel with the ratio of this application has a lower 2h water absorption thickness expansion rate, 24h water absorption thickness expansion rate and moisture content, and has higher internal bonding strength and surface bonding strength, has good resistance to halogen reversion, and is not prone to moisture reversion.
[0352] It can be seen from Examples 1, 10 and 11 that when magnesium chloride is added to the inorganic gel, the internal bonding strength and surface bonding strength of the inorganic board 10 can be improved. However, when the magnesium chloride content in the inorganic gel is too high, the anti-halogenation property of the inorganic board 10 is reduced, making it easy to get damp.
[0353] Example 12
[0354] The plate 100 of this embodiment is prepared by the following steps:
[0355] (1) Preparation of plywood 30: Provide four layers of 1.7 mm eucalyptus veneers and an adhesive, wherein the adhesive comprises 60% melamine-modified urea glue and 40% flour, apply the adhesive to three layers of eucalyptus veneers, and then adhere the four layers of eucalyptus veneers in sequence, with the amount of adhesive applied being 380 g / m 2 , at a pressure of 5kg / cm 2 Cold press for 30 minutes; hot press pressure 10kg / cm 2 , hot pressing temperature is 120°C, hot pressing time is 10min, and splint 30 is obtained;
[0356] (2) The first adhesive and the second adhesive are respectively coated on the two surfaces of the splint 30. The first adhesive and the second adhesive both include 60% melamine-modified urea adhesive and 40% flour. The coating amount is 440 g / m 2 ;
[0357] (3) providing a 1.7 mm thick eucalyptus veneer as the backboard 50 and providing the inorganic board 10 of Example 1, and laminating the inorganic board 10 and the backboard 50 to two opposite surfaces of the plywood 30 respectively;
[0358] (4) At pressure 7kg / cm 2 Cold press for 30 minutes; due to the hot press pressure of 9kg / cm 2 , hot pressing temperature is 120℃, hot pressing time is 8min, and plate 100 is obtained.
[0359] Embodiment 13
[0360] The plate 100 of this embodiment is prepared by the following steps:
[0361] (1) Preparation of inorganic composite board 10a: providing two inorganic boards 10 of Example 1, a 0.3 mm thick okoume as a toughening layer 60, and a third adhesive, wherein the third adhesive comprises 72% phenolic resin glue and 28% flour; coating the third adhesive on the two inorganic boards 10, and placing the okoume between the two inorganic boards 10, and the coating amount of the third adhesive is 170 g / m 2 ; Enter the cold press within 45 minutes, cold press for 30 minutes, pressure 5kg / cm 2 After cold pressing, let it stand for 30 minutes; then hot press it for 13 minutes at a pressure of 10 kg / cm 2 , hot pressing temperature 120℃;
[0362] (2) removing dust from the inorganic composite board 10a, by placing an impregnated paper on one surface of the inorganic composite board 10a and placing a balancing paper on the other surface;
[0363] (3) Hot pressing for 38 seconds at a pressure of 72 kg / cm 2 , the upper steel plate temperature is 192℃, the lower steel plate temperature is 198℃, the large plate is obtained, cured for 7 days, the large plate is sliced, the blank is milled, the blank is chamfered and painted, and plate 100 is obtained.
[0364] Embodiment 14
[0365] The plate 100 of this embodiment is prepared by the following steps:
[0366] (1) Preparation of inorganic composite board 10a: providing two inorganic boards 10 of Example 1, a 0.3 mm thick okoume as a toughening layer 60, and a third adhesive, wherein the third adhesive comprises 72% phenolic resin glue and 28% flour; coating the third adhesive on the two inorganic boards 10, and placing the okoume between the two inorganic boards 10, and the coating amount of the third adhesive is 170 g / m 2 ; Enter the cold press within 45 minutes, cold press for 30 minutes, pressure 5kg / cm 2 After cold pressing, let it stand for 30 minutes; then hot press it for 13 minutes at a pressure of 10 kg / cm 2 , hot pressing temperature 120℃;
[0367] (2) Dust removal of the inorganic composite board 10a: a fourth adhesive is coated on one surface of the inorganic composite board 10a to form a fourth adhesive layer, and a fifth adhesive is coated on the other surface to form a fifth adhesive layer. The coating amount of the fourth adhesive is 90 g / m 2 The coating amount of the fifth adhesive is 110g / m 2 ; The fourth adhesive and the fifth adhesive both include 72% phenolic resin glue and 28% flour;
[0368] (3) pasting natural veneer (decorative layer 80) on the fourth adhesive layer, and pasting 0.5 mm beech wood (balancing layer 90) on the fifth adhesive layer;
[0369] (4) Cold pressing for 30 minutes at a pressure of 5 kg / cm 2 ; Hot pressing, hot pressing time 5min, hot pressing pressure 8kg / cm 2 , hot pressing temperature is 110℃, made into large slabs, cured for 7 days, large slabs are sliced, blanks are milled, board surface and back are coated with UV paint, mortise and tenon are sealed with waterproof wax, plastic sealed and packed, and put into storage.
[0370] Embodiment 15
[0371] The plate 100 of this embodiment is prepared by the following steps:
[0372] (1) Preparation of inorganic composite board 10a: providing two inorganic boards 10 of Example 1, a 0.3 mm thick okoume as a toughening layer 60, and a third adhesive, wherein the third adhesive comprises 72% phenolic resin glue and 28% flour; coating the third adhesive on the two inorganic boards 10, and placing the okoume between the two inorganic boards 10, and the coating amount of the third adhesive is 170 g / m 2 ; Enter the cold press within 45 minutes, cold press for 30 minutes, pressure 5kg / cm 2 After cold pressing, let it stand for 30 minutes; then hot press it for 13 minutes at a pressure of 10 kg / cm 2 , hot pressing temperature 120℃;
[0373] (2) Dust removal of the inorganic composite board 10a: PUR glue (i.e., the fourth adhesive and the fifth adhesive are both PUR glue) is roller-coated on the upper and lower surfaces of the inorganic composite board 10a, and the amount of glue applied on the upper and lower surfaces is 60g / m 2 , after the upper and lower surfaces are attached to LVT, roll pressing;
[0374] (3) The large plate after rolling is cold pressed for 24 hours at a pressure of 8kg / cm 2 ; Cutting of large panels, milling of blanks, sealing of mortise and tenon grooves with waterproof wax, plastic packaging, and storage.
[0375] Example 16
[0376] The plate 100 of this embodiment is prepared by the following steps:
[0377] (1) Providing the inorganic board 10 of Example 1;
[0378] (2) removing dust from the inorganic board 10 by placing an impregnated paper on one surface of the inorganic board 10 and placing a balancing paper on the other surface;
[0379] (3) Hot pressing for 38 seconds at a pressure of 72 kg / cm2 , the upper steel plate temperature is 192℃, the lower steel plate temperature is 198℃, the large plate is obtained, cured for 7 days, the large plate is sliced, the blank is milled, the blank is chamfered and painted, and plate 100 is obtained.
[0380] Embodiment 17
[0381] The plate 100 of this embodiment is prepared by the following steps:
[0382] (1) Providing the inorganic board 10 of Example 1;
[0383] (2) Dust removal of the inorganic board 10: coating a fourth adhesive on one surface of the inorganic board 10 to form a fourth adhesive layer, and coating a fifth adhesive on the other surface to form a fifth adhesive layer. The coating amount of the fourth adhesive is 90 g / m 2 The coating amount of the fifth adhesive is 110g / m 2 ; The fourth adhesive and the fifth adhesive both include 72% phenolic resin glue and 28% flour;
[0384] (3) pasting natural veneer (decorative layer 80) on the fourth adhesive layer, and pasting 0.5 mm beech wood (balancing layer 90) on the fifth adhesive layer;
[0385] (4) Cold pressing for 30 minutes at a pressure of 5 kg / cm 2 ; Hot pressing, hot pressing time 5min, hot pressing pressure 8kg / cm 2 , hot pressing temperature is 110℃, made into large slabs, cured for 7 days, large slabs are sliced, blanks are milled, board surface and back are coated with UV paint, mortise and tenon are sealed with waterproof wax, plastic sealed and packed, and put into storage.
[0386] Embodiment 18
[0387] The plate 100 of this embodiment is prepared by the following steps:
[0388] (1) Providing the inorganic board 10 of Example 1;
[0389] (2) Dust removal of the inorganic board 10: PUR glue is applied by roller on the upper and lower surfaces of the inorganic board 10 (i.e., the fourth adhesive and the fifth adhesive are both PUR glue), and the amount of glue applied on the upper and lower surfaces is 60 g / m 2 , after the upper and lower surfaces are attached to LVT, roll pressing;
[0390] (3) The large plate after rolling is cold pressed for 24 hours at a pressure of 8kg / cm 2 ; Cutting of large panels, milling of blanks, sealing of tongue and groove with waterproof wax, plastic packaging, and storage.
[0391] Various performance tests were performed on the plates 100 of Examples 12 to 18, and the test results are shown in Table 4 below:
[0392] Table 4 Test data of the plate 100 of Examples 12 to 18
[0393]
[0394] From the test results of Examples 12 to 18, it can be seen that the board 100 prepared in the present application has a lower formaldehyde emission, a lower 2h water absorption thickness expansion rate and a lower 24h water absorption thickness expansion rate, and has higher internal bonding strength and surface bonding strength, has better resistance to halogen resorption, and is not easy to absorb water and moisture.
[0395] Mentioning "embodiment" and "implementation method" in this application means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrases in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments. In addition, it should also be understood that the features, structures or characteristics described in the various embodiments of the present application can be arbitrarily combined to form another embodiment that does not deviate from the spirit and scope of the technical solution of the present application, if there is no contradiction between them.
[0396] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the above preferred implementation modes, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.
Claims
1. A plate, characterized in that: The plate comprises: An inorganic board, comprising plant fiber and inorganic material, wherein the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, the raw material components of the inorganic material comprise magnesium sulfate and magnesium oxide, the mass ratio of the magnesium sulfate to the magnesium oxide is in the range of 0.4 to 0.5; the raw material components of the inorganic material further comprise magnesium chloride and a modifier, the mass ratio of magnesium chloride to magnesium oxide is in the range of 0.09 to 0.15; the modifier is citric acid; in the raw material components of the inorganic material, the mass ratio of the modifier to the magnesium chloride is in the range of 0.025 to 0.045; the 24h water absorption thickness expansion rate of the inorganic board is less than or equal to 3%.
2. The plate material according to claim 1, characterized in that The raw material components of the inorganic material include, by mass fraction, 4% to 6% of magnesium chloride, 17% to 23% of magnesium sulfate, and 40% to 48% of magnesium oxide.
3. The plate material according to claim 1, characterized in that: Before the citric acid is added, the citric acid is first mixed with a portion of the magnesium sulfate to form a mixed solution, so that the mass ratio of the citric acid to the magnesium sulfate in the mixed solution is in the range of 20 to 66.
4. The sheet material according to any one of claims 1 to 3, characterized in that: The raw material components of the inorganic material include the following components in parts by weight: 12 to 16 parts of magnesium chloride; 68 to 75 parts of magnesium sulfate; 150 to 170 parts of magnesium oxide; 0.3 to 1.2 parts of a modifier; as well as 110 to 120 parts of water.
5. The sheet material according to any one of claims 1 to 3, characterized in that: The density ρ of the inorganic plate is in the range of 1 mg / cm 3 ≤ρ≤1.5mg / cm 3 ; The 2h water absorption thickness expansion rate of the inorganic board is less than or equal to 2%; The fire protection level of the inorganic board is A2.
6. The sheet material according to claim 1, characterized in that The plate also includes: a first adhesive layer, the first adhesive layer being disposed on a surface of the inorganic board; A clamping plate, the clamping plate is arranged on a surface of the first adhesive layer away from the inorganic plate; a second adhesive layer, the second adhesive layer being disposed on a surface of the splint facing away from the first adhesive layer; and A back plate is arranged on a surface of the second adhesive layer facing away from the inorganic plate.
7. The sheet material according to claim 6, characterized in that The plywood includes multiple adhesive layers and multiple veneers, wherein the adhesive layers and the veneers are alternately stacked in sequence, wherein fibers of one of two adjacent veneers extend along a first direction, and fibers of the other extend along a second direction, wherein the first direction intersects with the second direction.
8. The plate material according to claim 1, characterized in that The inorganic board is multi-layered, and the board further comprises at least one toughening layer. The multi-layered inorganic board and the toughening layer are alternately stacked in sequence to form an inorganic composite board, and the toughening layer is thin wood or non-woven fabric.
9. The sheet material according to claim 1, 6 or 8, characterized in that The plate also includes: a decorative layer, the decorative layer being disposed on one side of the inorganic board; and A balancing layer is disposed on the other side of the inorganic board.
10. A method for preparing a plate, characterized in that: The preparation method comprises: Provided are an inorganic gel and a plant fiber, wherein the raw material components of the inorganic gel include magnesium sulfate and magnesium oxide, the mass ratio of the magnesium sulfate to the magnesium oxide is in the range of 0.4 to 0.5; the raw material components of the inorganic gel also include magnesium chloride and a modifier, the mass ratio of magnesium chloride to magnesium oxide is in the range of 0.09 to 0.15; the modifier is citric acid; in the raw material components of the inorganic gel, the mass ratio of the modifier to the magnesium chloride is in the range of 0.025 to 0.045; Stirring and mixing the inorganic gel and the plant fiber to obtain a mixture; and The mixture is laid, cold-pressed and dried in sequence to solidify the inorganic gel to form an inorganic material and obtain an inorganic board, wherein the board includes an inorganic board, in which the mass ratio of the inorganic material to the plant fiber is in the range of 1.2 to 1.5, and the 24h water absorption thickness expansion rate of the inorganic board is less than or equal to 3%.
11. The method for preparing a plate material according to claim 10, characterized in that: The inorganic gel provided comprises: Dissolving the magnesium chloride in water at room temperature; Add magnesium sulfate, and stir at room temperature until the magnesium sulfate is completely dissolved; and adding magnesium oxide and a modifier, and stirring at room temperature to allow magnesium chloride, magnesium sulfate and magnesium oxide to react to obtain the inorganic gel; The providing of plant fiber comprises: The plant fiber raw material is crushed to obtain plant fibers, wherein the plant fibers have a size ranging from 1.5 mm to 2.0 mm.
12. The method for preparing a plate according to claim 10, characterized in that: The mixed material is sequentially paved, cold-pressed and molded, and dried to solidify the inorganic gel to form an inorganic material, and the inorganic board is obtained, including: The mixed material is laid on a pad to obtain a green body, and a plurality of the green bodies are stacked in sequence; Cold-pressing and mold-locking the stacked green bodies to obtain a green body stack; and The green body stack is dried at a temperature of 125° C. to 145° C. to obtain the inorganic board.
13. The method for preparing a plate material according to claim 12, characterized in that: The method of drying the green body stack at a temperature of 125° C. to 145° C. to obtain the inorganic board comprises: Set the mold temperature controller so that the preset outlet temperature of the mold temperature controller is 160°C to 180°C and the preset reflow temperature is 125°C to 145°C; When the reflux temperature of the mold temperature controller reaches the preset reflux temperature, placing the green body stack in the mold temperature controller; In a first time period, the mold temperature controller is turned on every first time period, wherein the first time period includes a plurality of the first time periods; In a second time period, the mold temperature controller is turned on every second sub-time period, wherein the second time period includes a plurality of second time lengths, the second time length is greater than the first time length, and the second time period is after the first time period; and When the reflux temperature is 2° C. to 5° C. higher than the preset reflux temperature, the mold temperature controller is turned on to obtain the inorganic board.
14. The method for preparing a plate material according to claim 10, characterized in that: The preparation method further comprises: Providing a clamping plate and a back plate, and forming a first adhesive layer and a second adhesive layer on two opposite surfaces of the clamping plate respectively; Laying the inorganic plate on the surface of the first adhesive layer away from the clamping plate, and laying the back plate on the surface of the second adhesive layer away from the clamping plate; Performing a first cold pressing at a pressure of 5kg / cm² to 7kg / cm²; and The first hot pressing is performed at a pressure of 8kg / cm² to 13kg / cm² and a temperature of 115°C to 125°C, so that the first adhesive layer forms a first bonding layer and the second adhesive layer forms a second bonding layer; wherein, before the first hot pressing, the moisture content of the backplane is greater than the moisture content of the inorganic board.
15. The method for preparing a plate material according to claim 14, characterized in that: Before the first hot pressing, the moisture content of the back panel is greater than that of the splint, and the moisture content of the splint is greater than that of the inorganic panel; the moisture content of the back panel ranges from 12% to 20%; the moisture content of the splint ranges from 10% to 12%; and the moisture content of the inorganic panel ranges from 4% to 7%.
16. The method for preparing a plate material according to claim 14, characterized in that: The splint provided comprises: Provide adhesives and multi-layer veneers; Applying adhesive on the surface of some of the multi-layer veneers, and stacking the multi-layer veneers in sequence; At a pressure of 5kg / cm 2 Up to 7kg / cm 2 Performing a second cold pressing; and At a pressure of 8kg / cm 2 Up to 13kg / cm 2 , a second hot pressing is performed at a temperature of 115°C to 125°C to solidify the adhesive to form an adhesive layer, and the plywood is obtained, wherein the plywood includes multiple layers of adhesive layers and multiple layers of veneers, the adhesive layers and the veneers are alternately stacked in sequence, the fibers of one of the two adjacent layers of veneers extend along a first direction, and the fibers of the other extend along a second direction, wherein the first direction intersects with the second direction.