A method for producing small-section aluminum-containing square billet by slag washing and direct-lifting technology
Through the small section containing aluminum-containing blank slag washing process, combined with molten iron desulfurization, converter smelting and argon station slag washing, the problem of high cost of ladle refining furnace process is solved, and efficient casting blank production is achieved, reducing process costs and shortening The smelting cycle was completed.
Patent Information
- Application Number
- CN202411089281.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-09
AI Technical Summary
When steelmaking enterprises produce qualified casting billets that meet the needs of cold rolling process, the ladle refining furnace process is costly, which affects the production rhythm and daily output. They need to find simple refining methods to replace traditional processes.
The process of washing and washing the slag of the small section containing aluminum is adopted. By combining molten iron desulfurization, converter smelting, argon station slag washing and continuous casting machine casting, the sulfur content, temperature and composition are controlled to achieve efficient desulfurization of molten steel and aluminum. Effective treatment is made to produce qualified small sections containing aluminum blocks.
Compared with the traditional refining process, the slag washing and straight-up process significantly reduces the cost, shortens the smelting cycle, and improves production efficiency.
Smart Images

Figure CN118600149B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and relates to a processing technology for a small-section aluminum-containing rectangular billet, in particular to a slag washing and direct-lifting process production method for a small-section aluminum-containing rectangular billet. Background Art
[0002] As cold-rolled narrow strip products gradually develop into aluminum-containing and high-alloy products, steelmaking companies need to use the ladle refining furnace process to produce qualified ingots that meet the needs of the cold rolling process. However, the process cost of the ladle refining furnace process to produce ingots that meet the quality requirements is high, which will affect the production rhythm and daily output to a certain extent. Therefore, it is necessary to consider using a simpler refining method to replace the ladle refining furnace process.
[0003] In production practice, slag washing is the simplest refining method to obtain clean steel and properly carry out desulfurization and deoxidation. It uses the impact force of high-temperature molten steel and the mixed impact of strong bottom blowing pressure of the ladle during the steelmaking process to fully react with CaO-containing slag and inclusions, and emulsify the molten slag droplets, so that the steel-slag interface is expanded hundreds of times, which greatly increases the opportunity for the steel slag to fully react with inclusions in the steel, and at the same time generates low-melting-point compounds to achieve control of the morphology of Al2O3 inclusions. Summary of the invention
[0004] The purpose of the present invention is to provide a slag washing and direct casting process production method for small-section aluminum-containing rectangular billets. Through the aluminum-containing slag calcium washing treatment direct casting process, the existing process for generating thin-gauge cold-rolled materials is improved to produce qualified small-section aluminum-containing rectangular billets.
[0005] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:
[0006] A slag washing and straight-up process production method for small-section aluminum-containing square billets, comprising:
[0007] S1. When hot metal is desulfurized before entering the station, the sulfur content by mass percentage is required to be ≤0.05%;
[0008] S2, converter smelting, the final molten steel temperature is controlled at 1670-1680℃; fluorine-free slag washing material, high calcium ash, medium carbon ferromanganese, aluminum block are added after the furnace, argon is blown into the steel-making atmosphere, the top slag is melted, and the slag layer thickness is ≤30mm after the steel-making is completed;
[0009] S3, argon station slag washing;
[0010] S4, continuous casting machine casting.
[0011] Preferably, the amount of fluorine-free slag washing material added to S2 is 1 kg / t steel, the amount of high calcium ash is 4 kg / t steel, the amount of medium carbon ferromanganese is 1.7 kg / t steel, and the amount of aluminum block is 1.6 kg / t steel.
[0012] Preferably, the S3 argon station slag washing comprises:
[0013] S31, when the molten steel arrives at the station, argon gas is blown for 1-2 minutes, and the argon gas is adjusted to the soft blowing state to ensure accurate oxygen determination. The required amount of aluminum wire is determined according to the oxygen content, and oxygen control and temperature adjustment are performed. According to the melting condition of the top slag in S2, fluorite powder is added, and then aluminum calcium balls and aluminum chips are added in sequence to remove oxygen from the steel at one time, and the aluminum in the steel and the aluminum in the slag reach the forward and reverse reaction equilibrium within 10 minutes, and the acid-soluble aluminum Als content in the steel is controlled to be 0.02-0.045%;
[0014] S32, strong blowing of argon for 2-3 minutes to dip the top slag sample, adjust the top slag to white slag with basicity above 4.0, continue blowing argon for 1-2 minutes to dip the top slag sample again for identification, and enter the calcium line feeding link after the top slag composition meets the requirements. If the composition does not meet the requirements, fine-tune the composition during the strong blowing period before feeding the calcium line;
[0015] S33. Dip the sample before leaving the station to ensure that the mass percentage of Ca is not less than 0.0015%. After the ladle leaves the station, add the ladle covering agent and cover it at the same time to prevent the molten steel from overoxidation.
[0016] Preferably, the amount of fluorite powder added to S31 is 0.3-0.5kg / t steel, the amount of aluminum calcium balls is 0.7-1kg / t steel, and the amount of aluminum chips is 0.3-0.7kg / t steel.
[0017] Preferably, before feeding the calcium wire in S32, the argon gas is adjusted to a soft blowing state, and 120-150 m of the high calcium wire is fed. After feeding, soft blowing is performed for 12-15 minutes and then the slag sample is dipped for confirmation.
[0018] Preferably, the mass percentage of Ca in the S33 is optimally 0.0020%.
[0019] Preferably, the S4 continuous casting machine casting comprises:
[0020] S41. Preparation before continuous casting: The continuous casting machine needs to clean the water nozzle, water strip, and iron oxide on the roller surface, replace the fulcrum roller, adjust the arc, and ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered;
[0021] S42, the continuous casting ladle adopts a long nozzle combined with a sealing pad and argon gas for full protection pouring. After the ladle is poured, it is protected by a special protective slag containing aluminum rectangular billets. The protective slag must be dry, black surface operation, and small amounts of multiple even pouring;
[0022] S43, the continuous casting tundish adopts a plug rod to control the water flow inlet tundish, the tundish baking time is ≥4.5-6 hours, and the baking temperature is ≥1000℃; the middle of the tundish is opened first, and then the two sides, and the pulling speed is quickly increased to more than 1.2m / min. After the tundish is stably poured, the pulling speed is increased to 1.30-1.35m / min;
[0023] S44, the molten steel is cooled and crystallized in the crystallizer to form a preliminary solid shell;
[0024] S45, the ingot pulled out of the crystallizer enters the secondary cooling zone, where automatic water distribution directly cools the ingot to accelerate solidification;
[0025] S46, the ingot is then straightened by a billet straightening device.
[0026] Preferably, the middle package described in S43 adopts an aluminum-carbon immersion nozzle combined with a sealing gasket for full-process protection pouring. The nozzle baking temperature of the aluminum-carbon immersion nozzle is required to be greater than 800°C, and the insertion depth of the immersion nozzle is 95±10mm; the middle package covering agent adopts a high-alkalinity covering agent, and the mass percentage of acid-soluble aluminum Als loss is ≤0.005%.
[0027] Preferably, the water volume of the crystallizer in S44 is 170-180m 3 / h, the inlet and outlet water temperature difference is 6-8℃.
[0028] Preferably, the straightening temperature in S46 is ≥950°C.
[0029] The beneficial effects of the present invention are:
[0030] Compared with the refining process, the desulfurization effect of the aluminum-containing slag calcium washing process is not much different. Compared with the over-refining process, the cost of the aluminum-containing slag washing process is significantly reduced. Compared with the smelting cycle, the argon blowing time of the aluminum-containing slag washing process is longer than that of the normal process without slag washing, and the smelting cycle of the slag washing process is also significantly shortened compared with the traditional over-refining smelting cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a table of molten steel composition and temperature;
[0032] Figure 2 It is the converter control composition data table;
[0033] Figure 3 It is the process control data table of steel tapping and argon station;
[0034] Figure 4 It is the composition table of the primary sample of the argon station;
[0035] Figure 5 It is the composition table of the samples leaving the argon station;
[0036] Figure 6 It is the slag washing desulfurization rate data table;
[0037] Figure 7 It is the finished product ingredient data table. DETAILED DESCRIPTION
[0038] The present invention will be further described below in conjunction with embodiments:
[0039] A slag washing and straight-up process production method for small-section aluminum-containing square billets, comprising:
[0040] S1. When molten iron is desulfurized before entering the station, the mass percentage of sulfur is required to be ≤0.05%. If the molten iron does not meet the requirements, the slag washing process will be temporarily stopped.
[0041] S2, converter smelting, the final molten steel temperature is controlled at 1670-1680℃; fluorine-free slag washing material 1kg / t steel, high calcium ash 4kg / t steel, medium carbon ferromanganese 1.70kg / t steel, aluminum block 1.6kg / t steel are added after the furnace, argon is blown in the steel-tapping atmosphere, the top slag is melted, and the slag layer thickness is ≤30mm after the steel-tapping is completed.
[0042] S3, argon gas station slag washing;
[0043] S31. When the molten steel arrives at the station, argon is blown strongly for 1-2 minutes, and the argon is adjusted to a soft blowing state to ensure accurate oxygen determination. The required amount of aluminum wire is determined according to the oxygen content, and oxygen is controlled. If the temperature needs to be adjusted, it should be adjusted immediately and only once. No subsequent temperature adjustment action is required. According to the melting of the top slag in S2, the amount of fluorite powder added is 0.3-0.5kg / t steel, the amount of aluminum calcium balls is 0.7-1kg / t steel, and the amount of aluminum chips is 0.3-0.7kg / t steel. The oxygen in the steel is removed once, and the aluminum in the steel and the aluminum in the slag reach a forward and reverse reaction equilibrium within 10 minutes, and the mass percentage of acid-soluble aluminum Als in the steel is controlled to be 0.02-0.045%.
[0044] S32. Strongly blow argon for 2-3 minutes and dip the top slag sample. Adjust the top slag to white slag with alkalinity above 4.0. Continue blowing argon for 1-2 minutes and dip the slag sample again for identification. After the top slag meets the requirements, it enters the calcium wire feeding stage. If the composition does not meet the requirements, fine-tune the composition during the strong blowing period and then feed the calcium wire. Before hitting the calcium wire, adjust the argon to the soft blowing state and feed the high calcium wire for 120-150m. After feeding, soft blow for 12-15min and then dip the slag sample for confirmation.
[0045] S33. Dip the sample before leaving the station to ensure that the mass percentage of Ca is not less than 0.0015%, and the mass percentage of Ca is best at 0.0020%. After the ladle leaves the station, add ladle covering agent and cover it at the same time to prevent the molten steel from overoxidation.
[0046] S4, continuous casting machine casting;
[0047] S41. Preparation before continuous casting: The continuous casting machine needs to clean the water nozzle, water bar, iron oxide on the roller surface, replace the fulcrum roller, adjust the arc, and ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered.
[0048] S42. The continuous casting ladle adopts a long shroud combined with a sealing pad and argon gas for full protection pouring. After the ladle is poured, a special protective slag containing aluminum rectangular billets is used for protection. The protective slag must be dry and black-faced, and the principle of less, more frequent and more uniform must be implemented.
[0049] S43. The continuous casting tundish adopts a stopper rod to control the water flow inlet. The tundish baking time is ≥4.5-6 hours and the baking temperature is ≥1000℃. The middle of the tundish is opened first, and then the two sides, and the pulling speed is quickly increased to above 1.2m / min. After the tundish is stably poured, the pulling speed is increased to 1.30-1.35m / min. The tundish adopts an aluminum-carbon immersion nozzle combined with a sealing gasket for full-process protection casting. The nozzle baking temperature of the aluminum-carbon immersion nozzle is required to be greater than 800℃, and the insertion depth of the immersion nozzle is 95±10mm. The tundish covering agent uses a high-alkalinity covering agent, and the acid-soluble aluminum loss is ≤0.005%.
[0050] S44, the molten steel is cooled and crystallized in the crystallizer to form a preliminary solid shell; the crystallizer water volume is 170~180m 3 / h, the inlet and outlet water temperature difference is 6-8℃.
[0051] S45. The ingot pulled out of the crystallizer enters the secondary cooling zone, where automatic water distribution directly cools and accelerates the solidification of the ingot.
[0052] S46. The ingot is then straightened by the billet straightening equipment. The straightening temperature is ≥950°C and can be adaptively adjusted according to the billet quality, production rhythm and drawing speed. Example
[0053] The test steel type is square billet Q355XG, and its chemical composition is as follows: C: 0.20%, Si: 0.15%, Mn: 0.84%, P: ≤0.020%, S: ≤0.020%, Als: 0.020%.
[0054] The production method adopts the slag washing direct production process, and the steps include:
[0055] S1. When hot metal is desulfurized and enters the station, the sulfur content is required to be ≤0.05% by mass. If the sulfur content of hot metal does not meet the requirement, the slag washing process will be temporarily stopped.
[0056] The composition and temperature of molten steel used in practice are as follows: Figure 1 The table shows:
[0057] S2, converter smelting, the final molten steel temperature is controlled at 1670-1680℃, the composition is C: ≤0.05, P: 0.020, S: 0.020; 100kg of fluorine-free slag washing material, 400kg of purchased high calcium ash, 170kg of medium carbon ferromanganese, and 1.6kg of aluminum block are added after the furnace, argon is blown at the steel-making atmosphere, the top slag is melted, and the slag layer thickness is ≤30mm after the steel-making is completed; the control composition data of the converter in practice are as follows Figure 2 As shown in the table, the process control of steel tapping and argon station is as follows: Figure 3 As shown in the table.
[0058] S3, argon station slag washing;
[0059] S31, when the molten steel arrives at the station, argon gas is blown for 1-2 minutes, and the argon gas is adjusted to the soft blowing state to ensure accurate oxygen determination. The required amount of aluminum wire is determined according to the oxygen content, and oxygen control and temperature adjustment are performed. If the temperature needs to be adjusted here, the temperature is adjusted immediately. It is only adjusted once, and no subsequent temperature adjustment action is allowed. According to the melting of the top slag in S2, 30-50Kg of fluorite powder is added, and then 70-100Kg of aluminum calcium balls and 30-70Kg of aluminum chips are added in sequence to remove oxygen from the steel at one time, so that the aluminum in the steel and the aluminum in the slag reach the forward and reverse reaction equilibrium within 10 minutes, and the acid-soluble aluminum Als content in the steel is controlled to be 0.02-0.035%;
[0060] S32, strong blow argon for 2-3 minutes to dip the top slag sample, adjust the top slag to white slag with alkalinity above 4.0 according to the color, uniform density and presence of pores of the slag sample, continue blowing argon for 1-2 minutes and dip the slag sample again for identification. After the top slag meets the requirements, it enters the calcium wire feeding stage. If the composition does not meet the requirements, fine-tune the composition during the strong blowing period and then feed the calcium wire; after the dipped slag sample meets the requirements, adjust the argon to the soft blowing state before hitting the calcium wire, feed the high calcium wire for 120-150m, and then soft blow for 12-15min after feeding and then dip the slag sample for confirmation;
[0061] In practice, the composition data of the primary sample at the argon station is as follows: Figure 4 As shown in the table;
[0062] S33. Take samples before leaving the station to ensure that Ca is not less than 0.0015%, and Ca is best at 0.0020%; after the ladle leaves the station, add ladle covering agent and cover it at the same time to prevent the molten steel from overoxidation; the average slag washing desulfurization rate is about 36.84%.
[0063] In practice, the composition data of argon station samples are as follows: Figure 5 As shown in the table; slag washing desulfurization rate data as shown in Figure 6 As shown in the table.
[0064] S4, continuous casting machine casting;
[0065] S41. Preparation before continuous casting: The continuous casting machine needs to clean the water nozzle, water strip, and iron oxide on the roller surface, replace the fulcrum roller, adjust the arc, and ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered;
[0066] S42, the continuous casting ladle adopts a long nozzle combined with a sealing pad and argon gas for full protection pouring. After the ladle is poured, it is protected by a special protective slag containing aluminum rectangular billets. The protective slag must be dry and black surface operation is carried out in accordance with the principle of less, more frequent and more uniform;
[0067] S43, the continuous casting tundish adopts a plug rod to control the water flow inlet, the tundish baking time is ≥4.5-6 hours, and the baking temperature is ≥1000℃; the middle of the tundish is opened first, and then the two sides, and the pulling speed is quickly increased to above 1.2m / min. After the tundish is stably poured, the pulling speed is increased to 1.30-1.35m / min; the tundish adopts an aluminum-carbon immersion nozzle combined with a sealing gasket for full-process protection casting. The aluminum-carbon immersion nozzle has a nozzle baking temperature greater than 800℃ and an immersion nozzle insertion depth of 95±10mm; the tundish covering agent adopts a high-alkalinity covering agent, and the acid-soluble aluminum loss is ≤0.005%;
[0068] S44, the molten steel is cooled and crystallized in the crystallizer to form a preliminary solid shell; the crystallizer water volume is 170~180m 3 / h, inlet and outlet water temperature difference 6-8℃;
[0069] S45, the ingot pulled out of the crystallizer enters the secondary cooling zone, where automatic water distribution directly cools the ingot to accelerate solidification;
[0070] S46. The ingot is then straightened by the billet straightening equipment. The straightening temperature is ≥950°C and can be adaptively adjusted according to the billet quality, production rhythm and drawing speed.
[0071] In practice, the finished product ingredient data is Figure 7 As shown in the table.
Claims
1. A method for producing small-section aluminum-containing square billet by slag washing and straight-up process, Features: include: S1. When hot metal is desulfurized before entering the station, the sulfur content by mass percentage is required to be ≤0.05%; S2, converter smelting, the final molten steel temperature is controlled at 1670-1680℃; fluorine-free slag washing material, high calcium ash, medium carbon ferromanganese, steel sand aluminum are added after the furnace, argon is blown into the steel-making atmosphere, the top slag is melted, and the slag layer thickness is ≤30mm after the steel-making is completed; S3, argon gas station slag washing; S31, when the molten steel arrives at the station, argon gas is blown for 1-2 minutes, and the argon gas is adjusted to the soft blowing state to ensure accurate oxygen determination. The required amount of aluminum wire is determined according to the oxygen content, and oxygen control and temperature adjustment are performed. According to the melting condition of the top slag in S2, fluorite powder is added, and then aluminum calcium balls and aluminum chips are added in sequence to remove oxygen from the steel at one time, and the aluminum in the steel and the aluminum in the slag reach a forward and reverse reaction equilibrium within 10 minutes, and the acid-soluble aluminum Als content in the steel is controlled to be 0.02-0.035%; S32, strong blowing of argon for 2-3 minutes to dip the top slag sample, adjust the top slag to white slag with basicity above 4.0, continue blowing argon for 1-2 minutes to dip the top slag sample again for identification, and enter the calcium line feeding link after the top slag composition meets the requirements. If the composition does not meet the requirements, fine-tune the composition during the strong blowing period before feeding the calcium line; S33. Dip the sample before leaving the station to ensure that the mass percentage of Ca is not less than 0.0015%. After the ladle leaves the station, add the ladle covering agent and cover it at the same time to prevent the molten steel from overoxidation; S4, continuous casting machine casting; S41. Preparation before continuous casting: The continuous casting machine needs to clean the water nozzle, water strip, and iron oxide on the roller surface, replace the fulcrum roller, adjust the arc, and ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered; S42, the continuous casting ladle adopts a long nozzle combined with a sealing pad and argon gas for full protection pouring. After the ladle is poured, it is protected by a special protective slag containing aluminum rectangular billets. The protective slag must be dry, black surface operation, and small amounts of multiple even pouring; S43, the continuous casting tundish adopts a plug rod to control the water flow inlet tundish, the tundish baking time is ≥4.5-6 hours, and the baking temperature is ≥1000℃; the middle of the tundish is opened first, and then the two sides, and the pulling speed is quickly increased to more than 1.2m / min. After the tundish is stably poured, the pulling speed is increased to 1.30-1.35m / min; S44, the molten steel is cooled and crystallized in the crystallizer to form a preliminary solid shell; S45, the ingot pulled out of the crystallizer enters the secondary cooling zone, where automatic water distribution directly cools the ingot to accelerate solidification; S46, the ingot is then straightened by a billet straightening device.
2. The method for producing small-section aluminum-containing square billet by slag washing and straight-up process according to claim 1, Features: The amount of fluorine-free slag washing material added in S2 is 1kg / t steel, the amount of high calcium ash is 4kg / t steel, the amount of medium carbon ferromanganese is 1.7kg / t steel, and the amount of aluminum block is 1.6kg / t steel.
3. The method for producing small-section aluminum-containing square billet by slag washing and straight-up process according to claim 1, Features: The amount of fluorite powder added to the S31 is 0.3-0.5kg / t steel, the amount of aluminum calcium balls is 0.7-1kg / t steel, and the amount of aluminum chips is 0.3-0.7kg / t steel.
4. The method for producing a small-section aluminum-containing square billet by slag washing and straight-up process according to claim 1, Features: Before feeding the calcium wire as described in S32, adjust the argon gas to the soft blowing state, feed the high calcium wire for 120-150m, and after feeding, soft blow for 12-15min and then dip the slag sample for confirmation.
5. The method for producing small-section aluminum-containing square billet by slag washing and straight-up process according to claim 1, Features: The optimal mass percentage of Ca in S33 is 0.0020%.
6. The method for producing small-section aluminum-containing square billet by slag washing and straight-up process according to claim 1, Features: The middle package described in S43 adopts an aluminum-carbon immersion nozzle combined with a sealing gasket for full-process protection pouring. The nozzle baking temperature of the aluminum-carbon immersion nozzle is required to be greater than 800°C, and the insertion depth of the immersion nozzle is 95±10mm; the middle package covering agent adopts a high-alkalinity covering agent, and the mass percentage of acid-soluble aluminum Als loss is ≤0.005%.
7. The method for producing small-section aluminum-containing square billet by slag washing and straight-up process according to claim 1, Features: S44: Crystallizer water volume 170~180m 3 / h, the inlet and outlet water temperature difference is 6-8℃.