A magnesium alloy high-efficiency corrosion inhibitor and a preparation method thereof

By forming a dense film layer on the surface of magnesium alloys, the corrosion inhibitor utilizes the synergistic effect of MXene nanocapsules and modified polydopamine to solve the problems of easy oxidation and poor corrosion resistance of magnesium alloys, achieving a highly efficient corrosion inhibition effect, and is suitable for a variety of magnesium alloy materials.

CN118600430BActive Publication Date: 2026-11-10HEFEI HUAQING FANGXING SURFACING TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410893152.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2026-11-10
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Magnesium alloys are easily oxidized in air and have poor corrosion resistance. Existing corrosion inhibitors are prone to failure due to direct contact with corrosive media, making them difficult to widely apply in high-precision fields.

Method used

A high-efficiency corrosion inhibitor for magnesium alloys is composed of silane coupling agent, benzotriazole, 8-hydroxyquinoline, ionic liquid, nanoparticles, MXene, and modified polydopamine. It forms a dense film on the surface of magnesium alloy, uses MXene as a nano-container to load the corrosion inhibitor, and modifies the surface of MXene with modified polydopamine to enhance the corrosion inhibition effect.

Benefits of technology

It significantly improves the corrosion resistance of magnesium alloys under different corrosive environments, has good film density, high corrosion inhibitor stability, is suitable for a variety of magnesium alloy grades, and can withstand neutral salt spray test for up to 72 hours and immersion test for more than 96 hours.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004928193710000061
    Figure BDA0004928193710000061
  • Figure BDA0004928193710000071
    Figure BDA0004928193710000071
Patent Text Reader

Abstract

The application discloses a kind of magnesium alloy high-efficiency corrosion inhibitor and preparation method thereof, belong to metal material surface modification technical field, the high-efficiency corrosion inhibitor includes following weight parts raw materials: silane coupling agent 30-40 parts, benzotriazole 20-25 parts, 8-hydroxyquinoline 8-12 parts, ionic liquid 5-10 parts, nanoparticle 3-6 parts, MXene 25-35 parts, modified polydopamine 8-12 parts, dispersing agent 2-4 parts, anhydrous ethanol 1000 parts.The magnesium alloy high-efficiency corrosion inhibitor is prepared by using MXene nano container to load corrosion component and modified polydopamine modification approach, the corrosion inhibition effect is improved by double ways of blocking and corrosion prevention, can be suitable for different brands of magnesium alloy, neutral salt spray test can reach 72h, and immersion test can reach more than 96h.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of surface modification technology of metallic materials, specifically relating to a high-efficiency corrosion inhibitor for magnesium alloys and its preparation method. Background Technology

[0002] Magnesium alloys possess advantages such as low density, excellent damping properties, high elastic modulus, good casting properties, and excellent thermal conductivity and heat dissipation. Furthermore, my country is a major magnesium resource country with abundant reserves. Therefore, magnesium alloy products are widely used in aerospace, transportation, medical biology, battery energy, and other fields. Compared with other metals, magnesium alloys are more prone to corrosion due to magnesium's high chemical reactivity and low standard electrode potential (-2.37V vs SHE), limiting their application in high-precision fields. Improving the corrosion resistance of magnesium alloys mainly focuses on two directions: one is to improve the intrinsic corrosion resistance of magnesium alloys, i.e., by optimizing the alloy composition and improving the microstructure of magnesium alloys to enhance corrosion resistance, but this method is difficult and requires high expertise; the other is to treat magnesium alloys to form surface corrosion-resistant films and coatings, among which the development of highly efficient corrosion inhibitors is currently one of the research priorities.

[0003] Currently, commonly used corrosion inhibitors for magnesium alloys include inorganic, organic, natural, and polymeric corrosion inhibitors. Directly treating magnesium alloys with a mixture of the corrosion inhibitor and other auxiliary components is a common and cost-effective method. However, this method can lead to the corrosion-inhibiting components easily coming into direct contact with the corrosive medium and becoming ineffective. Materials such as graphene, MOF, and MXene, due to their large specific surface area, high mechanical strength, and abundant surface functional groups, can serve as nanocontainers for loading corrosion-inhibiting components. This reduces the direct contact between the corrosion-inhibiting components and the corrosive medium while extending their release time. Therefore, developing a highly efficient corrosion inhibitor for magnesium alloys based on MXene nanocontainers is of great significance in order to maximize the corrosion inhibition effect of the components. Summary of the Invention

[0004] To address the current problems of magnesium alloys being easily oxidized in air and having poor corrosion resistance, this invention provides a highly efficient corrosion inhibitor for magnesium alloys and its preparation method.

[0005] The objective of this invention can be achieved through the following technical solutions:

[0006] A high-efficiency corrosion inhibitor for magnesium alloys comprises the following raw materials in parts by weight: 30-40 parts of silane coupling agent, 20-25 parts of benzotriazole, 8-12 parts of 8-hydroxyquinoline, 5-10 parts of ionic liquid, 3-6 parts of nanoparticles, 25-35 parts of MXene, 8-12 parts of modified polydopamine, 2-4 parts of dispersant, and 1000 parts of anhydrous ethanol.

[0007] Furthermore, the silane coupling agent is any one or any two of methyltriethoxysilane, vinyltriethoxysilane, and octyltriethoxysilane mixed in any mass ratio.

[0008] Further, the ionic liquid is any one of 1-vinyl-3-butylimidazolium chloride, 1-vinyl-3-butylimidazolium bromide, and 1-vinyl-3-butylimidazolium iodide.

[0009] Furthermore, the nanoparticles are any one of hydrophilic silica nanoparticles with a particle size of 10-20 nm and hydrophilic titanium dioxide nanoparticles with a particle size of 5-10 nm, or a mixture of the two in any mass ratio.

[0010] Furthermore, the MXene is a multilayer nanosheet MXene with a thickness of 100-200 nm.

[0011] Further, the preparation method of the modified polydopamine includes the following steps: Tris(hydroxymethyl)aminomethane is stirred at 800-1000 r / min until completely dissolved in deionized water, then dopamine hydrochloride is added, and stirring is continued for 30-40 min, followed by sonication for 25-30 min. The mixture is then placed in a water bath at 55-65℃ and stirred at 500-800 r / min for 3-5 h. Cerium nitrate hexahydrate is then added and stirred for 0.5-1 h. Next, 1 mol / L sodium hydroxide solution is slowly added and stirring is continued for 2-3 h. The residue is filtered, washed, and dried in an oven at 50-60℃ for 6-8 h to obtain the modified polydopamine.

[0012] Furthermore, in the preparation method of the modified polydopamine, the solid-liquid ratio of deionized water, tris(hydroxymethyl)aminomethane, dopamine hydrochloride, cerium nitrate hexahydrate and 1 mol / L sodium hydroxide solution is 1 L: 18-22 g: 10-12 g: 5-8 g: 10-15 mL.

[0013] Furthermore, the dispersant is any one or any two of sodium dodecyl sulfonate, sodium butylnaphthalene sulfonate, and sodium dodecyl sulfate mixed in any mass ratio.

[0014] Furthermore, the preparation method of the high-efficiency corrosion inhibitor for magnesium alloys includes the following steps:

[0015] S1. Weigh each raw material according to its weight parts;

[0016] S2. Add silane coupling agent to anhydrous ethanol and stir at 400-600 r / min for 2-2.5 h. Then add benzotriazole, 8-hydroxyquinoline, ionic liquid, nanoparticles and MXene in sequence, sonicate for 30-40 min, and stir at 600-800 r / min for 4-6 h to form a mixture.

[0017] S3. Add modified polydopamine and dispersant to the above mixture, sonicate for 0.5-1 h, and continue stirring at 600-800 r / min for 3-4 h to obtain a high-efficiency corrosion inhibitor for magnesium alloys.

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0019] 1. This invention provides a high-efficiency corrosion inhibitor for magnesium alloys, which is composed of silane coupling agent, benzotriazole, 8-hydroxyquinoline, ionic liquid, nanoparticles, MXene, modified polydopamine, dispersant and anhydrous ethanol. The corrosion inhibitor can form a film on the surface of magnesium alloys.

[0020] 2. This invention improves corrosion inhibition performance through the synergistic effect of silane coupling agent, benzotriazole, 8-hydroxyquinoline, and ionic liquid. The addition of nanoparticles can effectively enhance the density of the film layer when the corrosion inhibitor forms a film on the magnesium alloy surface. Using MXene as a nano-container to load the above components can effectively block corrosive media and enhance the stability of the corrosion inhibitor components.

[0021] 3. This invention further modifies MXene nanocontainers with modified polydopamine. The non-covalent π-π interaction of polydopamine can effectively encapsulate the MXene surface, exerting its effect before the internally loaded corrosion inhibitors, thereby improving the corrosion inhibition effect through both blocking and corrosion prevention pathways. Detailed Implementation

[0022] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0023] Example 1

[0024] The preparation method of modified polydopamine includes the following steps:

[0025] 20g of tris(hydroxymethyl)aminomethane was stirred at 1000r / min until completely dissolved in 1L of deionized water. Then, 10g of dopamine hydrochloride was added, and the mixture was stirred for 35min and sonicated for 25min. The mixture was then placed in a 60℃ water bath and stirred at 600r / min for 4h. Subsequently, 6g of cerium nitrate hexahydrate was added and stirred for 1h. Then, 12mL of 1mol / L sodium hydroxide solution was slowly added and the mixture was stirred for 2.5h. The residue was filtered, washed, and dried in a 50℃ oven for 8h to obtain modified polydopamine.

[0026] Comparative Example 1

[0027] The preparation method of polydopamine is the control group of Example 1, except that cerium nitrate hexahydrate and sodium hydroxide solution are not added for modification, and includes the following steps:

[0028] 20g of tris(hydroxymethyl)aminomethane was stirred at 1000r / min until completely dissolved in 1L of deionized water. Then, 10g of dopamine hydrochloride was added, and the mixture was stirred for 35min and sonicated for 25min. The mixture was then placed in a 60℃ water bath and stirred at 600r / min for 4h. The residue was filtered, washed, and dried in a 50℃ oven for 8h to obtain polydopamine.

[0029] Example 2

[0030] The high-efficiency corrosion inhibitor for magnesium alloys in this embodiment comprises the following raw materials in parts by weight: 35 parts silane coupling agent, 22 parts benzotriazole, 10 parts 8-hydroxyquinoline, 8 parts ionic liquid, 5 parts nanoparticles, 30 parts MXene, 10 parts modified polydopamine, 3 parts dispersant, and 1000 parts anhydrous ethanol. Specifically: the silane coupling agent is a mixture of methyltriethoxysilane and vinyltriethoxysilane in a 1:1 mass ratio; the ionic liquid is 1-vinyl-3-butylimidazolium chloride; the nanoparticles are a mixture of hydrophilic silica nanoparticles with a particle size of 10-20 nm and hydrophilic titanium dioxide nanoparticles with a particle size of 5-10 nm in a 1:1 mass ratio; the modified polydopamine was prepared in Example 1; and the dispersant is a mixture of sodium dodecyl sulfonate and sodium butylnaphthalene sulfonate in a 1:1 mass ratio.

[0031] The high-efficiency corrosion inhibitor for magnesium alloys in this embodiment is prepared according to the following steps:

[0032] S1. Weigh each raw material according to its weight parts;

[0033] S2. Add silane coupling agent to anhydrous ethanol and stir at 500 r / min for 2.5 h. Then add benzotriazole, 8-hydroxyquinoline, ionic liquid, nanoparticles and MXene in sequence, sonicate for 35 min, and then stir at 700 r / min for 5 h to form a mixture.

[0034] S3. Add modified polydopamine and dispersant to the above mixture, sonicate for 0.5 h, and continue stirring at 700 r / min for 3.5 h to obtain a high-efficiency corrosion inhibitor for magnesium alloys.

[0035] Example 3

[0036] The high-efficiency corrosion inhibitor for magnesium alloys in this embodiment comprises the following raw materials in parts by weight: 30 parts silane coupling agent, 20 parts benzotriazole, 8 parts 8-hydroxyquinoline, 5 parts ionic liquid, 3 parts nanoparticles, 25 parts MXene, 8 parts modified polydopamine, 2 parts dispersant, and 1000 parts anhydrous ethanol. Specifically: the silane coupling agent is a mixture of methyltriethoxysilane and octyltriethoxysilane in a 1:1 mass ratio; the ionic liquid is 1-vinyl-3-butylimidazolium bromide; the nanoparticles are a mixture of hydrophilic silica nanoparticles with a particle size of 10-20 nm and hydrophilic titanium dioxide nanoparticles with a particle size of 5-10 nm in a 7:3 mass ratio; the modified polydopamine was prepared in Example 1; and the dispersant is a mixture of sodium dodecyl sulfonate and sodium dodecyl sulfate in a 7:3 mass ratio.

[0037] The high-efficiency corrosion inhibitor for magnesium alloys in this embodiment is prepared according to the following steps:

[0038] S1. Weigh each raw material according to its weight parts;

[0039] S2. Add silane coupling agent to anhydrous ethanol and stir at 400 r / min for 2 h. Then add benzotriazole, 8-hydroxyquinoline, ionic liquid, nanoparticles and MXene in sequence, sonicate for 30 min, and then stir at 600 r / min for 4 h to form a mixture.

[0040] S3. Add modified polydopamine and dispersant to the above mixture, sonicate for 0.5 h, and continue stirring at 600 r / min for 3 h to obtain a high-efficiency corrosion inhibitor for magnesium alloys.

[0041] Example 4

[0042] This embodiment of a high-efficiency corrosion inhibitor for magnesium alloys comprises the following raw materials in parts by weight: 40 parts of silane coupling agent, 25 parts of benzotriazole, 12 parts of 8-hydroxyquinoline, 10 parts of ionic liquid, 6 parts of nanoparticles, 35 parts of MXene, 12 parts of modified polydopamine, 4 parts of dispersant, and 1000 parts of anhydrous ethanol. Specifically: the silane coupling agent is a mixture of vinyltriethoxysilane and octyltriethoxysilane in a 1:1 mass ratio; the ionic liquid is 1-vinyl-3-butylimidazolium iodide; the nanoparticles are hydrophilic silica nanoparticles with a particle size of 10-20 nm; the modified polydopamine is prepared in Example 1; and the dispersant is a mixture of sodium butylnaphthalenesulfonate and sodium dodecyl sulfate in a 1:1 mass ratio.

[0043] The high-efficiency corrosion inhibitor for magnesium alloys in this embodiment is prepared according to the following steps:

[0044] S1. Weigh each raw material according to its weight parts;

[0045] S2. Add silane coupling agent to anhydrous ethanol and stir at 600 r / min for 2.5 h. Then add benzotriazole, 8-hydroxyquinoline, ionic liquid, nanoparticles and MXene in sequence, sonicate for 40 min, and then stir at 800 r / min for 6 h to form a mixture.

[0046] S3. Add modified polydopamine and dispersant to the above mixture, sonicate for 1 hour, and continue stirring at 800 r / min for 4 hours to obtain a high-efficiency corrosion inhibitor for magnesium alloys.

[0047] Example 5

[0048] The high-efficiency corrosion inhibitor for magnesium alloys in this embodiment comprises the following raw materials in parts by weight: 32 parts silane coupling agent, 23 parts benzotriazole, 9 parts 8-hydroxyquinoline, 7 parts ionic liquid, 5 parts nanoparticles, 28 parts MXene, 9 parts modified polydopamine, 3 parts dispersant, and 1000 parts anhydrous ethanol. Specifically: the silane coupling agent is methyltriethoxysilane; the ionic liquid is 1-vinyl-3-butylimidazolium chloride; the nanoparticles are hydrophilic titanium dioxide nanoparticles with a particle size of 5-10 nm; the modified polydopamine is prepared in Example 1; and the dispersant is sodium dodecyl sulfonate.

[0049] The high-efficiency corrosion inhibitor for magnesium alloys in this embodiment is prepared according to the following steps:

[0050] S1. Weigh each raw material according to its weight parts;

[0051] S2. Add silane coupling agent to anhydrous ethanol and stir at 550 r / min for 2.5 h. Then add benzotriazole, 8-hydroxyquinoline, ionic liquid, nanoparticles and MXene in sequence, sonicate for 35 min, and then stir at 650 r / min for 5 h to form a mixture.

[0052] S3. Add modified polydopamine and dispersant to the above mixture, sonicate for 0.5 h, and continue stirring at 650 r / min for 3.5 h to obtain a high-efficiency corrosion inhibitor for magnesium alloys.

[0053] Comparative Example 2

[0054] A high-efficiency corrosion inhibitor for magnesium alloys and its preparation method are disclosed. This is a control group of Example 2, except that the silane coupling agent in the raw materials and step S2 is replaced with polyvinylpyrrolidone, while the other components and preparation steps remain unchanged.

[0055] Comparative Example 3

[0056] A high-efficiency corrosion inhibitor for magnesium alloys and its preparation method are disclosed. This is a control group of Example 2, except that benzotriazole is removed from the raw materials and step S2, while the remaining components and preparation steps remain unchanged.

[0057] Comparative Example 4

[0058] A high-efficiency corrosion inhibitor for magnesium alloys and its preparation method are disclosed. This is a control group of Example 2, except that 8-hydroxyquinoline is removed from the raw materials and step S2, while the remaining components and preparation steps remain unchanged.

[0059] Comparative Example 5

[0060] A high-efficiency corrosion inhibitor for magnesium alloys and its preparation method are disclosed. This is a control group of Example 2, except that no ionic liquid is added in the raw materials and step S2, while the other components and preparation steps remain unchanged.

[0061] Comparative Example 6

[0062] A high-efficiency corrosion inhibitor for magnesium alloys and its preparation method are disclosed. This is a control group of Example 2, except that no nanoparticles are added in the raw materials and step S2, while the other components and preparation steps remain unchanged.

[0063] Comparative Example 7

[0064] A high-efficiency corrosion inhibitor for magnesium alloys and its preparation method are presented as a control group for Example 2. The difference lies in the removal of MXene from the raw materials and step S2, i.e., the absence of nano-container-loaded corrosion inhibitor components. The remaining components and preparation steps remain unchanged.

[0065] Comparative Example 8

[0066] A high-efficiency corrosion inhibitor for magnesium alloys and its preparation method are disclosed. This is a control group of Example 2, except that the modified polydopamine in the raw materials and step S3 is replaced with the polydopamine prepared by Comparative Example 1, while the other components and preparation steps remain unchanged.

[0067] Comparative Example 9

[0068] A magnesium alloy corrosion inhibitor and its preparation method are disclosed. The control group of Example 2 is described, except that the step of adding modified polydopamine in S3 is removed, while other raw materials and preparation methods remain unchanged, thus obtaining the magnesium alloy corrosion inhibitor.

[0069] The corrosion inhibitors for magnesium alloys prepared in Examples 2-5 and Comparative Examples 2-9 were tested for their corrosion inhibition effects on four different grades of magnesium alloys (AZ91D, AZ31B, AM60B, and ZK61M) under different corrosive environments. The specific test methods are as follows:

[0070] 1. Neutral Salt Spray Test: S1. Magnesium Alloy Surface Pretreatment: Grind the magnesium alloy to a bright finish and clean it with acetone until the surface is clean; S2. Heat the magnesium alloy corrosion inhibitor in a water bath to 40℃, immerse the pretreated magnesium alloy sample in the magnesium alloy corrosion inhibitor, stir at a constant temperature of 100r / min for 40min, remove it and dry it in a 50℃ drying oven for 2h, and after drying, place it in a 60℃ muffle furnace for curing at 1℃ / min for 20min to obtain the magnesium alloy sample with corrosion inhibitor surface treatment; S3. Conduct neutral salt spray tests (GB / T 10125-2021) on magnesium alloy samples of different grades. After 72h of testing, the film layer surface without rust is considered qualified, otherwise it is unqualified;

[0071] 2. Immersion Test: S1. Prepare a 3.5% NaCl solution at room temperature, then add a 1% magnesium alloy corrosion inhibitor to the NaCl solution and stir at 500 r / min for 30 min to form a mixed solution; S2. Magnesium alloy surface pretreatment: polish the magnesium alloy to a bright finish and clean it with acetone until the surface is clean; S3. Immerse the pretreated magnesium alloy sample completely in the mixed solution, and take it out every 12 hours to observe whether there is corrosion on the surface and record the time when corrosion appears.

[0072] The performance test results are shown in Table 1:

[0073] Table 1

[0074]

[0075]

[0076] As shown in Table 1:

[0077] Examples 2, 3, 4, and 5 test the corrosion inhibition performance of the high-efficiency corrosion inhibitors for magnesium alloys prepared under different parameter settings on different grades of magnesium alloys. The results show that the high-efficiency corrosion inhibitors prepared by this invention are applicable to different grades of magnesium alloys. The neutral salt spray test can reach 72 hours, and the immersion test can reach more than 96 hours.

[0078] Comparison of Comparative Example 2 and Example 2 shows that the silane coupling agent in the high-efficiency corrosion inhibitor can improve the corrosion inhibition effect of the inhibitor, because the silane coupling agent has a good film-forming effect on the magnesium alloy surface. Comparison of Comparative Examples 3, 4, and 5 with Example 2 shows that benzotriazole, 8-hydroxyquinoline, and ionic liquid in the high-efficiency corrosion inhibitor are the main corrosion inhibitor components, and their synergistic effect can maximize the corrosion inhibition effect of the inhibitor. Comparison of Comparative Example 6 with Example 2 shows that the addition of nanoparticles in the high-efficiency corrosion inhibitor can effectively enhance the density of the film layer when the inhibitor forms a film on the magnesium alloy surface, thereby improving its corrosion resistance.

[0079] As can be seen from the comparison between Comparative Example 7 and Example 2, using MXene as a nano-container for loading corrosion inhibitor components during the preparation of corrosion inhibitors can improve the corrosion inhibition ability of corrosion inhibitors. This is because MXene can effectively block corrosive media and enhance the stability of corrosion inhibitor components.

[0080] Comparing Comparative Example 8 and Example 2, it can be seen that when MXene is modified with polydopamine instead of modified polydopamine, the corrosion inhibition performance of the corrosion inhibitor decreases. This is because the corrosion protection performance of polydopamine is lower than that of modified polydopamine. Comparing Comparative Example 9 and Example 2, it can be seen that modified polydopamine can significantly improve the corrosion inhibition effect of the corrosion inhibitor on magnesium alloys in corrosive environments. This is not only due to the modification of polydopamine, but also because the non-covalent π-π interaction of polydopamine can effectively coat the surface of MXene, exerting its effect before the internally loaded corrosion inhibitor. This improves the corrosion inhibition effect through both blocking and corrosion prevention, thereby giving the treated magnesium alloy better corrosion resistance.

[0081] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0082] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A high-efficiency corrosion inhibitor for magnesium alloys, characterized in that, Including the following parts by weight of raw materials: 30-40 parts of silane coupling agent, 20-25 parts of benzotriazole, 8-12 parts of 8-hydroxyquinoline, 5-10 parts of ionic liquid, 3-6 parts of nanoparticles, 25-35 parts of MXene, 8-12 parts of modified polydopamine, 2-4 parts of dispersant, and 1000 parts of anhydrous ethanol. The nanoparticles are any one of hydrophilic silica nanoparticles with a particle size of 10-20 nm and hydrophilic titanium dioxide nanoparticles with a particle size of 5-10 nm, or a mixture of the two in any mass ratio. The method for preparing the modified polydopamine includes the following steps: Tris(hydroxymethyl)aminomethane is stirred at 800-1000 r / min until completely dissolved in deionized water, then dopamine hydrochloride is added, and stirring is continued for 30-40 min, followed by sonication for 25-30 min. The mixture is then placed in a water bath at 55-65℃ and stirred at 500-800 r / min for 3-5 h. Cerium nitrate hexahydrate is then added and stirred for 0.5-1 h. Next, 1 mol / L sodium hydroxide solution is slowly added and stirring is continued for 2-3 h. The residue is filtered, washed, and dried in an oven at 50-60℃ for 6-8 h to obtain the modified polydopamine.

2. The high-efficiency corrosion inhibitor for magnesium alloys according to claim 1, characterized in that, The silane coupling agent is any one or any two of methyltriethoxysilane, vinyltriethoxysilane, and octyltriethoxysilane mixed in any mass ratio.

3. The high-efficiency corrosion inhibitor for magnesium alloys according to claim 1, characterized in that, The ionic liquid is any one of 1-vinyl-3-butylimidazolium chloride, 1-vinyl-3-butylimidazolium bromide, and 1-vinyl-3-butylimidazolium iodide.

4. The high-efficiency corrosion inhibitor for magnesium alloys according to claim 1, characterized in that, The MXene is a multilayer nanosheet MXene with a thickness of 100-200 nm.

5. The high-efficiency corrosion inhibitor for magnesium alloys according to claim 1, characterized in that, In the preparation method of the modified polydopamine, the solid-liquid ratio of deionized water, tris(hydroxymethyl)aminomethane, dopamine hydrochloride, cerium nitrate hexahydrate and 1 mol / L sodium hydroxide solution is 1 L: 18-22 g: 10-12 g: 5-8 g: 10-15 mL.

6. The high-efficiency corrosion inhibitor for magnesium alloys according to claim 1, characterized in that, The dispersant is any one or any two of sodium dodecyl sulfonate, sodium butylnaphthalene sulfonate, and sodium dodecyl sulfate, mixed in any mass ratio.

7. A method for preparing the high-efficiency corrosion inhibitor for magnesium alloys according to any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Weigh each raw material according to its weight parts; S2. Add silane coupling agent to anhydrous ethanol and stir at 400-600 r / min for 2-2.5 h. Then add benzotriazole, 8-hydroxyquinoline, ionic liquid, nanoparticles and MXene in sequence, sonicate for 30-40 min, and stir at 600-800 r / min for 4-6 h to form a mixture. S3. Add modified polydopamine and dispersant to the mixture, sonicate for 0.5-1 h, and continue stirring at 600-800 r / min for 3-4 h to obtain a high-efficiency corrosion inhibitor for magnesium alloys.

Citation Information

Patent Citations

  • Quaternary ammonium salt ionic liquid, synthesis method and application of quaternary ammonium salt ionic liquid as metal corrosion inhibitor

    CN111825559A

  • Anticorrosive coating material composition for magnesium alloy and article having coating film made from the same

    JP2006137861A