Emulsion type thickener for enhanced oil recovery and preparation method thereof
By synthesizing cationic rigid monomers and embedding polyacrylamide molecular chains, a new quaternary copolymer is formed, which solves the problem of poor temperature and salt resistance of polyacrylamide thickeners in high-temperature and high-salt environments, and realizes the development of thickeners. Improved performance and enhanced sand carrying capacity.
Patent Information
- Application Number
- CN202411091908.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Polyacrylamide thickener has poor temperature and salt resistance in high-temperature and high-salt environments, which limits its wide application in oil fields.
By synthesizing benzaldehyde and 1,4-lutidine as a cationic rigid monomer, and embedding strong polar groups in the polyacrylamide molecular chain, a new quaternary copolymer is formed to improve the temperature and salt resistance of the thickener. performance.
It significantly improves the temperature and salt resistance of the thickener, enhances the sand-carrying capacity and hydrodynamic properties, reduces the apparent viscosity drop rate, and improves the hydrolysis resistance of the amide group.
Smart Images

Figure CN118599056B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thickeners, and specifically relates to an emulsion type thickener for enhancing oil recovery and a preparation method thereof. Background Art
[0002] Fracturing fluid refers to a heterogeneous and unstable chemical system formed by a certain ratio of multiple additives. It is a working fluid used for fracturing oil and gas layers. Its main function is to transfer the high pressure formed by ground equipment to the formation, so that the formation breaks to form cracks and transport proppants along the cracks. At present, fracturing fluids are mainly guar gum, clean fracturing fluid and polymer fracturing fluid. Polymer fracturing fluid has the advantages of low price, good sand carrying capacity, low friction and low damage, so it is widely used. Polyacrylamide is one of the most widely used artificial synthetic polymers in oil fields. It has cationic, anionic, non-ionic and zwitterionic types. Polyacrylamide can be formed by homopolymerization or copolymerization with acrylamide as the main monomer. It has the advantages of simple preparation method, low price, high molecular weight, good water solubility, easy modification, and no degradation by microorganisms. However, the application of polyacrylamide is severely restricted in high temperature and high salt environments.
[0003] The existing technology currently has the following main problems: polyacrylamide thickener has poor temperature and salt resistance. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides an emulsion-type thickener for enhancing oil recovery and a preparation method thereof. In order to solve the problem of poor heat and salt resistance of polyacrylamide thickener, the present invention proposes to obtain a monomer that combines hydrophobicity, cationism and rigidity by synthesizing a cationic rigid monomer by using benzaldehyde and 1,4-dimethylpyridine-1-iodide, and at the same time embedding a strong polar group in the polyacrylamide molecular chain to obtain a new type of tetrapolymer, thereby achieving the improvement of the heat and salt resistance of the polyacrylamide thickener.
[0005] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is as follows: The present invention proposes an emulsion-type thickener for enhancing oil recovery, which is prepared from the following components in parts by weight: 10-15 parts of emulsifier, 30-40 parts of deionized water, 35-45 parts of acrylamide, 25-35 parts of 2-acrylamide-2-methylpropane sulfonic acid, 4-5 parts of acrylic acid and 0.7-0.9 parts of cationic rigid monomer.
[0006] Preferably, the cationic rigid monomer is prepared by comprising the following components in parts by weight: 5.5-6.5 parts of benzaldehyde and 11.5-13.5 parts of 1,4-dimethylpyridine-1-iodide.
[0007] Preferably, the method for preparing the cationic rigid monomer comprises the following steps:
[0008] S1, adding benzaldehyde to 99.5wt% anhydrous ethanol, stirring to dissolve, then adding 1,4-dimethylpyridine-1-iodide, stirring to dissolve to obtain a mixed solution;
[0009] S2, adding piperidine dropwise into the mixed solution obtained in S1, and refluxing at 80° C. for 24 h in an argon atmosphere to obtain a reaction solution;
[0010] S3. Cool the reaction solution obtained in S2, filter to obtain a precipitate, add the precipitate into 99.5 wt % anhydrous ethanol, recrystallize, filter and dry to obtain a cationic rigid monomer.
[0011] Preferably, in S1, the amount of benzaldehyde added to 99.5wt% anhydrous ethanol is 0.026-0.03g / mL.
[0012] Preferably, in S2, the amount of piperidine added to the mixed solution obtained in S1 is 0.02-0.025 g / mL.
[0013] Preferably, in S3, the reaction solution is cooled to a temperature of 15-25°C.
[0014] The present invention also provides a method for preparing an emulsion-type thickener for enhanced oil recovery, which specifically comprises the following steps:
[0015] (1) adding an emulsifier to a reaction kettle, adding deionized water, stirring evenly, introducing nitrogen to expel air, and sequentially adding acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, acrylic acid, and a cationic rigid monomer to obtain a mixed solution;
[0016] (2) Add 10 mol / L NaOH solution to the mixed solution and adjust the pH to 8. Then, in a nitrogen atmosphere, add sodium persulfate and sodium bisulfite in a molar ratio of 1:1.2, and a total mass of 0.2% of the mass of the polymerized monomer. Stir vigorously at 1200 rpm for 10 min, and then stir in a water bath to obtain an emulsion-type thickener for enhanced oil recovery.
[0017] Preferably, in step (2), the water bath stirring temperature is 20-30°C, the speed is 80-120 rpm, and the time is 4-6 hours.
[0018] The beneficial effects achieved by the present invention are as follows: the present invention prepares a cationic rigid monomer that integrates hydrophobicity, cation and rigidity, and at the same time embeds a strong polar group in the polyacrylamide molecular chain to obtain a novel quaternary copolymer, thereby achieving the improvement of the heat and salt resistance of the thickener; acrylamide and acrylic acid provide an amide group and a carboxyl group for the thickener, which can be cross-linked with metals on the one hand, and on the other hand, the two groups can be adsorbed with sand particles through hydrogen bonds, thereby improving the sand carrying capacity of the fracturing fluid; the oxygen atom of the carbonyl group in the molecular structure of 2-acrylamide-2-methylpropane sulfonic acid can complex and adsorb metal cations to increase salt resistance; the cations in the cationic rigid monomer can produce a repulsive effect with the metal cations, thereby keeping the polymer molecular chain stretched in the salt solution, and at the same time, can adsorb negatively charged sand particles to improve the sand carrying capacity, the benzene ring can increase its fluid mechanics volume, and the introduction increases the steric hindrance, thereby improving the heat resistance and also improving the hydrolysis resistance of the amide group. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The results of the salt tolerance test of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.
[0020] Figure 2 The results of the heat resistance tests of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.
[0021] Figure 3 The synthetic flow chart of the cationic rigid monomer prepared by the present invention;
[0022] Figure 4 The present invention is a synthetic flow chart of the emulsion thickener for enhanced oil recovery prepared by the present invention.
[0023] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0025] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0026] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0027] Example 1
[0028] An emulsion type thickener for enhancing oil recovery is prepared from the following components in parts by weight: 10 parts of emulsifier, 30 parts of deionized water, 35 parts of acrylamide, 25 parts of 2-acrylamide-2-methylpropane sulfonic acid, 4 parts of acrylic acid and 0.7 parts of a cationic rigid monomer.
[0029] The cationic rigid monomer is prepared by including the following components in parts by weight: 5.5 parts of benzaldehyde and 11.5 parts of 1,4-dimethylpyridine-1-iodide.
[0030] The preparation method of the cationic rigid monomer specifically comprises the following steps:
[0031] S1. Add benzaldehyde in an amount of 0.026 g / mL to 99.5 wt % anhydrous ethanol, stir to dissolve, then add 1,4-dimethylpyridine-1-iodide, stir to dissolve to obtain a mixed solution;
[0032] S2, adding piperidine in an amount of 0.02 g / mL dropwise into the mixed solution obtained in S1, and refluxed at 80° C. for 24 h in an argon atmosphere to obtain a reaction solution;
[0033] S3. Cool the reaction solution obtained in S2 to 15° C., filter to obtain a precipitate, add the precipitate into 99.5 wt % anhydrous ethanol, recrystallize, filter and dry to obtain a cationic rigid monomer.
[0034] The present invention also provides a method for preparing an emulsion-type thickener for enhanced oil recovery, which specifically comprises the following steps:
[0035] (1) adding an emulsifier to a reaction kettle, adding deionized water, stirring evenly, introducing nitrogen to expel air, and sequentially adding acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, acrylic acid, and a cationic rigid monomer to obtain a mixed solution;
[0036] (2) Add 10 mol / L NaOH solution to the mixed solution and adjust the pH to 8. Then, in a nitrogen atmosphere, add sodium persulfate and sodium bisulfite in a molar ratio of 1:1.2, and the total mass is 0.2% of the mass of the polymerized monomer. Stir at 1200 rpm for 10 min, and then stir at 80 rpm in a 20°C water bath for 4 h to obtain an emulsion-type thickener for enhanced oil recovery.
[0037] Example 2
[0038] An emulsion type thickener for enhancing oil recovery is prepared from the following components in parts by weight: 15 parts of emulsifier, 40 parts of deionized water, 45 parts of acrylamide, 35 parts of 2-acrylamide-2-methylpropane sulfonic acid, 5 parts of acrylic acid and 0.9 parts of a cationic rigid monomer.
[0039] The cationic rigid monomer is prepared by including the following components in parts by weight: 6.5 parts of benzaldehyde and 13.5 parts of 1,4-dimethylpyridine-1-iodide.
[0040] The preparation method of the cationic rigid monomer specifically comprises the following steps:
[0041] S1. Add benzaldehyde in an amount of 0.03 g / mL to 99.5 wt % anhydrous ethanol, stir to dissolve, then add 1,4-dimethylpyridine-1-iodide, stir to dissolve to obtain a mixed solution;
[0042] S2, adding piperidine in an amount of 0.025 g / mL dropwise into the mixed solution obtained in S1, and refluxed at 80° C. for 24 h in an argon atmosphere to obtain a reaction solution;
[0043] S3. Cool the reaction solution obtained in S2 to 25° C., filter to obtain a precipitate, add the precipitate into 99.5 wt % anhydrous ethanol, recrystallize, filter and dry to obtain a cationic rigid monomer.
[0044] The present invention also provides a method for preparing an emulsion-type thickener for enhanced oil recovery, which specifically comprises the following steps:
[0045] (1) adding an emulsifier to a reaction kettle, adding deionized water, stirring evenly, introducing nitrogen to expel air, and sequentially adding acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, acrylic acid, and a cationic rigid monomer to obtain a mixed solution;
[0046] (2) Add 10 mol / L NaOH solution to the mixed solution and adjust the pH to 8. Then, in a nitrogen atmosphere, add sodium persulfate and sodium bisulfite in a molar ratio of 1:1.2, and the total mass is 0.2% of the mass of the polymerized monomer. Stir at 1200 rpm for 10 min, and then stir at 120 rpm in a 30°C water bath for 6 h to obtain an emulsion-type thickener for enhanced oil recovery.
[0047] Example 3
[0048] An emulsion type thickener for enhancing oil recovery is prepared from the following components in parts by weight: 12.5 parts of emulsifier, 35 parts of deionized water, 40 parts of acrylamide, 30 parts of 2-acrylamide-2-methylpropane sulfonic acid, 4.5 parts of acrylic acid and 0.8 parts of cationic rigid monomer.
[0049] The cationic rigid monomer is prepared by including the following components in parts by weight: 6 parts of benzaldehyde and 12.5 parts of 1,4-dimethylpyridine-1-iodide.
[0050] The preparation method of the cationic rigid monomer specifically comprises the following steps:
[0051] S1. Add benzaldehyde in an amount of 0.028 g / mL to 99.5 wt % anhydrous ethanol, stir to dissolve, then add 1,4-dimethylpyridine-1-iodide, stir to dissolve to obtain a mixed solution;
[0052] S2, adding piperidine in an amount of 0.0225 g / mL dropwise into the mixed solution obtained in S1, and refluxing at 80° C. for 24 h in an argon atmosphere to obtain a reaction solution;
[0053] S3. Cool the reaction solution obtained in S2 to 20° C., filter to obtain a precipitate, add the precipitate into 99.5 wt % anhydrous ethanol, recrystallize, filter and dry to obtain a cationic rigid monomer.
[0054] The present invention also provides a method for preparing an emulsion-type thickener for enhanced oil recovery, which specifically comprises the following steps:
[0055] (1) adding an emulsifier to a reaction kettle, adding deionized water, stirring evenly, introducing nitrogen to expel air, and sequentially adding acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, acrylic acid, and a cationic rigid monomer to obtain a mixed solution;
[0056] (2) Add 10 mol / L NaOH solution to the mixed solution and adjust the pH to 8. Then, in a nitrogen atmosphere, add sodium persulfate and sodium bisulfite in a molar ratio of 1:1.2, and the total mass is 0.2% of the mass of the polymerized monomer. Stir at 1200 rpm for 10 min, and then stir at 100 rpm for 5 h in a 25°C water bath to obtain an emulsion-type thickener for enhanced oil recovery.
[0057] Comparative Example 1
[0058] This comparative example provides a thickener, which is different from Example 1 only in that all components do not contain a cationic rigid monomer, and the remaining components and component contents are the same as those in Example 1.
[0059] Comparative Example 2
[0060] This comparative example provides a thickener, which differs from Example 1 only in that styrene is used to replace the cationic rigid monomer in all components, and the remaining components and component contents are the same as those in Example 1.
[0061] Experimental example
[0062] The rheometer used for the experimental determination of the apparent viscosity of the solution was an M5600 high temperature and high pressure rheometer with a shear rate of 80 s -1 .
[0063] 1. Salt resistance test
[0064] The examples 1-3 and comparative examples 1-2 were prepared into 1.2 wt% aqueous solutions with deionized water, and the apparent viscosity was tested with 0.1 g / mL-1 g / mL NaCl solution at 25°C. The apparent viscosity reduction rate was calculated by the following formula:
[0065] Apparent viscosity decrease rate = (0.1 g / mL apparent viscosity + 1 g / mL apparent viscosity) / 0.1 g / mL apparent viscosity.
[0066] Figure 1 The results of the salt resistance test of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in the figure; as shown in the figure, the apparent viscosity reduction rates of Examples 1-3 and Comparative Examples 1-2 are 32.65%, 34.21%, 31.35% and 52.33%, 65.16%, respectively, and the apparent viscosity reduction rate of Example 1-3 is significantly lower than that of Comparative Example 1-2, indicating that the use of cationic rigid monomers enhances the salt resistance of the thickener.
[0067] 2. Temperature resistance test
[0068] Example 1-3 and Comparative Example 1-2 were prepared into a 1.2 wt% aqueous solution with deionized water. The temperature was raised from 20°C at a rate of 5°C / min. The apparent viscosity was recorded at 20°C and 80°C, and the apparent viscosity reduction rate was calculated using the following formula:
[0069] Apparent viscosity decrease rate = (20℃ apparent viscosity - 80℃ apparent viscosity) / 20℃ apparent viscosity.
[0070] Figure 2 The result graph of the heat resistance test of Examples 1-3 and Comparative Examples 1-2 of the present invention is shown; as shown in the figure, the apparent viscosity reduction rates of Examples 1-3 and Comparative Examples 1-2 are 25.62%, 26.89%, 25.66% and 46.38%, 59.64%, respectively. The apparent viscosity reduction rate of Example 1-3 is significantly lower than that of Comparative Example 1-2, indicating that the use of cationic rigid monomers enhances the temperature resistance of the thickener.
[0071] Figure 3 The synthetic flow chart of the cationic rigid monomer prepared by the present invention; as shown in the figure, the monomer has a hydrophobic rigid benzene ring structure and a positively charged group.
[0072] Figure 4The synthetic flow chart of the emulsion thickener for enhanced oil recovery prepared by the present invention; as shown in the figure, the polymer is a quaternary polymer composed of acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, acrylic acid, and a cationic rigid monomer.
[0073] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.
[0074] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. An emulsion type thickener for enhanced oil recovery, It is characterized in that The invention is prepared from the following components in parts by weight: 10-15 parts of emulsifier, 30-40 parts of deionized water, 35-45 parts of acrylamide, 25-35 parts of 2-acrylamide-2-methylpropanesulfonic acid, 4-5 parts of acrylic acid and 0.7-0.9 parts of cationic rigid monomer; the cationic rigid monomer is prepared from the following components in parts by weight: 5.5-6.5 parts of benzaldehyde and 11.5-13.5 parts of 1,4-dimethylpyridine-1-iodide; the structure of the cationic rigid monomer is: .
2. A method for preparing the emulsion type thickener for enhanced oil recovery according to claim 1, It is characterized in that The specific steps include: (1) adding an emulsifier to a reaction kettle, adding deionized water, stirring evenly, introducing nitrogen to expel air, and sequentially adding acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, acrylic acid, and a cationic rigid monomer to obtain a mixed solution; (2) Add 10 mol / L NaOH solution to the mixed solution and adjust the pH to 8. Then, in a nitrogen atmosphere, add sodium persulfate and sodium bisulfite in a molar ratio of 1:1.2, and a total mass of 0.2% of the mass of the polymerized monomer. Stir vigorously at 1200 rpm for 10 min, and then stir in a water bath to obtain an emulsion-type thickener for enhanced oil recovery.
3. The method for preparing the emulsion type thickener for enhanced oil recovery according to claim 2, Features: In step (2), the water bath stirring temperature is 20-30°C, the speed is 80-120 rpm, and the time is 4-6 hours.
4. The method for preparing the emulsion type thickener for enhanced oil recovery according to claim 3, Features: The method for preparing the cationic rigid monomer specifically comprises the following steps: S1, adding benzaldehyde to 99.5wt% anhydrous ethanol, stirring to dissolve, then adding 1,4-dimethylpyridine-1-iodide, stirring to dissolve to obtain a mixed solution; S2, adding piperidine dropwise into the mixed solution obtained in S1, and reacting under reflux at 80° C. for 24 h in an argon atmosphere to obtain a reaction solution; S3. Cool the reaction solution obtained in S2, filter to obtain a precipitate, add the precipitate into 99.5 wt % anhydrous ethanol, recrystallize, filter and dry to obtain a cationic rigid monomer.
5. The method for preparing the emulsion type thickener for enhanced oil recovery according to claim 4, Features: In S1, the amount of benzaldehyde added to 99.5wt% anhydrous ethanol is 0.026-0.03g / mL.
6. The method for preparing the emulsion type thickener for enhanced oil recovery according to claim 5, Features: In S2, the amount of piperidine added to the mixed solution obtained in S1 is 0.02-0.025 g / mL.
7. The method for preparing the emulsion type thickener for enhanced oil recovery according to claim 6, Features: In S3, the reaction solution is cooled to a temperature of 15-25°C.