A method for preparing coreless high-entropy metal ceramics

Through the preparation of coreless structure microstructure of high-entropy alloys and high-entropy ceramic powders, the contradiction between the hardness and toughness of metal cermets is solved, and the balance of high hardness and high toughness is achieved. The preparation process is simplified and the reduction of Cost, suitable for industrial production.

CN118621171BActive Publication Date: 2024-12-03SUZHOU LABORATORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411111192.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Existing metal cermets often sacrifice hardness when improving their strength and toughness, making it difficult to meet extreme service conditions during high-precision manufacturing and processing. Moreover, the preparation process of high-entropy metal cermets is complex and costly, which limits its application range.

Method used

High-entropy alloy and high-entropy ceramic powder were used to prepare high-entropy metal cermets with coreless structure microstructures at the same time. Through high-energy ball milling and vacuum sintering processes, the lattice distortion and sintering temperature are regulated to form low interfacial stress and high density. material.

Benefits of technology

It achieves a balance of high hardness and high strength and toughness, simplifies the preparation process, reduces costs, is suitable for industrial production, and improves the comprehensive mechanical properties of metal cermets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118621171B_ABST
    Figure CN118621171B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a coreless high-entropy metal ceramic. The method comprises the following steps: preparing a high-entropy ceramic mixture by taking Ti, W, Mo, Ta, Cr and flaky graphite powder as raw materials, preparing a high-entropy alloy mixture by taking Ni, Co, Fe, Cr and Ti as raw materials, and preparing a mixture with mass percentages of Ti: 8.47-9.29wt%, W: 24.65-27.16wt%, Mo: 12.87-14.17wt%, Cr: 9.20-10.10wt%, Ta: 24.26-26.73wt%, Ni: 1.71-3.52wt%, Co: 1.72-3.54wt%, Fe: 1.63-3.35wt% and C: 8.41-9.20wt%. The mixture has higher hardness, wear resistance and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a coreless structure high-entropy metal ceramic, belonging to the technical field of powder metallurgy. Background Art

[0002] Ti(C,N)-based cermets have excellent wear resistance, red hardness, high temperature oxidation resistance, corrosion resistance and other characteristics. Especially in tool manufacturing, this material has the adaptability of efficient dry cutting, which not only improves cutting efficiency, but also prolongs service life, and the manufacturing cost is lower than that of cemented carbide. This makes Ti(C,N)-based cermets a promising alternative to traditional WC-Co cemented carbide. In addition to the cutting field, cermet materials also show great application potential in many fields such as molds, wear-resistant parts, and seals, which makes them widely used in aerospace, petroleum, mining, and automotive industries. However, despite the many advantages of cermets, their strength and toughness are relatively insufficient, so that their potential performance has not been fully utilized. In order to improve the strength and toughness of cermets, researchers have studied various ways such as preparation process optimization, composition adjustment, and sintering method innovation, and have achieved certain results. However, like cemented carbide, cermets also face the contradiction between hardness and toughness: improving toughness often means sacrificing the hardness of the material, and vice versa. This problem makes it more difficult for Ti(C,N)-based cermets to meet the requirements in the current high-precision manufacturing process under extreme service conditions, thus limiting their scope of application.

[0003] Ti(C,N) based cermets mainly use (TiC+TiN) or Ti(C,N) as hard phase, Ni, Co or their alloys as bonding phase, and carbides such as WC, TaC, NbC as additives. The bonding phase of traditional cermets is mainly one or two of Co and Ni, and the content and chemical composition of the bonding phase have a significant influence on the mechanical properties of cermets. High entropy alloys (HEA) have higher strength and hardness, excellent corrosion and oxidation resistance, strong fatigue resistance, good tribological properties, good creep resistance, high thermal stability and extremely low temperature mechanical properties compared to traditional metal bonding phases due to the high entropy effect in thermodynamics, slow diffusion effect in kinetics, high stability in organization, and lattice distortion effect in structure. On the other hand, in the metal ceramic microstructure, due to the addition of various carbides and the dissolution-precipitation process, the hard phase mainly exists in the form of a core-ring structure. There are differences in chemical composition and physical properties between the core and ring of the metal ceramic, and there will be some complex interface stresses and lattice distortions between their interfaces. In addition, the ring phase itself is a brittle phase, and too thick annular phase thickness will also be unfavorable to the improvement of material performance. If the hard phase powder is added in the form of (Ti, W, Mo, Ta, Cr) (C, N) high entropy ceramics (HEC), it can not only have performance characteristics similar to high entropy alloys, but also effectively reduce or even eliminate the existence of the core-ring structure, so that the strength and toughness of the metal ceramics are greatly improved. In summary, the simultaneous application of high entropy alloys and high entropy ceramics in the preparation of metal ceramics will be conducive to obtaining metal ceramic materials with both high hardness and high strength and toughness.

[0004] At present, there are few studies on high entropy metal ceramics, and the few patents that have been published mainly use high entropy alloys as the bonding phase to prepare metal ceramics. Among them, the "Ultrafine high entropy alloy bonding phase metal ceramic and its preparation method" disclosed in patent CN 108823478 B and the "Preparation method of TiC-based metal ceramic with high entropy alloy bonding phase" disclosed in patent CN 112680646 B both use pure metal powder high energy ball milling to prepare high entropy alloy bonding phase, and then mix with Ti (C, N) or TiC hard phase and sinter. Although the toughness of the metal ceramic is improved, the high energy ball milling time is too long, which greatly increases the adsorbed oxygen content on the surface of the alloy powder, which is not conducive to the densification of the metal ceramic sintered body. In addition, the patent CN 109022990 B discloses a method for preparing a high entropy alloy binder phase Ti(C,N)-based cermet and the patent CN 114850475 B discloses a method for preparing a high-temperature oxidation-resistant titanium carbonitride cermet based on a high entropy alloy binder and a method for preparing the same. After high-energy ball milling of metal powder and mixing with Ti(C,N), microwave sintering or spark plasma sintering is used to prepare a cermet sintered body. Although the new sintering method is conducive to shortening the preparation time of cermet, it has high equipment requirements and is not conducive to industrial production. The patent CN 116815031 A discloses a method for preparing a fine-grained cermet with a multi-principal alloy as a binder metal and a method for preparing the same. The high / medium entropy alloy powder of FeCoCrNi / CoCrNi is prepared by melt atomization and ball milling flake treatment, and is applied to the preparation of cermet. The cermet prepared by this method has a bending strength greater than 2700MPa, but the sintering process temperature exceeds 1500℃, which is relatively high.

[0005] High entropy ceramics with high hardness and toughness can also be prepared using high entropy ceramics as hard phases. For example, the patent CN 113444952 A discloses "a high-strength and high-toughness high entropy metal ceramic and its preparation method" and the patent CN 114262833 B discloses "a high-entropy carbide reinforced TiCN-based metal ceramic with high hardness and high toughness and its preparation method and application". TiO2, WO3, MoO3, Nb2O5, Ta2O5, V2O5 and other oxides are pre-ball milled and mixed, and then high entropy ceramic powder is prepared by carbon thermal reduction (nitridation), and then mixed with metal and carbide and sintered. This method can significantly improve the hardness of metal ceramics, but the disadvantage is that in order to obtain dense and high-toughness metal ceramics, it is necessary to use spark plasma sintering or press the powder under cold isostatic pressing conditions of more than 200MPa. The preparation process is relatively complicated and not conducive to mass production. Although the patent CN 111850373 B discloses a "Ti(C,N)-based metal ceramic with a high entropy ring phase structure and a preparation method thereof", the metal ceramic can be prepared by conventional vacuum sintering. However, in order to form a dense bond between the high entropy ceramic prepared by oxide and the metal, multiple sintering processes are required, and the sintering temperature is high, resulting in relatively large energy consumption.

[0006] Most of the existing patents for preparing high-entropy metal ceramics use the method of adding high-entropy alloy or high-entropy ceramic powder separately and sintering. Few patents use both powders to prepare metal ceramics. Only the patent CN 110607473B discloses "a transition metal carbonitride-based high-entropy metal ceramic and its preparation method and application" which prepares high-entropy alloy and high-entropy ceramic powders respectively through precursor reduction method, hydrothermal synthesis method and carbon thermal reduction nitridation method after high-energy ball milling, and prepares high-entropy metal ceramics through mixed sintering. The hardness, flexural strength and fracture toughness of the metal ceramics obtained by the metal ceramic preparation method described in the patent can reach 22GPa, 3450MPa and 19.8MPa·m respectively. 1 / 2 However, the disadvantage is that the entire preparation process involves multiple heat treatments and mixing processes, and a large amount of impurities may be introduced during the reduction reaction. The performance stability of metal ceramics is poor, which is not conducive to mass production.

[0007] In summary, the simultaneous application of high-entropy alloys and high-entropy ceramic powders in the preparation of metal ceramics can greatly improve the hardness and toughness of metal ceramics. However, due to the relatively complex preparation process, how to prepare high-entropy metal ceramics with uniform and dense properties through a simple and low-cost process so that they have both high hardness and high toughness is particularly important for the application and promotion of high-entropy metal ceramics. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing a coreless high-entropy metal ceramic, and at the same time use high-entropy alloy and high-entropy ceramic powder to prepare a high-entropy metal ceramic with a hard phase coreless structure microstructure, so as to solve the problem that the fracture toughness of metal ceramics is low under high hardness conditions and the comprehensive mechanical properties are not high.

[0009] This application is implemented through the following technical solutions:

[0010] The components of the Ti(C,N)-based metal ceramic are as follows: Ti: 8.47-9.29wt%, W: 24.65-27.16wt%, Mo: 12.87-14.17wt%, Cr: 9.20-10.10wt%, Ta: 24.26-26.73wt%, Ni: 1.71-3.52wt%, Co: 1.72-3.54wt%, Fe: 1.63-3.35wt%, and C: 8.41-9.20wt%.

[0011] Furthermore, all the metal elements in the above components are introduced from simple metal powders, and C is introduced from flake graphite powder; the particle size of the flake graphite powder is 7-10 μm, and the particle sizes of the remaining powders are all 2-4 μm.

[0012] The present invention provides a method for preparing a coreless high-entropy metal ceramic, comprising the following steps:

[0013] (1) Preparation of high entropy ceramic mixture: Ti, W, Mo, Ta, Cr and flake graphite powder are used as raw materials to prepare a mixture with the following mass percentages: Ti: 6.42-7.07wt%, W: 24.65-27.16wt%, Mo: 12.87-14.17wt%, Cr: 6.97-7.68wt%, Ta: 24.26-26.73wt%, C: 8.05-8.87wt%, and the high entropy ceramic mixture is prepared by high energy ball milling;

[0014] (2) Preparation of high entropy alloy mixture: Ni, Co, Fe, Cr, and Ti are used as raw materials to prepare a mixture with the following mass percentages: Ni: 1.71-3.52wt%, Co: 1.72-3.54wt%, Fe: 1.63-3.35wt%, Cr: 1.52-3.13wt%, and Ti: 1.40-2.87wt%, and the high entropy alloy mixture is prepared by high energy ball milling;

[0015] (3) wet grinding: the high entropy ceramic mixture and the high entropy alloy mixture prepared in step (1) and step (2) are mixed and wet-ground together with an additional 0.34-0.37 wt % of graphite in a ball mill to obtain a mixed metal-ceramic slurry;

[0016] (4) vacuum drying the mixed slurry obtained in step (3), adding a forming agent, pressing and vacuum sintering to obtain the high entropy metal ceramic with a coreless structure;

[0017] Furthermore, the high-energy ball milling in the above step (1) is carried out in a planetary ball mill, the ball milling process is dry milling, the grinding balls are cemented carbide balls, the ball-to-material ratio is 10:1-20:1, the ball milling speed is 350-450 rpm, the ball milling time is 8-16 h, and the whole ball milling process is carried out under N2 atmosphere, and the N2 pressure in the ball mill tank is 0.3-0.5 atm;

[0018] Furthermore, the high-energy ball milling in the above step (2) is carried out in a planetary ball mill, the ball milling process is dry milling, the grinding balls are cemented carbide balls, the ball-to-material ratio is 8:1-15:1, the ball milling speed is 400-500 rpm, the ball milling time is 6-12 h, the ball milling is carried out in an Ar atmosphere, and the argon pressure in the ball mill tank is 0.5-0.8 atm;

[0019] Furthermore, the wet grinding of the above step (3) is carried out in a planetary ball mill, the high entropy ceramic accounts for 68% to 84% of the total mass of the raw materials, the high entropy alloy mixture accounts for 16% to 32% of the total mass of the raw materials, the grinding balls are cemented carbide balls, the ball-to-material ratio is 4:1 to 6:1, the ball milling speed is 100 to 200 rpm, the ball milling time is 18 to 24 hours, and the wet grinding medium is anhydrous ethanol, and the amount thereof added is preferably 1.5 to 1.7 times the weight of the mixture;

[0020] Furthermore, the vacuum drying in the above step (4) refers to drying in a vacuum infrared drying oven, during which the pressure of the drying oven needs to be maintained below 0.5 atm throughout the drying process, and the drying temperature is 80-100°C.

[0021] Furthermore, the adding of the molding agent in the above step (4) refers to adding one or both of paraffin wax and polyethylene glycol, and the total addition ratio is 4-6wt% of the mixture; and the compression molding refers to bidirectional compression at a pressure of 220-320MPa.

[0022] Furthermore, the vacuum sintering process in the above step (4) is mainly divided into five stages: the first stage, heating to 400-600°C, the heating rate is 0.3-0.5°C / min, and the temperature is kept for 2-4h; the second stage, heating to 800-1200°C, the heating rate is 1-2°C / min, and the temperature is kept for 1-2h; the third stage, heating to 1300-1350°C, the heating rate is 0.5-1°C / min, and the temperature is kept for 2-3h; the fourth stage, heating to 1400-1480°C, the heating rate is 1-2°C / min, and the temperature is kept for 1-1.5h; the fifth stage, cooling rapidly to room temperature at a cooling rate of 15-25°C / min; the above sintering processes are all carried out at a vacuum degree higher than 1.0×10-2 Pa conditions.

[0023] To achieve this purpose, the above steps (1) and (2) directly use metal powder and graphite powder to directly prepare high entropy alloy and high entropy ceramic powder by high energy ball milling. The preparation of high entropy alloy and high entropy ceramic powder can be directly and synchronously completed by high energy ball milling without multiple heat treatments. In addition, since high entropy alloy and high entropy ceramic are directly prepared by metal powder, more crystal defects can be artificially created during the ball milling process, which is conducive to improving the sintering characteristics of subsequent powders, further reducing the sintering temperature, and improving the densification degree of metal ceramics. At the same time, the high entropy ceramics formed by high energy ball milling are prepared by mixing metal powder with flake graphite and N2, which forms a large number of vacant solid solution high entropy ceramics between metal and C and N, and the internal non-metal atomic vacancies can change the atomic impurity state of the hard phase, and greatly affect its valence electron structure parameters, so that the electron density on the interface between the ceramic hard phase and the metal bonding phase is changed from discontinuous to continuous, thereby significantly improving the interface bonding strength. In addition, the metal is gradually flattened during the ball milling process, so that it combines with the flaky graphite to form lath-shaped hard phase particles. The above reasons are very beneficial to improving the strength and toughness of the sintered metal ceramics.

[0024] To achieve this purpose, in the above step (4), the ball-milled mixture of high entropy alloy and high entropy ceramic is dried in a vacuum far-infrared drying oven, the purpose is to allow alcohol to evaporate faster during the drying process, effectively shorten the drying time, reduce the interaction between the high-activity high entropy alloy and high entropy ceramic powder and external oxygen during the drying process, and maintain the high quality and purity of the mixed powder. At the same time, during the vacuum drying process, the dried alloy and ceramic powder will form particles of various shapes and sizes, which have very good fluidity and compressibility, which helps to improve the powder fluidity in the subsequent pressing process and improve the compact density.

[0025] To achieve this goal, vacuum sintering is divided into five stages. In the first stage, the temperature is raised to 400-600°C, the heating rate is 0.3-0.5°C / min, and the temperature is kept for 2-4 hours. In this stage, the temperature is slowly raised and kept for a long time, mainly to make the adsorbed oxygen on the surface of the highly active powder react with the additional free graphite, so that the oxygen is removed more thoroughly and the molding agent between the powders is completely decomposed; in the second stage, the temperature is raised to 800-1200°C, the heating rate is 1-2°C / min, and the temperature is kept for 1-2 hours. It is the solid phase reaction stage. Due to the slow diffusion effect of high entropy alloy and high entropy ceramic powder, the mutual diffusion between elements in this stage is slow. The contact and densification between alloy powder and ceramic powder mainly occur. Under the joint action of solid phase reaction and sintering, the bonding between powder particles is gradually strengthened to form a dense continuous structure. The grain boundaries are formed by the initial point contact or surface contact between grains, and the connection between grains is formed by material diffusion. The third stage is heated to 1300-1350℃, and the heating rate is 0.5-1℃ / min, keep warm for 2 to 3 hours. Due to the high activity of the high entropy alloy, part of the liquid phase will appear in the organization at this stage. As the grains continue to grow and fill with part of the liquid phase, the pores gradually shrink, and the density and strength of the sample are further improved. At the same time, accompanied by the strong mutual diffusion between the bonding phase and the hard phase elements, the bonding strength between the two phases is further increased; the fourth stage is heated to 1400-1480℃, the heating rate is 1-2℃ / min, and the heat preservation is 1-1.5h. This stage is the liquid phase sintering stage. The dissolution-precipitation process continues, the edges and corners of the large-grained hard phase are gradually blunted, and the proportion of the small-grained hard phase is further reduced. Under the capillary force of the liquid phase, the distribution of the ceramic hard phase particles in the bonding phase becomes more uniform. At the same time, the appearance of a large amount of liquid phase makes the high-entropy metal ceramics fully densified; the fifth stage is rapidly cooled to room temperature at a cooling rate of 15-25℃ / min. The rapid cooling in this stage can effectively inhibit the dissolution-precipitation of alloy elements, inhibit the formation of annular phases, and ensure the stability of the hard phase coreless structure. In addition, rapid cooling can also refine the ceramic phase particles to a certain extent, retaining more fine particles. Coupled with the lattice distortion effect of high-entropy alloys and high-entropy ceramics, the hardness and wear resistance of the material will be greatly improved. The formation of coreless structured metal ceramics greatly reduces the interfacial stress between the hard phase and the bonding phase of the metal ceramics, making the interface between the two phases more tightly bonded, and more energy is consumed when fractured by external forces, thus helping to improve the strength and toughness of the material, and ultimately making the coreless structured high-entropy metal ceramics have good comprehensive mechanical properties.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The high-entropy metal ceramic provided by the present invention directly prepares high-entropy alloys and high-entropy ceramics by high-energy ball milling of metal powder and graphite powder, and is simultaneously used in the preparation of metal ceramics. Since all powders are subjected to high-energy ball milling, the lattice distortion of the powder after high entropy treatment is large, which can effectively reduce the sintering temperature. Its hardness and toughness are significantly higher than those of metal ceramics prepared by traditional methods. By reasonably designing the alloy composition and preparation process, the degree of lattice distortion can be controlled, the performance of the metal ceramic can be optimized, and metal ceramic materials with different mechanical properties can be prepared.

[0028] 2. The present invention uses high-energy ball milling to gradually flatten the metal during the ball milling process, and combines with flaky graphite to form partially lath-shaped high-entropy ceramic hard phase particles. After sintering, due to the presence of the lath-shaped hard phase, the metal ceramic will play a role in passivating cracks, deflecting cracks, and absorbing impact energy when loaded, thereby hindering crack propagation and increasing the fracture toughness of the material.

[0029] 2. The metal ceramic hard phase structure prepared by the present invention is a coreless structure with lower interface stress. The formation of this structure is related to the slow diffusion effect of high entropy alloy and high entropy ceramic powder. In addition, the reasonable regulation of the heating rate and the holding time in different sintering stages makes the material fully dense while retaining the high hardness, high toughness and other characteristics brought by the high entropy powder to the greatest extent, effectively improving the comprehensive mechanical properties of the metal ceramic.

[0030] 3. The entire preparation process of the present invention is carried out under only one thermal cycle condition, the process is simple, and an ordinary vacuum sintering furnace can meet the production requirements, which is conducive to reducing costs and industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the SEM microstructure image of the high entropy metal ceramic prepared in Example 1. DETAILED DESCRIPTION

[0032] The following examples further illustrate the technical effects of the present invention. The raw materials used in the following examples are Ti powder, W powder, Mo powder, Ta powder, Cr powder, Ni powder, Co powder, Fe powder and flake graphite powder; the particle size of the flake graphite powder is 7-10 μm, and the particle sizes of the other powders are all 2-4 μm;

[0033] Table 1 shows the composition of high entropy ceramic mixtures with 4 component formulas, Table 2 shows the composition of high entropy alloy mixtures with 4 component formulas, and Table 3 shows the composition of high entropy metal ceramic mixtures with 4 component formulas. The three different process parameters of Examples 1-3 were used to prepare metal ceramics, and the Rockwell hardness, flexural strength and fracture toughness of the samples were measured. The following Rockwell hardness was measured according to GB / T 3849.1-2015 standard, the room temperature flexural strength was measured according to GB / T 3851-2015 standard, and the fracture toughness was measured according to GB / T33819-2017 standard.

[0034] Table 1 High entropy ceramic mixture composition (wt%)

[0035]

[0036] Table 2 Composition of high entropy alloy mixture (wt%)

[0037]

[0038] Table 3 Composition of high entropy metal ceramic mixture (wt%)

[0039] Example

[0040] 1. Preparation of high entropy ceramic mixture: Ti, W, Mo, Ta, Cr and flake graphite powder were used as raw materials to prepare high entropy ceramic mixture by high energy ball milling. Four kinds of high entropy ceramic mixtures were prepared according to Table 1 and placed in a planetary ball mill for ball milling. The ball-to-material ratio was 13:1, the ball mill speed was 450 rpm, and the ball milling time was 10 h. The whole process of ball milling was carried out under N2 atmosphere, and the N2 pressure in the ball mill was 0.3 atm.

[0041] 2. Preparation of high entropy alloy mixture: Ni, Co, Fe, Cr, and Ti were used as raw materials to prepare high entropy alloy mixtures by high-energy ball milling. Four kinds of high entropy alloy mixtures were prepared according to Table 2 and placed in a planetary ball mill for ball milling. The ball-to-material ratio was 8:1, the ball mill speed was 440 rpm, and the ball milling time was 10 h. The whole process of ball milling was carried out under Ar atmosphere, and the argon pressure in the ball mill tank was 0.7 atm.

[0042] 3. Wet grinding: According to the ingredients in Table 3, the high entropy ceramic mixture and the high entropy alloy mixture were mixed and wet-milled with graphite in a ball mill. The wet-milling medium was anhydrous ethanol, the amount of which was 1.7 times the weight of the mixture, the ball-to-material ratio was 4:1, the ball milling speed was 160 rpm, the ball milling time was 18 h, and after the ball milling, a mixed metal ceramic slurry was obtained;

[0043] 4. Vacuum drying: Place the metal ceramic slurry obtained in step 3 in a vacuum infrared drying oven for drying. During the drying process, the pressure of the drying oven must be maintained at 0.3 atm throughout the process, and the drying temperature is 80°C;

[0044] 5. Adding a molding agent: Add a molding agent to the mixed powder after vacuum drying in step 4. The molding agent is a polyethylene glycol aqueous solution, and the addition ratio is 6wt% of the mixed material;

[0045] 6. Pressing: Bidirectional pressing is adopted, and the pressure used for pressing is 280MPa;

[0046] 7. Vacuum sintering: It is carried out in a vacuum / atmosphere integrated furnace. First, the sintering furnace with the green body is heated to 400°C at a heating rate of 0.4°C / min and kept at this temperature for 4 hours; then the temperature is raised to 1000°C at a heating rate of 1°C / min and kept at this temperature for 1.5 hours; then the temperature is raised to 1350°C at a heating rate of 1°C / min and kept at this temperature for 2 hours; then the temperature is raised to 1450°C at a heating rate of 2°C / min and kept at this temperature for 1 hour; finally, the temperature is rapidly cooled to room temperature at a cooling rate of 20°C / min. The above sintering processes are all carried out in a vacuum degree higher than 1.0×10 - 2 Pa conditions.

[0047] Under the above preparation process conditions, the mechanical properties of metal ceramics prepared with different component ratios are shown in Table 4.

[0048] Table 4 Mechanical properties of different metal ceramics prepared in Example 1

[0049]

[0050] Figure 1 This is a SEM microstructure image of the high entropy metal ceramic prepared in this embodiment, in which it can be seen that the hard phase of the metal ceramic has no obvious black core structure, and it is a coreless high entropy metal ceramic.

[0051] Example 2

[0052] The steps for preparing the metal ceramic in this embodiment are as follows:

[0053] 1. Preparation of high entropy ceramic mixture: Ti, W, Mo, Ta, Cr and flake graphite powder were used as raw materials to prepare high entropy ceramic mixture by high-energy ball milling. Four kinds of high entropy ceramic mixtures were prepared according to Table 1 and placed in a planetary ball mill for ball milling. The ball-to-material ratio was 20:1, the ball mill speed was 350 rpm, the ball milling time was 8 h, and the ball milling was carried out under N2 atmosphere throughout the process. The N2 pressure in the ball mill was 0.4 atm.

[0054] 2. Preparation of high entropy alloy mixture: Ni, Co, Fe, Cr, and Ti were used as raw materials to prepare high entropy alloy mixtures by high-energy ball milling. Four kinds of high entropy alloy mixtures were prepared according to Table 2 and placed in a planetary ball mill for ball milling. The ball-to-material ratio was 12:1, the ball mill speed was 500 rpm, and the ball milling time was 12 h. The whole process of ball milling was carried out under Ar atmosphere, and the argon pressure in the ball mill was 0.8 atm.

[0055] 3. Wet grinding: According to the ingredients in Table 3, the high entropy ceramic mixture and the high entropy alloy mixture were mixed and wet-milled with graphite in a ball mill. The wet-milling medium was anhydrous ethanol, the amount of which was 1.6 times the weight of the mixture, the ball-to-material ratio was 6:1, the ball milling speed was 100 rpm, the ball milling time was 24 h, and after the ball milling, a mixed metal ceramic slurry was obtained;

[0056] 4. Vacuum drying: Place the metal ceramic slurry obtained in step 3 in a vacuum infrared drying oven for drying. The pressure of the drying oven needs to be maintained at 0.5 atm throughout the drying process, and the drying temperature is 100°C.

[0057] 5. Adding a molding agent: Add a molding agent to the mixed powder after vacuum drying in step 4. The molding agent is a mixed aqueous solution of paraffin and polyethylene glycol, and the addition ratio is 5wt% of the mixed material;

[0058] 6. Pressing: Bidirectional pressing is adopted, and the pressure used for pressing is 220MPa;

[0059] 7. Vacuum sintering: It is carried out in a vacuum / atmosphere integrated furnace. First, the sintering furnace with the green body is heated to 600℃, the heating rate is 0.5℃ / min, and the temperature is kept for 3h; then the temperature is raised to 800℃, the heating rate is 2℃ / min, and the temperature is kept for 2h; then the temperature is raised to 1320℃, the heating rate is 0.7℃ / min, and the temperature is kept for 2.5h; then the temperature is raised to 1400℃, the heating rate is 1℃ / min, and the temperature is kept for 1.5h; finally, it is quickly cooled to room temperature at a cooling rate of 25℃ / min. The above sintering processes are all carried out in a vacuum degree higher than 1.0×10 -2 Pa conditions.

[0060] Under the above preparation process conditions, the mechanical properties of metal ceramics prepared with different component ratios are shown in Table 5.

[0061] Table 5 Mechanical properties of different metal ceramics prepared in Example 2

[0062] Example

[0063] The steps for preparing the metal ceramic in this embodiment are as follows:

[0064] 1. Preparation of high entropy ceramic mixture: Ti, W, Mo, Ta, Cr and flake graphite powder were used as raw materials to prepare high entropy ceramic mixture by high energy ball milling. Four kinds of high entropy ceramic mixtures were prepared according to Table 1 and placed in a planetary ball mill for ball milling. The ball-to-material ratio was 10:1, the ball mill speed was 380 rpm, and the ball milling time was 16 h. The whole process of ball milling was carried out under N2 atmosphere, and the N2 pressure in the ball mill was 0.5 atm.

[0065] 2. Preparation of high entropy alloy mixture: Ni, Co, Fe, Cr, and Ti were used as raw materials to prepare high entropy alloy mixtures by high-energy ball milling. Four kinds of high entropy alloy mixtures were prepared according to Table 2 and placed in a planetary ball mill for ball milling. The ball-to-material ratio was 15:1, the ball mill speed was 400 rpm, and the ball milling time was 6 h. The whole process of ball milling was carried out under Ar atmosphere, and the argon pressure in the ball mill tank was 0.5 atm.

[0066] 3. Wet grinding: According to the ingredients in Table 3, the high entropy ceramic mixture and the high entropy alloy mixture were mixed and wet-milled with graphite in a ball mill. The wet-milling medium was anhydrous ethanol, the amount of which was 1.5 times the weight of the mixture, the ball-to-material ratio was 5:1, the ball milling speed was 200 rpm, the ball milling time was 20 h, and after the ball milling was completed, a mixed metal ceramic slurry was obtained;

[0067] 4. Vacuum drying: Place the metal ceramic slurry obtained in step 3 in a vacuum infrared drying oven for drying. During the drying process, the pressure of the drying oven must be maintained at 0.4 atm throughout the process, and the drying temperature is 90°C;

[0068] 5. Adding molding agent: Add molding agent to the mixed powder after vacuum drying in step 4. The molding agent is a paraffin aqueous solution, and the addition ratio is 4wt% of the mixed material;

[0069] 6. Pressing: Bidirectional pressing is adopted, and the pressure used for pressing is 320MPa;

[0070] 7. Vacuum sintering: It is carried out in a vacuum / atmosphere integrated furnace. First, the sintering furnace with the green body is heated to 450℃, the heating rate is 0.3℃ / min, and the temperature is kept for 3.5h; then the temperature is raised to 1200℃, the heating rate is 1.5℃ / min, and the temperature is kept for 1h; then the temperature is raised to 1300℃, the heating rate is 0.5℃ / min, and the temperature is kept for 3h; then the temperature is raised to 1480℃, the heating rate is 1.5℃ / min, and the temperature is kept for 1h; finally, the temperature is quickly cooled to room temperature at a cooling rate of 15℃ / min. The above sintering processes are all carried out in a vacuum degree higher than 1.0×10 -2 Pa conditions.

[0071] Under the above preparation process conditions, the mechanical properties of metal ceramics prepared with different component ratios are shown in Table 6.

[0072] Table 6 Mechanical properties of different metal ceramics prepared in Example 3

[0073]

[0074] Within the value range of the claims, the synthesis process parameters and sintering parameters of high entropy alloy and high entropy ceramic powders have a relatively large influence on the mechanical properties. Only when the sintering temperature and holding time in the sintering stage are reasonably matched, the solid-phase and liquid-phase sintering processes in the above stages can be reasonably and fully carried out to prepare high entropy metal ceramics with better comprehensive mechanical properties. Within the value range of the claims, its influence on the mechanical properties of the material is limited.

[0075] The above embodiments are only used to illustrate the contents of the present invention rather than to limit the present invention. Therefore, any changes within the meaning and scope equivalent to the claims of the present invention should be considered to be included in the scope of the claims.

[0076] The present invention has many specific application paths. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements can be made without departing from the principle of the present invention. These improvements should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a coreless high-entropy metal ceramic, characterized in that: The metal ceramic is prepared from high entropy ceramic and high entropy alloy powder as raw materials, and the metal ceramic microstructure is composed of hard phase particles with a coreless structure and a high entropy alloy matrix bonding phase; The raw materials of the metal ceramic are composed of the following mass percentages: Ti: 8.47-9.29wt%, W: 24.65-27.16wt%, Mo: 12.87-14.17wt%, Cr: 9.20-10.10wt%, Ta: 24.26-26.73wt%, Ni: 1.71-3.52wt%, Co: 1.72-3.54wt%, Fe: 1.63-3.35wt%, C: 8.41-9.20wt%; In the composition of the metal ceramic, all metal elements are introduced from single metal powder, and C is introduced from flake graphite powder; wherein the particle size of the flake graphite powder is 7-10 μm, and the particle size of the remaining powders is 2-4 μm; The method for preparing the metal ceramic further comprises the following steps: (1) Preparation of high entropy ceramic mixtures: A mixture of Ti, W, Mo, Ta, Cr and flake graphite powder is prepared as raw materials with the following mass percentages: Ti: 6.42-7.07wt%, W: 24.65-27.16wt%, Mo: 12.87-14.17wt%, Cr: 6.97-7.68wt%, Ta: 24.26-26.73wt%, C: 8.05-8.87wt%, and a high entropy ceramic mixture is prepared by high-energy ball milling; Preparation of high entropy alloy mixture: A mixture of Ni, Co, Fe, Cr and Ti with a mass percentage of Ni: 1.71-3.52wt%, Co: 1.72-3.54wt%, Fe: 1.63-3.35wt%, Cr: 1.52-3.13wt%, and Ti: 1.40-2.87wt% is prepared using Ni, Co, Fe, Cr and Ti as raw materials, and a high entropy alloy mixture is prepared by high-energy ball milling; (3) wet grinding: the high entropy ceramic mixture and the high entropy alloy mixture prepared in step (1) and step (2) are mixed and wet-ground together with an additional 0.34-0.37 wt % of graphite in a ball mill to obtain a mixed metal-ceramic slurry; (4) vacuum drying the mixed slurry obtained in step (3), adding a forming agent, pressing and vacuum sintering to obtain the high entropy metal ceramic with a coreless structure; The high-energy ball milling of step (1) is carried out in a planetary ball mill, the ball milling process is dry milling, the grinding balls are carbide balls, the ball-to-material ratio is 10:1-20:1, the ball milling speed is 350-450 rpm, the ball milling time is 8-16 h, the ball milling is carried out in a N2 atmosphere, and the N2 pressure in the ball mill is 0.3-0.5 atm; the high-energy ball milling of step (2) is carried out in a planetary ball mill, the ball milling process is dry milling, the grinding balls are carbide balls, the ball-to-material ratio is 8:1-15:1, the ball milling speed is 400-500 rpm, the ball milling time is 6-12 h, the ball milling is carried out in an Ar atmosphere, and the argon pressure in the ball mill is 0.5-0.8 atm; The wet grinding of step (3) is carried out in a planetary ball mill, wherein the high entropy ceramic accounts for 68% to 84% of the total mass of the raw materials, the high entropy alloy mixture accounts for 16% to 32% of the total mass of the raw materials, the grinding balls are cemented carbide balls, the ball-to-material ratio is 4:1 to 6:1, the ball milling speed is 100 to 200 rpm, the ball milling time is 18 to 24 hours, and the wet grinding medium is anhydrous ethanol, and the amount thereof added is preferably 1.5 to 1.7 times the weight of the mixture; The vacuum sintering process of step (4) is mainly divided into five stages: the first stage, heating to 400-600°C, heating rate of 0.3-0.5°C / min, and keeping warm for 2-4h; the second stage, heating to 800-1200°C, heating rate of 1-2°C / min, and keeping warm for 1-2h; the third stage, heating to 1300-1350°C, heating rate of 0.5-1°C / min, and keeping warm for 2-3h; the fourth stage, heating to 1400-1480°C, heating rate of 1-2°C / min, and keeping warm for 1-1.5h; the fifth stage, rapidly cooling to room temperature at a cooling rate of 15-25°C / min; the above sintering processes are all carried out at a vacuum degree higher than 1.0×10 -2 Pa conditions.

2. The method for preparing a coreless high-entropy metal ceramic according to claim 1, characterized in that: The vacuum drying in step (4) refers to drying in a vacuum infrared drying oven. During the drying process, the pressure of the drying oven must be maintained below 0.5 atm throughout the process, and the drying temperature is 80-100°C.

3. The method for preparing a coreless high-entropy metal ceramic according to claim 1, characterized in that: The adding of molding agent in step (4) refers to adding one or both of paraffin wax and polyethylene glycol, and the total adding ratio is 4-6wt% of the mixture; the pressing molding refers to bidirectional pressing at a pressure of 220-320MPa.