A method for comprehensive recovery of P, Fe and Li from black powder of lithium iron phosphate battery

Through side-blown melt selective reduction and melt iron extraction reduction technology, combined with wet lithium extraction, the problem of large amount of acid and alkali reagents in the positive electrode material recovery of lithium iron phosphate batteries is solved, and efficient recovery and high quality of phosphorus, iron and lithium are achieved. The production of purity products reduces environmental pollution and resource waste.

CN118637569BActive Publication Date: 2024-11-01CHINA ENFI ENG CORP +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411111909.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-01
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The large amount of acid and alkali reagents and excessive impurities are used in the recycling of the positive electrode materials of existing lithium iron phosphate batteries, which makes it difficult to economically recover iron slag, and the formation of lithium fluoride affects the leaching recovery rate and product purity.

Method used

Side-blown melt selective reduction of volatile phosphorus and melt iron extraction reduction technology are used to control the temperature and additive ratio, and then the lithium is extracted by wet method to reduce the use of acid and alkali reagents and improve product purity.

Benefits of technology

It realizes efficient recycling of P, Fe and Li in lithium iron phosphate battery black powder, reduces waste slag and wastewater problems, improves resource utilization and product purity, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118637569B_ABST
    Figure CN118637569B_ABST
Patent Text Reader

Abstract

The invention discloses a method for comprehensive recovery of P, Fe and Li from black powder of lithium iron phosphate battery, wherein the method comprises phosphorus recovery: controlling the Fe / SiO2 mass ratio in the raw material to 0.5-1.6 by adding quartz stone, and performing side-blowing melting selective reduction volatilization phosphorus refining at 1300-1450°C to obtain yellow phosphorus or P2O5; iron recovery: adding limestone to the smelting slag after phosphorus recovery to control the CaO / SiO2 mass ratio to 0.5-1.2, and controlling the temperature to 1400-1500°C under reducing conditions to perform melting iron reduction to obtain molten iron and slag; in the step of phosphorus recovery, the raw material is the black powder of lithium iron phosphate battery or the phosphorus iron slag obtained after the black powder of lithium iron phosphate battery is wet-processed to extract lithium. The invention can effectively produce high-purity phosphorus and iron products without a large amount of acid and alkali reagents, and realize high-value recovery of phosphorus and iron resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of recycling waste materials such as lithium iron phosphate batteries, and in particular to a method for comprehensively recycling P, Fe and Li from black powder of lithium iron phosphate batteries. Background Art

[0002] The average service life of lithium iron phosphate batteries is 5 to 8 years, and they will inevitably face the situation of large-scale retirement of lithium iron phosphate batteries in the future. The existing recycling of lithium iron phosphate battery positive electrode materials usually adopts hydrometallurgical processes to extract valuable metal elements by full component leaching or selective leaching. Due to the relatively low inherent value of P and Fe in the positive electrode materials, and the difficulty in removing impurities such as Al and Cu in the lithium extraction slag, the current hydrometallurgical recycling of lithium iron phosphate batteries mainly recycles lithium Li with higher economic value, resulting in the production of a large amount of phosphorus iron slag containing P and Fe elements, which is mainly stored in the form of waste slag, occupying a large amount of land resources and causing pollution to the environment. At the same time, as an urban mineral resource containing P and Fe, it has not been effectively recycled, resulting in a huge waste of resources.

[0003] Waste materials such as lithium iron phosphate batteries contain positive electrode material lithium iron phosphate, negative electrode material (graphite), current collector, electrolyte, diaphragm, shell, etc., and their composition is relatively complex. In the prior art, in order to improve the separation of valuable elements and improve the regeneration process conditions of positive electrode materials, it is necessary to carry out a relatively complex pretreatment and sorting process on waste battery materials to minimize the impact of the content of iron, aluminum, copper, and organic impurities in the raw materials on the purity of subsequent products. During the pretreatment of waste batteries, the battery electrolyte lithium hexafluorophosphate is very easy to decompose during the pretreatment process and then enter the positive and negative electrode powders. Fluorine enters the positive electrode powder obtained by pretreatment and is easy to form lithium fluoride during the roasting process. The formation of lithium fluoride will seriously affect the subsequent lithium leaching recovery rate. In addition, fluorine also affects the purity of subsequent products.

[0004] The currently disclosed recovery technology for positive electrode materials of lithium iron phosphate batteries is mainly to selectively leach and extract lithium, and then dissolve and classify the phosphorus and / or iron from the ferrophosphorus slag to extract phosphorus and / or iron; for example: the wet recovery of lithium iron phosphate, selective leaching and extraction of lithium, and the recovery of phosphorus and / or iron in the positive electrode materials of lithium iron phosphate batteries after lithium extraction disclosed in documents such as CN 113896211A, CN110331288A, and CN 115369249 A. However, in the technical solutions for selective leaching and extraction of lithium and recovery of positive electrode materials of lithium iron phosphate batteries after lithium extraction recorded above, there are generally high reagent costs, large amounts of wastewater, and leaching of copper and aluminum impurity elements during acid leaching, which leads to difficulties in subsequent impurity removal and difficulty in economic recovery of ferrophosphorus slag. Therefore, how to achieve economic recovery of low-value iron and phosphorus is a technical direction that urgently needs to be broken through in the future. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the prior art in the recovery of P, Fe, and Li in the positive electrode material of lithium iron phosphate batteries or the recovery of P and Fe in ferrophosphorus slag, such as the large amount of acid and alkali reagents used and the excessive impurities in the regenerated iron phosphate product, thereby providing a method for comprehensive recovery of P, Fe, and Li from black powder of lithium iron phosphate batteries to solve the above problems.

[0006] A method for comprehensively recovering P, Fe and Li from lithium iron phosphate battery black powder, comprising the steps of recovering lithium, recovering phosphorus and recovering iron from the lithium iron phosphate battery black powder;

[0007] When the raw material is lithium iron phosphate battery black powder, the steps of phosphorus recovery, iron recovery and lithium recovery are performed in sequence; when the raw material is phosphorus iron slag obtained by wet lithium extraction from lithium iron phosphate battery black powder, the steps of phosphorus recovery and iron recovery are performed in sequence;

[0008] In the phosphorus recovery step: the Fe / SiO2 mass ratio in the raw material is controlled to be 0.5-1.6 by adding quartz stone, and the side-blowing melting selective reduction volatilization phosphorus refining is carried out at 1300-1500°C to obtain yellow phosphorus or P2O5;

[0009] In the iron recovery step: limestone is added to the smelting slag after phosphorus recovery to control the CaO / SiO2 mass ratio to 0.5-1.2, and the temperature is controlled to 1400-1500° C. under reducing conditions to perform molten iron reduction to obtain molten iron and slag;

[0010] In the lithium recovery step, the slag obtained from the iron recovery step is subjected to wet lithium extraction to recover lithium.

[0011] In the phosphorus recovery step, the temperature of the side blowing melt is preferably 1350-1500°C.

[0012] In the process of side-blowing molten selective reduction volatilization phosphorus refining, the C / P molar ratio is (0.5-3):1, preferably (0.5-1):1.

[0013] In the process of side-blowing molten selective reduction volatilization phosphorus refining, the combustion coefficient of the injected fuel is controlled to be 0.6-0.85. The combustion coefficient refers to the mass ratio of the actual amount of oxygen required for the injected fuel to the theoretical amount of oxygen required.

[0014] The injection fuel is one or more of natural gas, pulverized coal, anthracite, heavy oil and the like.

[0015] In the step of smelting iron reduction, an electric furnace or a side-blown furnace is used for smelting.

[0016] In the step of molten iron reduction, when smelting is performed in an electric furnace, the C / Fe molar ratio is (1-3):1, preferably (1-2):1.

[0017] In the step of molten iron reduction, when a side-blown furnace is used for smelting, pulverized coal injection is used to supply heat and achieve iron reduction, the pulverized coal combustion coefficient is 0.65-0.8, and oxygen-enriched air is injected to utilize excess pulverized coal to participate in iron reduction. After injecting oxygen-enriched air, the oxygen concentration is controlled to be 55%-80%.

[0018] The technical solution of the present invention has the following advantages:

[0019] 1. A method for comprehensively recovering P, Fe and Li from lithium iron phosphate battery black powder provided by the present invention comprises the steps of recovering lithium, recovering phosphorus and recovering iron from the raw material; when the raw material is lithium iron phosphate battery black powder, the steps of recovering phosphorus, recovering iron and recovering lithium are performed in sequence; when the raw material is phosphorus iron slag obtained after wet lithium extraction from lithium iron phosphate battery black powder, the steps of recovering phosphorus and recovering iron are performed in sequence; in the phosphorus recovery step: the Fe / SiO2 mass ratio in the raw material is controlled to 0.5-1.6 by adding quartz stone, and side-blowing molten selective reduction volatilization phosphorus is performed at 1300-1500°C to obtain yellow phosphorus or P2O5; in the iron recovery step: limestone is added to the smelting slag after phosphorus recovery to control the CaO / SiO2 mass ratio to 0.5-1.2, and the temperature is controlled to 1400-1500°C under reducing conditions to perform molten iron extraction reduction to obtain molten iron and slag; in the lithium recovery step, the slag obtained in the iron recovery step is used to perform wet lithium extraction to recover lithium. The method of the present invention can not only realize the recovery of P, Fe and Li in the black powder of lithium iron phosphate batteries, but also effectively realize the recovery of P and Fe in ferrophosphorus slag, and effectively solve the problems of waste slag, wastewater, etc., so as to realize the purpose of converting and utilizing low-value metals into high-value products.

[0020] The implementation mechanism of the present invention is: controlling the selective reduction of phosphorus and iron during the reduction melting process, wherein, in the side-blowing melting selective reduction volatilization phosphorus smelting process, by controlling the temperature and the Fe / SiO2 mass ratio within a specific range, the selective reduction of phosphorus is effectively achieved while the iron is not reduced, and the phosphorus volatilization is achieved by combining with the temperature control, and the phosphorus resources can be recovered by condensing the phosphorus-containing flue gas. This method can obtain high-purity yellow phosphorus or P2O5; and the smelting slag after dephosphorization is then melted for iron extraction reduction, and the effective reduction of iron is effectively achieved by controlling the CaO / SiO2 mass ratio within a specific range, and the temperature control is combined to obtain low-phosphorus molten iron and slag, and the molten iron can be discharged regularly. Dephosphorization produces qualified and high-purity molten iron, and then ingot casting produces pig iron; if the raw material is lithium iron phosphate battery black powder, lithium iron phosphate battery black powder can be used to first recover phosphorus and then recover iron to obtain lithium-rich slag, and after iron recovery is achieved, the slag can be used for wet lithium extraction to achieve lithium recovery; in the lithium recovery step, since phosphorus and iron have been excluded, the slag can be directly subjected to conventional wet lithium extraction without the need for a large amount of acid and alkali reagents to achieve lithium recovery; and under the treatment method of the present invention, fluorine opens the circuit in the form of smoke and dust during the volatilization of phosphorus refining and molten iron extraction, effectively solving the impact of fluorine on subsequent lithium products, and can further ensure the yield and purity of subsequent lithium products, and can achieve separate classification and recovery of fluorine. Therefore, the method of the present invention can effectively produce high-purity phosphorus, iron, lithium and other products without the need for a large amount of acid and alkali reagents, and realize high-value recovery of phosphorus, iron and lithium resources.

[0021] 2. The present invention adopts a pyrometallurgical melting method to recover P, Fe, and Li in the positive electrode material of the battery. It has no special requirements on the content of elements such as iron, aluminum, copper, fluorine, and organic impurities in the raw materials. It has strong applicability and can comprehensively classify and recover valuable alloys and phosphorus resources, and separately recover fluorine-containing smoke.

[0022] 3. The method of the present invention has high smelting reduction reaction efficiency, high side-blowing heat utilization rate, relatively pure flue gas, reduced waste slag discharge, land occupied by storage, avoided environmental pollution, and improved technical and economic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 is a process flow chart of Example 1 of the present invention;

[0025] Figure 2 is a process flow chart of Example 2 of the present invention;

[0026] Figure 3 It is a schematic diagram of the structure of the system of Example 7 of the present invention.

[0027] Reference numerals:

[0028] 1-side blowing smelting area; 2-secondary combustion nozzle of side blowing flue; 3-side blowing flue; 4-side blowing charging port; 5-fuel spray gun and carrier spray gun in side blowing area; 6-liquid level line; 7-bottom base of side blowing furnace; 8-molten iron layer in electric heating reduction area; 9-slag layer in electric heating area; 10-electrode; 11-slag discharge port; 12-molten iron discharge port; 13-connecting channel between side blowing area and electric heating reduction area. DETAILED DESCRIPTION

[0029] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0030] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0031] Example 1

[0032] A method for comprehensive recovery of P, Fe and Li from black powder of lithium iron phosphate battery, such as Figure 1 As shown, it includes: the recovery of phosphorus, iron and lithium resources from lithium iron phosphate battery black powder, the selective reduction and volatilization of phosphorus through a side-blown furnace to obtain P2O5 smoke (including smoke and phosphorus-containing flue gas), the deep reduction through an electric furnace to obtain pig iron products, and the enriched lithium-containing tailings through hydrometallurgical extraction.

[0033] Specifically, the composition of lithium iron phosphate battery black powder is shown in Table 1. Based on 100 parts by mass, 11.77% of quartz stone is added to the side-blown furnace to control the Fe / SiO2 mass ratio to 1.51, 28% of anthracite is added to make the C / P molar ratio to 0.65:1, and 18Nm of natural gas is introduced. 3 / h and oxygen-enriched air 41.90Nm 3 / h provides heat energy to make the smelting temperature reach 1400℃, wherein the oxygen concentration in the side-blown furnace is 80% to control the combustion coefficient of the injected fuel between 0.6 and 0.85; the dephosphorized smelting slag produced is shown in Table 2, and the composition of the phosphorus-containing flue gas is shown in Table 3. After condensing the phosphorus-containing flue gas, a P2O5 product with a purity of 80% is obtained, and the yield of the P2O5 product is 92%.

[0034] Table 1 Lithium iron phosphate battery black powder composition wt%

[0035]

[0036] Table 2 Composition of side-blowing dephosphorization smelting slag wt%

[0037]

[0038] Table 3 Phosphorus-containing flue gas components V%

[0039]

[0040] The dephosphorization smelting slag is subjected to a molten iron reduction treatment, limestone is added to adjust the CaO / SiO2 mass ratio to 1.2, the reducing agent is anthracite, and the preferred addition amount of anthracite is 20-25% of the dephosphorization smelting slag. In this embodiment, the anthracite addition amount is 23% to control the C / Fe molar ratio to 1.75, and the temperature in the electric furnace is controlled to be 1450°C. The composition of the produced lithium-containing tailings (lithium-containing slag) is shown in Table 4, and the composition of the reduced molten iron (phosphorus iron) is shown in Table 5.

[0041] Table 4 wt% of lithium-containing tailings after deep reduction and iron extraction in electric furnace

[0042]

[0043] Table 5 Reduced iron composition wt%

[0044]

[0045] After conversion of the acquired data, it was concluded that the yield of iron was 94%.

[0046] The lithium-containing tailings after iron extraction are extracted by conventional hydrometallurgy. The specific hydrometallurgical process of extracting lithium is: the lithium-containing tailings are leached by sulfuric acid process, filtered to obtain filtrate, purified and impurity-removed, and sodium carbonate is added for evaporation and crystallization to obtain sodium sulfate and lithium carbonate products. The lithium carbonate content in the lithium carbonate product of the present invention is 95% to 97%, and the recovery rate of lithium is 85% to 90%.

[0047] Example 2

[0048] A method for comprehensive recovery of P, Fe and Li from black powder of lithium iron phosphate battery, such as Figure 2 As shown, it includes: recovering phosphorus and iron resources from the ferrophosphorus slag after lithium extraction from the black powder of lithium iron phosphate batteries. Among them, the selective reduction and volatilization of phosphorus is completed in the side-blown furnace to obtain P2O5 smoke (including smoke and phosphorus-containing flue gas), and the pig iron product is obtained by deep reduction in the electric furnace.

[0049] Specifically, the composition of the ferrophosphorus slag after lithium extraction from the black powder of the lithium iron phosphate battery is shown in Table 6. Based on the mass fraction of the ferrophosphorus slag being 100, 17.05% of the mass of quartz stone is added to the side-blown furnace to control the Fe / SiO2 at 1.2, 42% of the mass of anthracite is added to make the C / P molar ratio reach 0.85:1, and 28Nm of natural gas is introduced. 3 / h and oxygen-enriched air 67Nm 3 / h provides heat energy to make the smelting temperature reach 1430℃, wherein the oxygen concentration in the side-blown furnace is 80% to control the combustion coefficient of the injected fuel between 0.6 and 0.85; the composition of the produced dephosphorized smelting slag is shown in Table 7, and the composition of the phosphorus-containing flue gas is shown in Table 8. After condensation of the phosphorus-containing flue gas, phosphoric acid with a concentration of 78% is obtained, and the recovery rate of P is 93%.

[0050] Table 6 Phosphorus ferro-slag composition wt%

[0051]

[0052] Table 7 Composition of side-blowing dephosphorization molten slag by weight

[0053]

[0054] Table 8 Phosphorus-containing flue gas components V%

[0055]

[0056] The dephosphorization smelting slag was subjected to a molten iron reduction treatment, and limestone was added to adjust the CaO / SiO2 to 1.2. The reducing agent was anthracite, and the amount of anthracite added was 20.84% ​​of the dephosphorization smelting slag, thereby controlling the C / Fe molar ratio to 1.35:1, and the temperature in the electric furnace was controlled to be 1450°C. The composition of the iron-extracting lithium-containing tailings is shown in Table 9, and the composition of the reduced molten iron (phosphorus iron) is shown in Table 10.

[0057] Table 9 Composition of tailings from deep iron extraction in electric furnace (wt%)

[0058]

[0059] Table 10 Reduced iron composition wt%

[0060]

[0061] After conversion of the test data, it was found that the iron yield was 92%.

[0062] Example 3

[0063] A method for comprehensive recovery of P, Fe and Li from black powder of lithium iron phosphate battery, such as Figure 1As shown, it includes: the recovery of phosphorus, iron and lithium resources from lithium iron phosphate battery black powder, the selective reduction and volatilization of phosphorus through a side-blown furnace to obtain P2O5 smoke, the deep reduction through an electric furnace to obtain pig iron products, and the lithium-containing tailings after extraction and enrichment through hydrometallurgy.

[0064] Specifically, the composition of lithium iron phosphate battery black powder is shown in Table 1. Based on the mass percentage of lithium iron phosphate battery black powder being 100, quartz is added into the side-blown furnace to control the Fe / SiO2 mass ratio to be 0.6, anthracite is added to make the C / P molar ratio to be 1, and 30Nm natural gas is introduced. 3 / h and oxygen-enriched air 70Nm 3 / h provides heat energy to make the smelting temperature reach 1480℃, wherein the oxygen concentration in the side-blown furnace is 55% to control the combustion coefficient of the injected fuel between 0.6 and 0.85; the dephosphorized smelting slag produced is shown in Table 11, and the composition of the phosphorus-containing flue gas is shown in Table 12. After condensing the phosphorus-containing flue gas, P2O5 with a purity of 72% is obtained, and the yield of P2O5 is 80%.

[0065] Table 11 Side-blowing dephosphorization smelting slag composition wt%

[0066]

[0067] Table 12 Phosphorus-containing flue gas components V%

[0068]

[0069] The dephosphorized smelting slag was subjected to a molten iron reduction treatment, limestone was added to adjust the CaO / SiO2 mass ratio to 0.8, anthracite was used as the reducing agent, the C / Fe molar ratio after the anthracite was added was 1, and the temperature in the electric furnace was controlled to be 1400°C. The composition of the iron-extracting lithium-containing tailings produced is shown in Table 13, and the composition of the reduced molten iron is shown in Table 14.

[0070] Table 13 wt% of lithium-containing tailings after deep reduction and iron extraction in electric furnace

[0071]

[0072] Table 14 Reduced iron molten iron composition wt%

[0073]

[0074] After conversion of the above data, it was found that the iron yield was 93%.

[0075] The lithium-containing tailings after iron extraction are subjected to conventional hydrometallurgical extraction of lithium, and the specific hydrometallurgical extraction process of lithium is the same as that of Example 1. The lithium carbonate content in the lithium carbonate product of the present invention is 95%-97%, and the recovery rate of lithium is 85%-90%.

[0076] Example 4

[0077] A method for comprehensive recovery of P, Fe and Li from black powder of lithium iron phosphate battery, such as Figure 1 As shown, it includes: the recovery of phosphorus, iron and lithium resources from lithium iron phosphate battery black powder, the selective reduction and volatilization of phosphorus through a side-blown furnace to obtain P2O5 smoke, the deep reduction through an electric furnace to obtain pig iron products, and the lithium-containing tailings after extraction and enrichment through hydrometallurgy.

[0078] Specifically, the composition of lithium iron phosphate battery black powder is shown in Table 1. Based on 100 parts by mass of lithium iron phosphate battery black powder, quartz is added into the side-blown furnace to control the Fe / SiO2 mass ratio to 1.2, anthracite is added to make the C / P molar ratio to 1, and 16Nm natural gas is introduced. 3 / h and oxygen-enriched air 36Nm 3 / h provides heat energy to make the smelting temperature reach 1380℃, wherein the oxygen concentration in the side-blown furnace is 70% to control the combustion coefficient of the injected fuel between 0.6 and 0.85; the dephosphorized smelting slag produced is shown in Table 15, and the composition of the phosphorus-containing flue gas is shown in Table 16. After condensing the phosphorus-containing flue gas, P2O5 with a purity of 82% is obtained, and the yield of P2O5 is 88%.

[0079] Table 15 Side-blowing dephosphorization smelting slag composition wt%

[0080]

[0081] Table 16 Phosphorus-containing flue gas components V%

[0082]

[0083] The dephosphorized smelting slag was subjected to a molten iron reduction treatment, limestone was added to adjust the CaO / SiO2 to 1.15, anthracite was used as the reducing agent, the C / Fe molar ratio after the anthracite was added was 2, and the temperature in the electric furnace was controlled to be 1500°C. The composition of the iron-extracting lithium-containing tailings produced is shown in Table 17, and the composition of the reduced molten iron is shown in Table 18.

[0084] Table 17 wt% of lithium-containing tailings after deep reduction and iron extraction in electric furnace

[0085]

[0086] Table 18 Reduced iron molten iron composition wt%

[0087]

[0088] After conversion of the above data, it was found that the iron yield was 94%.

[0089] The lithium-containing tailings after iron extraction are subjected to conventional hydrometallurgical extraction of lithium, and the specific hydrometallurgical extraction process of lithium is the same as that of Example 1. In the present invention, the lithium carbonate content is about 95% to 97%, and the recovery rate of lithium is 85% to 90%.

[0090] Example 5

[0091] A method for comprehensive recovery of P, Fe and Li from black powder of lithium iron phosphate battery, such as Figure 2 As shown, it includes: recovering phosphorus and iron resources from the ferrophosphorus slag after lithium extraction from the black powder of lithium iron phosphate batteries, obtaining P2O5 smoke by selective reduction and volatilization of phosphorus through a side-blown furnace, and obtaining pig iron products by deep reduction in an electric furnace.

[0092] Specifically, the composition of the ferrophosphorus slag after lithium extraction from the black powder of lithium iron phosphate battery is shown in Table 6. Based on the mass percentage of ferrophosphorus slag of 100, quartz stone is added to the side-blown furnace to control the Fe / SiO2 mass ratio to 0.5, anthracite is added to make the C / P molar ratio to 1, and 23Nm of natural gas is introduced. 3 / h and oxygen-enriched air 50Nm 3 / h provides heat energy to make the smelting temperature reach 1450℃, wherein the oxygen concentration in the side-blown furnace is 55% and the combustion coefficient of the injected fuel is controlled between 0.6 and 0.85; the dephosphorized smelting slag produced is shown in Table 19, and the composition of the phosphorus-containing flue gas is shown in Table 20. After condensation of the phosphorus-containing flue gas, the dilute phosphoric acid with a purity of 77% is obtained, of which the yield of P2O5 is 93%.

[0093] Table 19 Side-blowing dephosphorization molten slag composition wt%

[0094]

[0095] Table 20 Phosphorus-containing flue gas components V%

[0096]

[0097] The dephosphorized smelting slag was subjected to a molten iron reduction treatment, limestone was added to adjust the CaO / SiO2 to 1.0, anthracite was used as the reducing agent, and the C / Fe molar ratio after the addition of anthracite was 2.5, and the temperature in the electric furnace was controlled to be 1500°C. The composition of the iron-extracting lithium-containing tailings is shown in Table 21, and the composition of the reduced molten iron is shown in Table 22.

[0098] Table 21 Composition of tailings from deep iron extraction furnace by weight

[0099]

[0100] Table 22 Reduced iron molten iron composition wt%

[0101]

[0102] After conversion of the above data, it was found that the iron yield was 94%.

[0103] Example 6

[0104] A method for comprehensive recovery of P, Fe and Li from black powder of lithium iron phosphate battery, such as Figure 2 As shown, it includes: recovering phosphorus and iron resources from the ferrophosphorus slag after lithium extraction from the black powder of lithium iron phosphate batteries, obtaining P2O5 smoke by selective reduction and volatilization of phosphorus through a side-blown furnace, and obtaining pig iron products by deep reduction in an electric furnace.

[0105] Specifically, the composition of the ferrophosphorus slag after lithium extraction from the black powder of the lithium iron phosphate battery is shown in Table 6. Based on 100 parts by mass of the ferrophosphorus slag, quartz is added to the side-blown furnace to control the Fe / SiO2 at 1.35, anthracite is added to make the C / P molar ratio 2.2, and 20Nm of natural gas is introduced. 3 / h and oxygen-enriched air 44Nm 3 / h provides heat energy to make the smelting temperature reach 1300℃, wherein the oxygen concentration in the side-blown furnace is 70% to control the combustion coefficient of the injected fuel between 0.6 and 0.85; the dephosphorized smelting slag produced is shown in Table 23, and the composition of the phosphorus-containing flue gas is shown in Table 24. After condensation of the phosphorus-containing flue gas, dilute phosphoric acid with a concentration of 85% is obtained, and the converted P2O5 yield is 96%.

[0106] Table 23 Side-blowing dephosphorization molten slag composition wt%

[0107]

[0108] Table 24 Phosphorus-containing flue gas components V%

[0109]

[0110] The dephosphorized smelting slag was subjected to a molten iron reduction treatment, limestone was added to adjust the CaO / SiO2 to 1.0, anthracite was used as the reducing agent, and the C / Fe molar ratio after the addition of anthracite was 2, and the temperature in the electric furnace was controlled to be 1400°C. The composition of the iron-extracting lithium-containing tailings is shown in Table 25, and the composition of the reduced molten iron is shown in Table 26.

[0111] Table 25 Composition of tailings from deep iron extraction furnace by weight%

[0112]

[0113] Table 26 Reduced iron molten iron composition wt%

[0114]

[0115] After conversion of the above data, it was found that the iron yield was 88%.

[0116] Example 7

[0117] A method for comprehensive recovery of P, Fe and Li from black powder of lithium iron phosphate battery, such as Figure 3 As shown, a side-blowing reduction integrated furnace is used to complete the comprehensive recovery of phosphorus, iron and lithium. Specifically:

[0118] like Figure 3 As shown, the side-blowing smelting area 1 is used to complete the volatilization of phosphorus and adjust the slag type to iron silicon slag. Specifically, anthracite and quartz are added through the side-blowing feeding port 4, and the fuel and lithium iron phosphate battery black powder are sprayed into the side-blowing smelting area 1 through the fuel spray gun and the loading spray gun 5 in the side-blowing area. The mass ratio of Fe / SiO2 and the C / P molar ratio are controlled to be the same as those in Example 1. The lithium iron phosphate battery black powder is smelted under the same smelting conditions as in Example 1. During the smelting process, phosphorus is reduced and gasified and enters the side-blowing flue 3 with the smoke. Secondary combustion is performed based on the secondary combustion nozzle 2 of the side-blowing flue, and phosphorus-containing flue gas, the side-blowing furnace bottom base 7 and the dephosphorization smelting slag at the position where the liquid level line 6 is reached are effectively obtained. The composition of the phosphorus-containing flue gas is shown in Table 27, and the composition of the dephosphorization smelting slag is shown in Table 28. After condensation, the phosphorus-containing flue gas is condensed to obtain dilute phosphoric acid with a concentration of 76%, and the converted P2O5 yield is 88%.

[0119] Table 27 Phosphorus-containing flue gas components V%

[0120]

[0121] Table 28 Side-blowing dephosphorization smelting slag composition wt%

[0122]

[0123] Anthracite and limestone are added to the dephosphorized smelting slag through the side-blowing feed port 4 to adjust the CaO / SiO2 mass ratio and C / Fe molar ratio to the same as in Example 1 to obtain iron silicon slag, which flows into the electric furnace reduction zone through the side-blowing area and the electric thermal reduction area connecting channel 13, and the iron silicon slag is heated by the electrode 10 to ensure that the temperature of the iron silicon slag remains exactly the same as in Example 1, completing the reduction of iron, and finally discharging the molten iron in the electric thermal reduction zone iron liquid layer 8 through the molten iron discharge port 12, and discharging the slag in the electric thermal zone slag layer 9 through the slag discharge port 11. The composition of the iron-extracting lithium-containing tailings produced is shown in Table 29, and the composition of the reduced molten iron is shown in Table 30.

[0124] Table 29 wt% of lithium-containing tailings after deep reduction and iron extraction in electric furnace

[0125]

[0126] Table 30 Reduced iron molten composition wt%

[0127]

[0128] After conversion of the test data, it was found that the iron yield was 93%.

[0129] The lithium-containing tailings after iron extraction are subjected to conventional hydrometallurgical extraction of lithium, and the specific hydrometallurgical extraction process of lithium is the same as that of Example 1. The lithium carbonate content in the lithium carbonate product of the present invention is 95%-97%, and the recovery rate of lithium is 85%-90%.

[0130] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for comprehensive recovery of P, Fe and Li from lithium iron phosphate battery black powder, comprising the steps of recovering lithium, phosphorus and iron from the raw materials; characterized in that: When the raw material is lithium iron phosphate battery black powder, the steps of phosphorus recovery, iron recovery and lithium recovery are performed in sequence; when the raw material is phosphorus iron slag obtained by wet lithium extraction from lithium iron phosphate battery black powder, the steps of phosphorus recovery and iron recovery are performed in sequence; In the phosphorus recovery step: the Fe / SiO2 mass ratio in the raw material is controlled to be 0.5-1.6 by adding quartz stone, and side-blowing melt selective reduction volatilization phosphorus refining is carried out at 1300-1500°C to obtain yellow phosphorus or P2O5; in the process of side-blowing melt selective reduction volatilization phosphorus refining, the C / P molar ratio is (0.5-3):1, and the combustion coefficient of the injection fuel is controlled to be 0.6-0.85; In the iron recovery step: limestone is added to the smelting slag after phosphorus recovery to control the CaO / SiO2 mass ratio to 0.5-1.2, and the temperature is controlled to 1400-1500° C. under reducing conditions to perform molten iron reduction to obtain molten iron and slag; In the lithium recovery step, the slag obtained from the iron recovery step is subjected to wet lithium extraction to recover lithium.

2. The method according to claim 1, characterized in that The temperature of the side blowing melting is 1350-1500°C.

3. The method according to claim 1, characterized in that The C / P molar ratio is (0.5~1):

1.

4. The method according to any one of claims 1 to 3, characterized in that: The injection fuel is one or more of natural gas, pulverized coal, anthracite, and heavy oil.

5. The method according to claim 1, characterized in that In the step of smelting iron reduction, an electric furnace or a side-blown furnace is used for smelting.

6. The method according to claim 5, characterized in that In the step of molten iron reduction, when smelting is performed in an electric furnace, the C / Fe molar ratio is (1-3):

1.

7. The method according to claim 6, characterized in that The C / Fe molar ratio is (1~2):

1.

8. The method according to claim 5, characterized in that In the step of molten iron reduction, when a side-blown furnace is used for smelting, pulverized coal injection is used to supply heat and achieve iron reduction, the pulverized coal combustion coefficient is 0.65-0.8, and oxygen-enriched air is injected to utilize excess pulverized coal to participate in iron reduction. After injecting oxygen-enriched air, the oxygen concentration is controlled to be 55%-80%.

Citation Information

Cited By

  • Method and system for recovering phosphorus and iron from ferrophosphorus solid waste

    CN122609779A