Method for preparing low temperature resistant perfluoroether elastomer by radiation crosslinking

Through the two-step process of radiation cross-linking and high-temperature vulcanization, the problems of low efficiency and insufficient low-temperature resistance of traditional high-temperature vulcanization cross-linking methods are solved, and the mechanical strength and plasma etching resistance of perfluoroether rubber are improved, achieving a more efficient preparation process.

CN118599145BActive Publication Date: 2024-10-01SHANGHAI MORISEAL NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411087655.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-01
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Traditional high-temperature vulcanization cross-linking methods lead to the decomposition of unstable end groups in fluoroelastomers, which reduces production efficiency and mechanical strength, and limits the application of low-temperature-resistant perfluoroether elastomers in semiconductor manufacturing processes.

Method used

The radiation cross-linking method is used to obtain perfluoroether elastomer micropowder through emulsion polymerization, and solid-liquid phase reaction grafting is performed at room temperature, combined with high-temperature vulcanization to reduce the amount of vulcanizing agent and cross-linking accelerator, and improve mechanical strength and plasma resistance. Etching performance.

Benefits of technology

It is possible to improve the mechanical properties and cleanliness of fluoroelastomers without adding carbon black and acid absorbers, reduce high-temperature vulcanization time, maintain low-temperature resistance, and improve the mechanical strength and plasma engraving resistance of perfluoroether rubber products. Corrosion performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118599145B_ABST
    Figure CN118599145B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a low-temperature resistant perfluoroether elastomer by radiation crosslinking, which belongs to the field of fluoroelastomers, including emulsion polymerization of perfluoroalkoxyalkyl vinyl ether, tetrafluoroethylene, perfluoroalkyl vinyl ether and vulcanization point monomers by weight to obtain a perfluoroether elastomer emulsion, and after condensation, washing and drying and devolatilization, the end groups are kept or the end groups are passivated to obtain a perfluoroether elastomer powder; the perfluoroether elastomer powder is mixed with a liquid rubber containing an active end group under the condition of 60-90°C, and the solid-liquid phase reaction grafting is carried out by radiation crosslinking at room temperature for the first time, and then a vulcanizing agent and a crosslinking accelerator and modified PTFE powder are added to continue mixing to obtain a mixed rubber; the mixed rubber is molded, and after the second room temperature radiation crosslinking, high temperature vulcanization is performed to obtain a low-temperature resistant perfluoroether elastomer composition. Through the processing scheme of the present application, the low-temperature resistance of the perfluoroether elastomer is maintained and the mechanical strength and plasma etching resistance of its products are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fluoroelastomers, and in particular to a method for preparing low-temperature resistant perfluoroether elastomer through radiation cross-linking. Background Art

[0002] Fluoroelastomer compositions are widely used in sealing, insulating and protective materials in the fields of chemical industry, nuclear industry, etc. The properties of fluoroelastomer compositions depend on the selected formula and processing technology. The vulcanization process is a very critical link in the processing technology, including high-temperature vulcanization cross-linking and room-temperature radiation vulcanization cross-linking. High-temperature vulcanization cross-linking is a commonly used method that uses a vulcanizing agent at high temperature for cross-linking, which requires a long vulcanization time and consumes a lot of energy.

[0003] When preparing fluoroelastomer compositions, the existing traditional high temperature crosslinking has the following problems:

[0004] The traditional high temperature vulcanization cross-linking method requires a long vulcanization time, which reduces production efficiency and consumes a lot of energy. At the same time, the traditional high temperature vulcanization cross-linking method easily causes the unstable end groups in the fluoroelastomer to decompose into volatile components to form pores, affecting the performance of the fluoroelastomer composition.

[0005] In addition, the existing low-temperature resistant perfluoroether elastomers need to introduce low-temperature resistant modified monomers such as vinylidene fluoride when synthesizing the emulsion, and have poor plasma etching resistance, which limits their application in semiconductor processes.

[0006] Therefore, it is necessary to provide a new preparation method to solve these problems. Summary of the invention

[0007] Therefore, in order to overcome the above-mentioned shortcomings of the prior art, the present invention provides a method for preparing a low-temperature resistant perfluoroether elastomer by radiation crosslinking, which improves the mechanical strength and plasma etching resistance of the perfluoroether rubber product while maintaining the low-temperature resistance.

[0008] In order to achieve the above-mentioned object, the present invention provides a method for preparing a low-temperature resistant perfluoroether elastomer through radiation crosslinking, comprising: S1, emulsion polymerizing 10 to 20 parts by weight of a perfluoroalkoxyalkyl vinyl ether having a total carbon number of 5 to 15, 22 to 59 parts of tetrafluoroethylene, 30 to 55 parts of a perfluoroalkyl vinyl ether and 1 to 2 parts of a sulfide point monomer containing bromine or iodine to obtain a perfluoroether elastomer emulsion, and obtaining a perfluoroether elastomer powder after condensation, washing, drying and devolatilization, and maintaining or passivating the end groups; the perfluoroalkyl vinyl ether comprises at least one of perfluoromethyl vinyl ether, perfluoroethyl vinyl ether and perfluoropropyl vinyl ether; S2, heating the emulsion at 60 to 90 °C. ℃, mixing perfluoroether elastomer powder with 1~15 parts of liquid rubber containing active end groups, performing solid-liquid phase reaction grafting by radiation crosslinking at room temperature for the first time, and then adding 0.5~2 parts of vulcanizing agent and 1~2.5 parts of crosslinking accelerator and 5~20 parts of modified PTFE powder to continue mixing and kneading to obtain a rubber mixture, wherein the liquid rubber containing active end groups is a linear perfluoropolyether with a molecular weight of 2000-4000; S3, molding the rubber mixture, performing radiation crosslinking at room temperature for the second time and then vulcanizing at high temperature to obtain a low-temperature resistant perfluoroether elastomer composition, wherein the first radiation crosslinking dose is 10-40 kGy, and the second radiation crosslinking dose is 10-100 kGy.

[0009] In one embodiment, the modified PTFE micropowder has a tetrafluoroethylene content of 80-99 wt %, and a perfluoroalkyl vinyl ether content of 1-20 wt %.

[0010] In one embodiment, the active end group is a carboxyl group or a hydroxymethyl group.

[0011] In one embodiment, the perfluoroalkoxyalkyl vinyl ether is at least one of CF3OCF2OCF2CF2OCF=CF2, CF3CF2CF2(OCF2CF2CF2)3OCF=CF2, CF3CF2OCF2OCF=CF2, and CF3(OCF2CF2CF2)4OCF=CF2.

[0012] In one embodiment, the sulfurization site monomer is 4-bromo-tetrafluoro-1-butene or 4-iodo-tetrafluoro-1-butene.

[0013] In one embodiment, the vulcanizing agent includes at least one of bisphenol AF, di-tert-butyl peroxide isocyanurate, and dipentadienyl vulcanizing agent, and the crosslinking accelerator is triallyl isocyanurate.

[0014] In one embodiment, the end group passivation is to treat the dry fluoroelastomer powder with fluorine or NF3, N2 is the balance gas during the passivation process, and the volume ratio of fluorine or NF3 in the total gas is 10%.

[0015] In one embodiment, the drying in S1 includes low-temperature drying or vacuum drying, and liquid or supercritical CO2 devolatilization is used after drying.

[0016] In one embodiment, the radiation cross-linking is performed at room temperature using a linear electron accelerator.

[0017] In one embodiment, the high temperature vulcanization condition of S3 is a vulcanization temperature of 180-220° C. and a vulcanization time of 0.5-4 hr.

[0018] Compared with the prior art, the advantages of the present invention are: by radiation, the vulcanization cross-linking and mechanical properties of the elastomer are achieved without adding carbon black and acid absorbent, and the cleanliness of the elastomer is improved; and the room temperature radiation cross-linking is divided into two steps, the first room temperature radiation is solid-liquid phase reaction grafting, and the second room temperature radiation can greatly reduce the high temperature vulcanization time, reduce the amount of vulcanizing agent and cross-linking accelerator, while maintaining the low temperature resistance, on the basis of reducing the low temperature compression permanent deformation, improve the mechanical strength and plasma etching resistance of the perfluoroether rubber product. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 It is a simplified flow chart of the method for preparing low-temperature resistant perfluoroether elastomer by radiation cross-linking in an embodiment of the present invention. DETAILED DESCRIPTION

[0021] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0022] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0023] It should be noted that various aspects of the embodiments within the scope of protection of the present invention are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0024] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0025] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0026] like Figure 1 As shown, the present application embodiment provides a method for preparing a low-temperature resistant perfluoroether elastomer by radiation cross-linking, comprising the following steps:

[0027] S1. According to weight, 10 to 20 parts of perfluoroalkoxyalkyl vinyl ether with a total carbon number of 5 to 15, 22 to 59 parts of tetrafluoroethylene, 30 to 55 parts of perfluoroalkyl vinyl ether and 1 to 2 parts of bromine or iodine-containing vulcanization point monomers are subjected to emulsion polymerization to obtain a perfluoroether elastomer emulsion, and after condensation, washing, drying and devolatilization, and maintaining the end group or passivating the end group, a perfluoroether elastomer powder is obtained. The perfluoroalkyl vinyl ether includes at least one of perfluoromethyl vinyl ether, perfluoroethyl vinyl ether and perfluoropropyl vinyl ether. The bromine or iodine-containing vulcanization point monomers include R1CH=CR2CR3, R f -I and IR f -I, wherein R1, R2, R3 are selected from H, Br, F, R f or R f Br, and at least one of R1, R2, and R3 is Br or R f Br, R f It is a perfluoroalkyl group.

[0028] The temperature of emulsion polymerization is 50~90 ℃.

[0029] The total carbon number of the perfluoroalkoxy alkyl vinyl ether is 5 to 15, and the ratio of the perfluoroalkoxy group to the alkyl group is within a mass ratio of 5 to 15%.

[0030] By introducing perfluoroalkoxyalkyl vinyl ether and perfluoroalkyl vinyl ether, flexible ether bonds are introduced into the side chains of fluoroelastomers to lower the glass transition temperature. The active end groups of liquid rubber are grafted with the main chains of fluoroelastomers through radiation reaction, thereby lowering the glass transition temperature of the perfluoroether elastomer composition, further improving its low temperature resistance, mechanical strength and chemical stability against plasma etching.

[0031] S2. Mix the perfluoroether elastomer powder with 1-15 parts of liquid rubber containing active end groups at 60-90 °C, perform the first room temperature radiation cross-linking for solid-liquid phase reaction grafting, then add 0.5-2 parts of vulcanizing agent and 1-2.5 parts of cross-linking accelerator and 5-20 parts of modified PTFE powder (modified polytetrafluoroethylene powder) and continue mixing to obtain a mixed rubber. The liquid rubber containing active end groups is a linear perfluoropolyether.

[0032] The molecular weight of liquid rubber ranges from 2000 to 4000, and the active end groups are carboxyl or hydroxymethyl.

[0033] There are about 3000 kinds of radiation that can directly or indirectly ionize the air, and any one of them can be selected. The radiation vulcanization crosslinking can be electron beam vulcanization crosslinking or gamma ray radiation vulcanization crosslinking.

[0034] The purpose of the first radiation crosslinking is to cause solid-liquid phase reaction grafting to form the mixed rubber. The radiation dose has a great influence on the performance of the elastomer composition, and the radiation effect is a competitive mechanism. When the rubber is irradiated, the intermolecular crosslinking reaction and the degradation reaction occur simultaneously, that is, on the one hand, the molecular weight of the network macromolecules formed by intermolecular crosslinking continues to increase; on the other hand, the radiation causes the chemical bonds to break and the relative molecular weight decreases. Therefore, the radiation dose is an important parameter for determining the radiation vulcanization and crosslinking process of the elastomer composition. The first radiation crosslinking dose is 10-40 kGy. Radiation is calculated by dose. When doing the experiment, the sample is placed on the turntable, and the dose is calculated once, and finally the total dose is calculated according to the number of times.

[0035] Electron beam radiation vulcanization technology uses high-energy electron beams emitted by electron accelerators to activate elastomer molecules in the elastomer matrix, generate elastomer macromolecular free radicals, and cross-link elastomer macromolecules to form a three-dimensional network structure. In addition to ions, electrons, and excited molecules, the primary chemical products formed by radiation also include free radicals and certain molecular products. These primary particles are highly active and can undergo a variety of reactions such as cracking, rearrangement, electron transfer, dehydrogenation, and addition. Usually, radiation vulcanization and cross-linking do not require the addition of vulcanizing agents and are carried out at room temperature and pressure. Compared with traditional high-temperature vulcanization processes, electron beam radiation vulcanization and cross-linking processes can improve the aging resistance of fluoroelastomer compositions and accelerate the vulcanization rate.

[0036] S3, molding the mixed rubber, subjecting it to a second room temperature radiation cross-linking and then vulcanizing it at a high temperature to obtain a low temperature resistant perfluoroether elastomer composition.

[0037] In this embodiment, due to the use of radiation cross-linking to assist high temperature cross-linking, the dosage of the added vulcanizing agent and cross-linking accelerator is reduced by about half compared with conventional high temperature vulcanization, thereby improving the mechanical properties and plasma resistance of the elastomer. The second radiation cross-linking dosage is 10-100 kGy.

[0038] In one embodiment, the high temperature vulcanization condition of S3 is a vulcanization temperature of 180-220° C. and a vulcanization time of 0.5-4 hr.

[0039] Radiation vulcanization cross-linking combined with conventional high-temperature vulcanization cross-linking can significantly reduce the vulcanization time and improve the mechanical properties and plasma resistance of the product.

[0040] The above method realizes the vulcanization cross-linking of the elastomer through radiation without adding carbon black and acid absorbent, thereby improving the mechanical properties of the fluoroelastomer; and the room temperature radiation cross-linking is divided into two steps. The first room temperature radiation is solid-liquid phase reaction grafting, and the second room temperature radiation is to reduce the high temperature vulcanization time and reduce the amount of vulcanizing agent and cross-linking accelerator. While maintaining the low temperature resistance, the mechanical strength and plasma etching resistance of the perfluoroether rubber product are improved.

[0041] In one embodiment, the tetrafluoroethylene content in the modified PTFE micropowder is 80-99 wt %, and the perfluoroalkyl vinyl ether content is 1-20 wt %.

[0042] Modified PTFE micropowder is obtained by emulsion polymerization of TFE monomer (tetrafluoroethylene) and PMVE (perfluoromethyl vinyl ether) or PPVE monomer (perfluoro-n-propyl vinyl ether) at 50-80 ℃ and 1.85-2.07 MPa.

[0043] In one embodiment, the active terminal group is a carboxyl group or a hydroxymethyl group.

[0044] In one embodiment, the perfluoroalkoxyalkyl vinyl ether is at least one of CF3OCF2OCF2CF2OCF=CF2, CF3CF2CF2(OCF2CF2CF2)3OCF=CF2, CF3CF2OCF2OCF=CF2, and CF3(OCF2CF2CF2)4OCF=CF2.

[0045] In one embodiment, the cure site monomer is 4-bromo-tetrafluoro-1-butene or 4-iodo-tetrafluoro-1-butene.

[0046] In one embodiment, the vulcanizing agent includes at least one of bisphenol AF, di-tert-butyl peroxide isocyanurate, and dipentadienyl vulcanizing agent, and the crosslinking accelerator is triallyl isocyanurate (TAIC).

[0047] In one embodiment, the end group passivation is to treat the dried fluoroelastomer powder with fluorine or NF3, N2 is the balance gas during the passivation process, and the volume ratio of fluorine or NF3 in the total gas is 10%. The volume ratio of F2 or NF3 and the balance gas N2 is 10:90, so the volume ratio of F2 or NF3 in the total gas is 10%.

[0048] In one embodiment, the drying in S1 includes low temperature drying or vacuum drying, and liquid or supercritical CO2 devolatilization is used after drying.

[0049] In one embodiment, the radiation crosslinking is performed at room temperature using a linear electron accelerator, specifically, the linear electron accelerator is an ISO24 model, with a power of 24 kW and an electron energy of 10 MeV.

[0050] In the present application, emulsion polymerization, mixing and thin-pass and compression molding processes are conventional processes in the industry.

[0051] Examples 1-3

[0052] S1. 11.5 g CF3OCF2OCF2CF2OCF=CF2 (Cas No 39654-39-2), 42 g tetrafluoroethylene, 45 g perfluoromethyl vinyl ether and 1.5 g 4-bromo-tetrafluoro-1-butene monomer are subjected to emulsion polymerization to obtain a perfluoroether elastomer emulsion; the perfluoroether elastomer emulsion is condensed, washed and vacuum dried, and devolatilized by supercritical CO2 to obtain a perfluoroether elastomer powder.

[0053] S2. At 80 °C, mix the perfluoroether elastomer powder with 8 g of liquid rubber Famlbin Z Diac (HOOCCF2O(CF2CF2O) containing active end groups. m (CF2O) nCOOH, molecular weight about 2000) was mixed, and the first room temperature radiation cross-linking was carried out for solid-liquid phase reaction grafting, and the radiation dose was 20 kGy; 1 g of vulcanizing agent di-25 and 1.5 g of cross-linking accelerator TAIC (triallyl isocyanurate) were added, and 13 g of PTFE powder was continued to mix and thin to obtain a mixed rubber. The tetrafluoroethylene content in the PTFE powder was 94.5 wt%, and the perfluoropropyl vinyl ether content was 5.5 wt%.

[0054] S3, the mixed rubber is molded and subjected to a second room temperature radiation crosslinking, with radiation doses of 40 kGy, 60 kGy, and 80 kGy, respectively, and vulcanized at 200 °C for 1 hr to obtain a perfluoroether elastomer composition, corresponding to Examples 1, 2, and 3, respectively.

[0055] The proportions of the components in Examples 1 to 3 are the same, and the difference lies in the second radiation dose.

[0056] Comparative Examples 1-3

[0057] S1. 11.5 g CF3OCF2OCF2CF2OCF=CF2 (Cas No 39654-39-2), 42 g tetrafluoroethylene, 45 g perfluoromethyl vinyl ether and 1.5 g 4-bromo-tetrafluoro-1-butene monomer are subjected to emulsion polymerization to obtain a perfluoroether elastomer emulsion; the perfluoroether elastomer emulsion is condensed, washed and vacuum dried, and devolatilized by supercritical CO2 to obtain a perfluoroether elastomer powder.

[0058] S2. At 80 °C, mix the perfluoroether elastomer powder with 8 g of liquid rubber Famlbin Z Diac (HOOCCF2O(CF2CF2O) containing active end groups. m (CF2O) n COOH, molecular weight about 2000) was mixed, 2 g of vulcanizing agent dichlorobenzene and 3 g of crosslinking accelerator TAIC were added, and 13 g of PTFE powder was continued to mix and knead to obtain a mixed rubber. The tetrafluoroethylene content in the PTFE powder was 94.5 wt%, and the perfluoropropyl vinyl ether content was 5.5 wt%.

[0059] S3, molding the mixed rubber, and performing secondary vulcanization by conventional high temperature vulcanization, the high temperature vulcanization temperature is 200° C., the vulcanization time is 18 hr, 20 hr, and 24 hr, to obtain a perfluoroether elastomer composition.

[0060] The proportions of the components in Control Examples 1 to 3 are the same, and the difference lies in the different vulcanization times.

[0061] Main test results of the examples and comparative examples of this application

[0062]

[0063] The plasma etching conditions are: 13.56 MHz, O2 flow rate 50 sccm, pressure 500 mt, and power 800 W.

[0064] The enterprise standard is Q / SMS 001-2024 Test method for plasma etching resistance of perfluoroether rubber seals, which can be obtained through the National Standard Information Public Service Platform.

[0065] The following effects

[0066] The weight loss of the perfluoroether rubber of Comparative Examples 1-3 during plasma etching resistance is 0.42-0.64%, which is greater than 0.18-0.25% of Examples 1-3 of the present application.

[0067] The radiation dose has a great influence on the performance of the elastomer composition, and the radiation effect is a competitive mechanism. When the rubber is irradiated, the intermolecular crosslinking reaction and the degradation reaction occur simultaneously, that is, on the one hand, the relative molecular mass of the network macromolecules formed by intermolecular crosslinking continues to increase; on the other hand, the radiation causes the chemical bonds to break and the relative molecular mass to decrease. Therefore, the radiation dose is an important parameter for determining the radiation vulcanization and crosslinking process of the elastomer composition. From the comparison of Examples 1-3, it can be seen that when the first radiation dose is fixed, the second radiation dose of 60 kGy (corresponding to Example 2) is relatively moderate, and the radiation dose is insufficient below this (corresponding to Example 1), and the radiation dose is too large above this (corresponding to Example 3). However, the plasma etching resistance test of the perfluoroether elastomer composition obtained with the second radiation dose within 10~100 kGy is still higher than the plasma etching resistance test of the comparative example.

[0068] Short-term high-temperature crosslinking (200 °C and 1 hr) is beneficial to improving hardness and resistance to permanent compression set, but the glass transition temperature is slightly reduced (Comparative Example 2). When the perfluoroether elastomer composition needs to be used in a low-temperature environment, the high-temperature crosslinking time can be controlled to reduce the glass transition temperature.

[0069] The present application introduces perfluoroalkoxyalkyl vinyl ether and perfluoroalkyl vinyl ether, introduces flexible ether bonds into the side chains of fluoroelastomers to lower the glass transition temperature, and at the same time, reactively grafts flexible blocks onto the surface of fluoroelastomer micropowders to lower the glass transition temperature of the perfluoroether elastomer composition and improve its low temperature resistance. The obtained perfluoroether elastomer composition has a temperature adaptability range of -43.5-200°C, thereby improving the low temperature resistance, mechanical strength and chemical stability of the perfluoroether elastomer composition against plasma etching.

[0070] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a low-temperature resistant perfluoroether elastomer by radiation crosslinking, characterized in that: include: S1. Emulsion polymerize 10 to 20 parts of a perfluoroalkoxyalkyl vinyl ether having a total carbon number of 5 to 15, 22 to 59 parts of tetrafluoroethylene, 30 to 55 parts of a perfluoroalkyl vinyl ether and 1 to 2 parts of a bromine- or iodine-containing vulcanization point monomer to obtain a perfluoroether elastomer emulsion, and obtain a perfluoroether elastomer powder after coagulation, washing, drying and devolatilization, and maintaining or passivating the end groups, wherein the perfluoroalkyl vinyl ether includes at least one of perfluoromethyl vinyl ether, perfluoroethyl vinyl ether and perfluoropropyl vinyl ether; S2, mixing perfluoroether elastomer powder with 1-15 parts of liquid rubber containing active end groups at 60-90°C, performing solid-liquid phase reaction grafting by radiation crosslinking at room temperature for the first time, and then adding 0.5-2 parts of vulcanizing agent and 1-2.5 parts of crosslinking accelerator and 5-20 parts of modified PTFE powder to continue mixing and kneading to obtain a rubber mixture, wherein the liquid rubber containing active end groups is a linear perfluoropolyether with a molecular weight of 2000-4000; S3. The mixed rubber is molded, subjected to a second room temperature radiation cross-linking and then subjected to high temperature vulcanization to obtain a low temperature resistant perfluoroether elastomer composition, wherein the first radiation cross-linking dose is 10-40 kGy, and the second radiation cross-linking dose is 10-100 kGy.

2. The method according to claim 1, characterized in that: The modified PTFE micropowder has a tetrafluoroethylene content of 80-99 wt %, and a perfluoroalkyl vinyl ether content of 1-20 wt %.

3. The method according to claim 1, characterized in that The active terminal group is a carboxyl group or a hydroxymethyl group.

4. The method according to claim 1, characterized in that: The perfluoroalkoxyalkyl vinyl ether includes at least one of CF3OCF2OCF2CF2OCF=CF2, CF3CF2CF2(OCF2CF2CF2)3OCF=CF2, CF3CF2OCF2OCF=CF2, and CF3(OCF2CF2CF2)4OCF=CF2.

5. The method according to claim 1, characterized in that The sulfurization point monomer is 4-bromo-tetrafluoro-1-butene or 4-iodo-tetrafluoro-1-butene.

6. The method according to claim 1, characterized in that The vulcanizing agent includes at least one of bisphenol AF, di-tert-butyl peroxide isocyanurate and dipentadienyl vulcanizing agent, and the crosslinking accelerator is triallyl isocyanurate.

7. The method according to claim 1, characterized in that The end group passivation is to treat the dried fluoroelastomer powder with fluorine or NF3, during the passivation process, N2 is the balance gas, and the volume ratio of fluorine or NF3 in the total gas is 10%.

8. The method according to claim 1, characterized in that The drying in S1 includes low temperature drying or vacuum drying, and after drying, liquid or supercritical CO2 devolatilization treatment is used.

9. The method according to claim 1, characterized in that: The radiation cross-linking is carried out at room temperature using a linear electron accelerator for radiation.