A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings

By using the heating device and temperature control unit in the induction melting furnace to achieve in-situ heating of the mold, the problems of poor melt fluidity and insufficient vacuum in refractory high-entropy alloy casting are solved, the molding quality and fluidity of the castings are improved, and the mold quality is reduced. casting defects.

CN118616692BActive Publication Date: 2024-10-22BEIJING INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411105157.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-22
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The high melting point and activity of refractory high-entropy alloys lead to poor melt fluidity. During the casting process, there are problems such as insufficient solidification feeding ability, many casting defects, and low yield. The existing high-temperature mold preheating method has complicated operations and poor vacuum. Insatiable shortcomings.

Method used

A heating device is installed in the middle of the induction melting furnace, and the mold is heated in situ through graded vacuuming and temperature control units to ensure a high vacuum and high temperature environment, reduce heat loss, and improve the fluidity and filling capacity of the alloy melt.

Benefits of technology

It effectively improves the molding quality of alloy castings, reduces casting defects, ensures stable conditions of high temperature and high vacuum, and enhances the fluidity and filling ability of the alloy melt in the mold.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118616692B_ABST
    Figure CN118616692B_ABST
Patent Text Reader

Abstract

The present invention relates to a mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings, and belongs to the field of alloy technology. By placing a heating device in an induction melting furnace, placing a mold in the heating device, and heating the heating device through a temperature control unit, the in-situ heating and heat preservation of the mold are realized, the temperature difference between the alloy melt and the casting mold is reduced, the solidification rate of the alloy melt in the mold is slowed down, the fluidity of the alloy melt in the mold is improved, and the filling capacity of the alloy melt in the mold is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings, and belongs to the technical field of alloys. Background Art

[0002] Refractory high entropy alloys are a type of high entropy alloys formed by alloying a variety of highly active elements such as Ti, Zr, Nb, Ta, Hf, Al, etc. or these elements with other elements with higher melting points (W, Mo, Ta, etc.). The high melting point and high activity of this type of alloy make the alloy only suitable for cold crucible smelting, and this technology has almost no superheat during smelting. The melting point of refractory high entropy alloys is very high, resulting in very poor fluidity of the melt. Therefore, there are many problems in alloy casting, such as insufficient solidification shrinkage compensation ability, many casting defects, and very low yield, making it difficult to form high-quality alloy castings.

[0003] Using high-temperature preheating of the mold is an effective means to improve the filling capacity of the alloy melt. Usually, the mold is preheated first, and then placed in the melting furnace. After the vacuum reaches the target value, it is melted and cast. This method requires moving the mold back and forth, and the operation process is complicated. At the same time, after the mold is heated and placed in the melting furnace until casting, the mold temperature will drop rapidly, which will cause the fluidity of the alloy melt to decrease significantly. When the mold is placed in a vacuum furnace for heating, a large amount of heat radiation will be generated when the mold is heated. In addition, the mold material (usually graphite, oxide ceramics, etc.) is easy to degas at high temperatures, resulting in a decrease in the vacuum degree of the equipment, which makes it difficult to meet the melting requirements of refractory high-entropy alloys. Summary of the invention

[0004] In view of this, an object of the present invention is to provide a mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows.

[0006] A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings, the method steps comprising:

[0007] (1) Place the heating device in an induction melting furnace and place the mold in the heating device;

[0008] (2) Evacuate the induction melting furnace to a vacuum degree of ≤1×10 4 After Pa, the control unit controls the heating device to heat the mold;

[0009] (3) After the temperature reaches the set mold preheating temperature and remains stable; evacuate to a vacuum degree of ≤2×10 -2Pa, the heating device continuously heats the mold, and under a protective gas atmosphere, the refractory high-activity multi-component high-entropy alloy raw material is placed in the crucible of an induction melting furnace for smelting, and the smelted alloy melt is poured into the mold in the heating device. After 10 to 30 minutes, the heating of the mold is stopped, and the alloy casting is obtained after the alloy melt solidifies.

[0010] Furthermore, in step (1), the heating device is placed in front of the crucible in the induction melting furnace and fixed.

[0011] Furthermore, the heating device includes a cylindrical ceramic fiber, a resistance wire and a thermocouple; the resistance wire is wound inside the cylindrical ceramic fiber wall, the mold is placed inside the cylindrical ceramic fiber, and the thermocouple is inserted into the mold; the temperature control unit includes a solid-state relay and a temperature controller, the resistance wire is connected to the solid-state relay, and the solid-state relay and the thermocouple are respectively connected to the temperature controller.

[0012] Furthermore, the ceramic fiber is aluminum silicate ceramic fiber.

[0013] Furthermore, the inner diameter of the cylindrical ceramic fiber is 80-400 mm, the wall thickness is 60-100 mm, and the height is 200-400 mm. The outer diameter of the mold used is 60-360 mm, and the height is 200-400 mm.

[0014] Furthermore, the resistance wire is made of nickel-chromium-aluminum alloy.

[0015] Furthermore, in step (2), a mechanical pump is used to create a vacuum.

[0016] Furthermore, in step (3), a mechanical pump is first used to evacuate the air to a vacuum degree of ≤2×10 2 Pa, and then use Roots pump to evacuate to a vacuum degree of ≤2×10 -1 Pa, and finally use a molecular pump to evacuate to a vacuum degree of ≤2×10 -2 Pa.

[0017] Furthermore, the time for evacuating the air using the molecular pump is 1.5 to 2 hours.

[0018] Furthermore, in step (3), the protective gas is an inert gas.

[0019] Beneficial Effects

[0020] The present invention provides a method for in-situ heating of a mold for improving the molding quality of a refractory high-activity multi-component high-entropy alloy casting. The method comprises placing a heating device in an induction melting furnace, placing a mold in the heating device, and heating the heating device through a temperature control unit to achieve in-situ heating and heat preservation of the mold, thereby reducing the temperature difference between the alloy melt and the casting mold, slowing down the solidification rate of the alloy melt in the mold, improving the fluidity of the alloy melt in the mold, and enhancing the filling capacity of the alloy melt in the mold.

[0021] The present invention provides a mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings. During the mold in-situ heating process, the efficiency of the mold in-situ heating can be improved by vacuuming the mold in stages, so that the heat is more concentrated in the mold, and a large amount of heat in the heating device is effectively prevented from being lost to the smelting furnace. The problem that the vacuum degree in the smelting furnace cannot meet the requirements of smelting due to the increase in gas pressure in the smelting furnace caused by the large amount of heat generated by the heating device and the degassing of the mold at high temperature is solved. The vacuum degree is stably maintained at 10 -2 Below Pa, high-temperature and high-vacuum in-situ heating of the casting mold is achieved, creating ideal conditions for melting and casting. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1-2 It is a schematic structural diagram of the heating device of the present invention.

[0023] Figure 3 It is a schematic diagram of the connection structure of the heating device, mold and control unit of the present invention.

[0024] Figure 4-5 This is a physical picture of the alloy casting obtained by in-situ heating of the mold in Example 1. DETAILED DESCRIPTION

[0025] The present invention will be further described in detail below in conjunction with specific embodiments.

[0026] A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings, the method steps comprising:

[0027] (1) Place the heating device in an induction melting furnace and place the mold in the heating device;

[0028] (2) Place the refractory high-activity multi-component high-entropy alloy raw material in the crucible of the induction melting furnace, and evacuate the induction melting furnace to a vacuum degree of ≤1×10 4 After Pa, the control unit controls the heating device to heat the mold;

[0029] (3) After the temperature reaches the set mold preheating temperature and remains stable; evacuate to a vacuum degree of ≤2×10 -2Pa, the heating device continuously heats the mold, fills in protective gas, melts the raw materials in the crucible, and pours the molten alloy into the mold in the heating device. After 10 to 30 minutes, the heating of the mold is stopped, and the alloy casting is obtained after the alloy melt solidifies.

[0030] In some embodiments, in step (1), the heating device is placed in front of the crucible in the induction melting furnace and fixed.

[0031] In some embodiments, Figure 1-3 As shown, the heating device includes a cylindrical ceramic fiber, a resistance wire and a thermocouple; the resistance wire is wound in the cylindrical ceramic fiber wall, the mold is placed in the cylindrical ceramic fiber, and the thermocouple 3 is inserted into the mold; the temperature control unit includes a temperature controller 1 and a solid-state relay 2, the resistance wire is connected to the solid-state relay 2, and the solid-state relay 2 and the thermocouple 3 are respectively connected to the temperature controller 1.

[0032] In some embodiments, the ceramic fiber is aluminum silicate ceramic fiber.

[0033] In some embodiments, the inner diameter of the cylindrical ceramic fiber is 80-400 mm, the wall thickness is 60-100 mm, and the height is 200-400 mm.

[0034] In some embodiments, the resistance wire is made of nickel-chromium-aluminum alloy.

[0035] In some embodiments, in step (2), a mechanical pump is used to create a vacuum.

[0036] In some embodiments, in step (3), a mechanical pump is first used to evacuate the vacuum to a vacuum degree of ≤2×10 2 Pa, and then use Roots pump to evacuate to a vacuum degree of ≤2×10 -1 Pa, and finally use a molecular pump to evacuate to a vacuum degree of ≤2×10 -2 Pa.

[0037] In some embodiments, the vacuuming time using the molecular pump is 1.5 to 2 hours.

[0038] In some embodiments, in step (3), the protective gas is an inert gas, such as argon.

[0039] Example 1

[0040] In this embodiment, the ceramic fiber is aluminum silicate ceramic fiber, and its main components include Al2O3 and SiO2. The mass content of Al2O3 is greater than 45%, the mass content of Al2O3+SiO2 is greater than 99%, and the mass content of Fe2O3 is less than 0.2%.

[0041] The outer diameter of the cylindrical ceramic fiber is 300mm, the inner diameter is 200mm, and the height is 200mm. The resistance wire is wound at the ceramic fiber diameter of 224mm. The resistance wire is made of HRE nickel-chromium-aluminum alloy, with a wire diameter of 1.5mm, a winding center diameter of 1mm, a total length of 29.47m, a resistance value of 24.2Ω, a molding length of 1395mm, an assembly length of 2800mm, and a resistance wire distance of 12mm from the inner wall surface and 26mm from the upper and lower surfaces of the ceramic fiber.

[0042] The heating device uses 220V voltage when heating, the heating temperature range is 100~1000℃, and the total power is 0.5~4KW. The temperature controller can realize self-tuning PID control, the thermocouple is N-type thermocouple, the maximum measurable temperature is 1300℃, and the maximum operating current allowed by the solid-state relay is 15A.

[0043] The outer diameter of the graphite mold is 160 mm and the height is 120 mm.

[0044] A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings, the method steps comprising:

[0045] (1) Place the heating device in front of the crucible in the induction melting furnace and fix it, and place the graphite mold in the heating device; insert the N-type thermocouple into the graphite mold; connect the double-stranded resistance wire connecting wire and the thermocouple wire to the internal terminal of the induction melting furnace respectively; connect the external terminal corresponding to the resistance wire to the solid-state relay and to the temperature controller; connect the external terminal corresponding to the thermocouple to the temperature controller; and connect the 220V AC to the temperature controller;

[0046] (2) Place 3kg Ti, 0.45kg Zr, 0.9kg Nb, and 0.5kg Al metal raw materials into the crucible of the melting furnace, close the furnace door, turn on the power, and use the mechanical pump to evacuate the induction melting furnace to a vacuum degree of ≤1×10 4 After Pa, the mechanical pump is turned off, the temperature controller is turned on, and the heating device heats the mold;

[0047] (3) After the temperature reaches the set mold preheating temperature of 600°C and remains stable, turn on the mechanical pump to evacuate the vacuum again, and the vacuum degree should be ≤2×10 2 Pa, the Roots pump was turned on; the vacuum degree reached 2×10 -1 Pa, the molecular pump was turned on; after 1.5 hours, the vacuum degree reached 2×10 -2 Pa, fill argon into the melting chamber, turn on the power, gradually increase the power current to 450A, melt for 15 minutes, pour the molten alloy into the mold in the heating device, turn off the temperature controller after 20 minutes, stop heating the mold, and obtain the alloy casting after the alloy melt solidifies.

[0048] The actual picture of the alloy casting is as follows Figure 4-5 As shown in the figure, when the mold is heated to 600℃ in situ, a conical thin-walled part is cast. The casting is completely filled, the surface is relatively bright, there is no oxidation phenomenon, no loose shrinkage holes, and no cold shut and other defects, indicating that the alloy melt has good fluidity in the mold and high molding quality. However, when melting and casting is carried out without mold heating, the alloy melt cannot be filled in the mold, large shrinkage holes are produced on the surface of the casting, and the molding quality of the casting is poor; when melting and casting is carried out by preheating outside the furnace and then putting it into the furnace, the alloy melt has poor filling ability in the mold, and there are defects such as loose shrinkage holes on the surface of the casting, and it cannot be completely filled, indicating that the alloy melt has poor fluidity in the mold and poor molding quality.

[0049] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.

Claims

1. A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings, characterized in that: The method steps include: (1) Place the heating device in an induction melting furnace and place the mold in the heating device; (2) Place the refractory high-activity multi-component high-entropy alloy raw material in the crucible of the induction melting furnace, and evacuate the induction melting furnace to a vacuum degree of ≤1×10 4 After Pa, the temperature control unit controls the heating device to heat the mold; (3) After the temperature reaches the set mold preheating temperature and remains stable; evacuate to a vacuum degree of ≤2×10 -2 Pa, the heating device continuously heats the mold, fills in protective gas, melts the raw materials in the crucible, and pours the molten alloy into the mold in the heating device. After 10-30 minutes, the heating of the mold is stopped, and the alloy casting is obtained after the molten alloy solidifies; The heating device comprises a cylindrical ceramic fiber, a resistance wire and a thermocouple; the resistance wire is wound inside the cylindrical ceramic fiber wall, the mold is placed inside the cylindrical ceramic fiber, and the thermocouple is inserted into the mold; the temperature control unit comprises a solid-state relay and a temperature controller, the resistance wire is connected to the solid-state relay, and the solid-state relay and the thermocouple are respectively connected to the temperature controller; In step (2), a mechanical pump is used to create a vacuum; In step (3), first use a mechanical pump to evacuate the vacuum to a degree of ≤2×10 2 Pa, and then use Roots pump to evacuate to a vacuum degree of ≤2×10 -1 Pa, and finally use a molecular pump to evacuate to a vacuum degree of ≤2×10 -2 Pa.

2. A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings as claimed in claim 1, characterized in that: In step (1), the heating device is placed in front of the crucible in the induction melting furnace and fixed.

3. A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings as claimed in claim 1, characterized in that: The ceramic fiber is aluminum silicate ceramic fiber.

4. A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings as claimed in claim 1, characterized in that: The inner diameter of the cylindrical ceramic fiber is 80-400 mm, the wall thickness is 60-100 mm, and the height is 200-400 mm; the outer diameter of the mold used is 60-360 mm, and the height is 200-400 mm.

5. A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings as claimed in claim 1, characterized in that: The resistance wire is made of nickel-chromium-aluminum alloy.

6. A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings as claimed in claim 1, characterized in that: The time for vacuuming using a molecular pump is 1.5~2h.

7. A mold in-situ heating method for improving the molding quality of refractory high-activity multi-component high-entropy alloy castings as claimed in claim 1, characterized in that: In step (3), the protective gas is an inert gas.