A high temperature, high humidity and high pressure resistant epoxy resin material and preparation method thereof
By optimizing the chemical structure of epoxy resin and selecting appropriate curing agents and modified fillers, the lack of performance of traditional epoxy resins in high temperature, high humidity and high pressure environments is solved, and high temperature, high humidity and high pressure performance is achieved. Improve and expand application scope.
Patent Information
- Application Number
- CN202411092059.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Traditional epoxy resin materials have insufficient performance in high temperature, high humidity and high pressure environments, which limits their wider application.
Using a high-temperature, high-humidity and high-pressure epoxy resin material, by optimizing the chemical structure of the epoxy resin, adding high-temperature functional groups, combined with AP104 polyurea resin and WK305 dicyandiamide curing agent, carbon fiber and silicon dioxide are used With silicone rubber/graphene composite materials as modified fillers, ultrasonic dispersion and vacuum defoaming are carried out to shorten the curing time and improve material performance.
It significantly improves the material's high temperature, humidity and pressure resistance, reduces shrinkage and water absorption, broadens the application range, and is simple in preparation technology, which is suitable for industrial production.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of epoxy resins, and in particular to a high temperature, high humidity and high pressure resistant epoxy resin material and a preparation method thereof. Background Art
[0002] Epoxy resin is an important thermosetting resin. Its molecular structure contains two or more epoxy groups, which can form a three-dimensional network solidified product in the presence of appropriate chemical agents. Since P. Castam applied for a Swiss patent in 1938, the development of epoxy resin has gone through several stages. In 1946, Ciba developed the earliest epoxy adhesive, and in 1949, SOCreentee in the United States developed epoxy coatings. my country began industrial production of epoxy resin in 1958, and since then, epoxy resin has been widely used and developed in China.
[0003] The main advantage of epoxy resin is that it has low application value when used alone, but when used in combination with a curing agent, it can form a material with excellent properties. This material has the characteristics of good corrosion resistance, wear resistance, temperature resistance, and weather resistance, and has a high-quality gloss and is easy to polish. Therefore, it is widely used in many fields such as aerospace, electronics, automobile manufacturing, and architectural decoration.
[0004] However, epoxy resin also has some disadvantages, such as easy discoloration, high flammability and easy shrinkage. In harsh environments such as high temperature, high humidity and high pressure, traditional epoxy resin materials often cannot meet performance requirements, limiting their wider application. Therefore, the present invention proposes a high temperature, high humidity and high pressure resistant epoxy resin material and a preparation method thereof. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a high temperature, high humidity and high pressure resistant epoxy resin material and a preparation method thereof.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprising the following raw materials in percentage by mass:
[0008] Epoxy resin mixture: 22-46%;
[0009] Composite curing agent: 3-5%;
[0010] Coupling agent: 0.01~2.00%;
[0011] Accelerator: 0.01~2.00%;
[0012] Modified filler: 45-74.98%;
[0013] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2-3.5:4-5.5:1;
[0014] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.5-3:5;
[0015] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.01-0.5:2.5-4.5:0.5.
[0016] Furthermore, the coupling agent is a silane coupling agent KH560, and the accelerator is a substituted urea accelerator of UR300.
[0017] Furthermore, the molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0018] Furthermore, the molecular weight of the E-51 epoxy resin is 5000-6000.
[0019] Furthermore, the epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0020] Furthermore, the silicone rubber / graphene composite material is formed by mixing silicone rubber in latex form and graphene in a ratio of 1-3:1.
[0021] Furthermore, the carbon fiber is T300 carbon fiber.
[0022] A method for preparing a high temperature, high humidity and high pressure resistant epoxy resin material comprises the following preparation steps:
[0023] Step 1: Mixing ingredients: mixing the epoxy resin mixture, composite curing agent, coupling agent and accelerator according to the above proportions, and performing ultrasonic dispersion and vacuum degassing treatment to obtain a matrix resin;
[0024] Step 2: Add the modified filler into the base resin, mix, grind and degas in sequence to obtain the high temperature, high humidity and high pressure resistant epoxy resin material.
[0025] The present invention has the following technical effects:
[0026] The invention proposes a high temperature, high humidity and high pressure resistant epoxy resin material. By optimizing the chemical structure of the epoxy resin and introducing functional groups with good stability in high temperature, corrosion and high humidity environments, the high temperature, high humidity and high pressure resistance of the material are improved. A curing agent with good compatibility with the epoxy resin matrix and high reaction activity is selected to shorten the curing time and improve the production efficiency. A high temperature resistant filler is added to further improve the high temperature, humidity and high pressure resistance of the material and broaden the application range of the material. The invention also has the characteristics of low shrinkage and low water absorption. The preparation process is simple, easy to operate and suitable for industrial production. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0028] The present embodiment provides a high temperature, high humidity and high pressure resistant epoxy resin material, wherein the epoxy resin material comprises the following raw materials in percentage by weight:
[0029] Epoxy resin mixture: 22-46%;
[0030] Composite curing agent: 3-5%;
[0031] Coupling agent: 0.01~2.00%;
[0032] Accelerator: 0.01~2.00%;
[0033] Modified filler: 45-74.98%;
[0034] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2-3.5:4-5.5:1;
[0035] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.5-3:5;
[0036] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.01-0.5:2.5-4.5:0.5.
[0037] The coupling agent in this embodiment is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0038] The molecular weight of the E-12 epoxy resin in this embodiment is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0039] The molecular weight of the E-51 epoxy resin in this embodiment is 5000-6000.
[0040] The epoxy equivalent of the E-44 epoxy resin in this example is 220-230 g / eq and the softening point is 15-20°C.
[0041] The silicone rubber / graphene composite material of this embodiment is prepared by mixing silicone rubber in latex form and graphene in a ratio of 1-3:1.
[0042] The carbon fiber in this embodiment is T300 carbon fiber.
[0043] The present invention provides a method for preparing a high temperature, high humidity and high pressure resistant epoxy resin material, comprising the following steps:
[0044] Step 1: Mixing ingredients: mixing the epoxy resin mixture, composite curing agent, coupling agent and accelerator according to the above proportions, and performing ultrasonic dispersion and vacuum degassing treatment to obtain a matrix resin;
[0045] Step 2: Add the modified filler into the base resin, mix, grind and degas in sequence to obtain the high temperature, high humidity and high pressure resistant epoxy resin material.
[0046] Embodiment 1: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprises the following raw materials in percentage by mass:
[0047] Epoxy resin mixture: 22%;
[0048] Composite curing agent: 3%;
[0049] Coupling agent: 0.01%;
[0050] Accelerator: 0.01%;
[0051] Modified filler: 74.98%;
[0052] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2:4:1;
[0053] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.5:5;
[0054] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.01:2.5:0.5.
[0055] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0056] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0057] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0058] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0059] The silicone rubber / graphene composite material is formed by mixing silicone rubber in latex form and graphene in a ratio of 1:1.
[0060] The carbon fiber is T300 carbon fiber.
[0061] Embodiment 2: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprises the following raw materials in percentage by mass:
[0062] Epoxy resin mixture: 34%;
[0063] Composite curing agent: 4%;
[0064] Coupling agent: 1.00%;
[0065] Accelerator: 1.00%;
[0066] Modified filler: 60%;
[0067] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2.8:4.8:1;
[0068] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.7:5;
[0069] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.25:3.5:0.5.
[0070] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0071] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0072] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0073] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0074] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 2:1.
[0075] The carbon fiber is T300 carbon fiber.
[0076] Embodiment 3: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprises the following raw materials in percentage by mass:
[0077] Epoxy resin mixture: 46%;
[0078] Composite curing agent: 5%;
[0079] Coupling agent: 2.00%;
[0080] Accelerator: 2.00%;
[0081] Modified filler: 45%;
[0082] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 3.5:5.5:1;
[0083] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 3:5;
[0084] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.5:4.5:0.5.
[0085] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0086] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0087] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0088] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0089] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 3:1.
[0090] The carbon fiber is T300 carbon fiber.
[0091] Embodiment 4: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprises the following raw materials in percentage by mass:
[0092] Epoxy resin mixture: 34%;
[0093] Composite curing agent: 4%;
[0094] Coupling agent: 1.00%;
[0095] Accelerator: 1.00%;
[0096] Modified filler: 60%;
[0097] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2:4:1;
[0098] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.7:5;
[0099] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.25:3.5:0.5.
[0100] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0101] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0102] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0103] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0104] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 2:1.
[0105] The carbon fiber is T300 carbon fiber.
[0106] Embodiment 5: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprises the following raw materials in percentage by mass:
[0107] Epoxy resin mixture: 34%;
[0108] Composite curing agent: 4%;
[0109] Coupling agent: 1.00%;
[0110] Accelerator: 1.00%;
[0111] Modified filler: 60%;
[0112] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2:4:1;
[0113] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.7:5;
[0114] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.5:4.5:0.5.
[0115] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0116] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0117] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0118] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0119] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 2:1.
[0120] The carbon fiber is T300 carbon fiber.
[0121] Comparative Example 1: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprises the following raw materials in percentage by mass:
[0122] Epoxy resin mixture: 34%;
[0123] Composite curing agent: 4%;
[0124] Coupling agent: 1.00%;
[0125] Accelerator: 1.00%;
[0126] Modified filler: 60%;
[0127] The epoxy resin mixture is composed of E-12 epoxy resin and E-44 epoxy resin in a weight ratio of 2.8:1;
[0128] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.7:5;
[0129] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.25:3.5:0.5.
[0130] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0131] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0132] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0133] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 2:1.
[0134] The carbon fiber is T300 carbon fiber.
[0135] Comparative Example 2: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprising the following raw materials in percentage by mass:
[0136] Epoxy resin mixture: 34%;
[0137] Composite curing agent: 4%;
[0138] Coupling agent: 1.00%;
[0139] Accelerator: 1.00%;
[0140] Modified filler: 60%;
[0141] The epoxy resin mixture is composed of E-12 epoxy resin and E-51 epoxy resin in a weight ratio of 2.8:4.8;
[0142] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.7:5;
[0143] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.25:3.5:0.5.
[0144] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0145] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0146] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0147] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 1-3:1.
[0148] The carbon fiber is T300 carbon fiber.
[0149] Comparative Example 3: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprising the following raw materials in percentage by mass:
[0150] Epoxy resin mixture: 34%;
[0151] Composite curing agent: 4%;
[0152] Coupling agent: 1.00%;
[0153] Accelerator: 1.00%;
[0154] Modified filler: 60%;
[0155] The epoxy resin mixture consists of E-12 epoxy resin;
[0156] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.7:5;
[0157] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.25:3.5:0.5.
[0158] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0159] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0160] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 2:1.
[0161] The carbon fiber is T300 carbon fiber.
[0162] Comparative Example 4: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprising the following raw materials in percentage by mass:
[0163] Epoxy resin mixture: 34%;
[0164] Composite curing agent: 4%;
[0165] Coupling agent: 1.00%;
[0166] Accelerator: 1.00%;
[0167] Modified filler: 60%;
[0168] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2.8:4.8:1;
[0169] The composite curing agent is WK305 dicyandiamide curing agent;
[0170] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.25:3.5:0.5.
[0171] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0172] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0173] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0174] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0175] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 2:1.
[0176] The carbon fiber is T300 carbon fiber.
[0177] Comparative Example 5: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprising the following raw materials in percentage by mass:
[0178] Epoxy resin mixture: 34%;
[0179] Composite curing agent: 4%;
[0180] Coupling agent: 1.00%;
[0181] Accelerator: 1.00%;
[0182] Modified filler: 60%;
[0183] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2.8:4.8:1;
[0184] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.7:5;
[0185] The modified filler is composed of carbon fiber and silicon dioxide in a weight ratio of 0.25:3.5.
[0186] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0187] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0188] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0189] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0190] The carbon fiber is T300 carbon fiber.
[0191] Comparative Example 6: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprising the following raw materials in percentage by mass:
[0192] Epoxy resin mixture: 34%;
[0193] Composite curing agent: 4%;
[0194] Coupling agent: 1.00%;
[0195] Accelerator: 1.00%;
[0196] Modified filler: 60%;
[0197] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2.8:4.8:1;
[0198] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.7:5;
[0199] The modified filler is silicon dioxide.
[0200] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0201] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0202] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0203] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0204] Comparative Example 7: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprising the following raw materials in percentage by mass:
[0205] Epoxy resin mixture: 34%;
[0206] Composite curing agent: 4%;
[0207] Coupling agent: 1.00%;
[0208] Accelerator: 1.00%;
[0209] Modified filler: 60%;
[0210] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2.8:4.8:1;
[0211] The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.7:5;
[0212] The modified filler is a silicone rubber / graphene composite material.
[0213] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0214] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0215] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0216] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0217] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 2:1.
[0218] Comparative Example 8: A high temperature, high humidity and high pressure resistant epoxy resin material, the epoxy resin material comprising the following raw materials in percentage by mass:
[0219] Epoxy resin mixture: 34%;
[0220] Composite curing agent: 4%;
[0221] Coupling agent: 1.00%;
[0222] Accelerator: 1.00%;
[0223] Modified filler: 60%;
[0224] The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2.8:4.8:1;
[0225] The composite curing agent is AP104 polyurea resin;
[0226] The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.25:3.5:0.5.
[0227] The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300.
[0228] The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s.
[0229] The molecular weight of the E-51 epoxy resin is 5000-6000.
[0230] The epoxy equivalent of the E-44 epoxy resin is 220-230 g / eq and the softening point is 15-20°C.
[0231] The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 2:1.
[0232] The carbon fiber is T300 carbon fiber.
[0233] Comparative experiment of the embodiment and the comparative example: An experiment of a high temperature, high humidity and high pressure resistant epoxy resin material. The component dosage (unit: gram) and test results of the epoxy resin material are shown in the following table:
[0234] Among them, E-12 epoxy resin: produced by Shenzhen Yoshida Chemical Co., Ltd.;
[0235] E-51 epoxy resin and E-44 epoxy resin: produced by Guangzhou Chenshi Chemical Co., Ltd.;
[0236] Silica: HL-300 fumed silica from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.
[0237] Silicone rubber: 107 room temperature vulcanized silicone rubber produced by Shenzhen Jipeng Silicon Fluoride Materials Co., Ltd. is selected;
[0238] Graphene: Nanographene produced by Jiangsu Changzhou Yaobang Friction Material Factory is used, with a thermal conductivity of 5300W / mK;
[0239] E-12 Epoxy Resin E-51 Epoxy Resin E-44 Epoxy Resin AP104 polyurea resin WK305 dicyandiamide curing agent Coupling agent KH560 UR300 substituted urea accelerator Carbon Fiber Silicon dioxide Silicone rubber / graphene composite material Example 1 200 400 100 31.82 63.64 0.32 0.32 7.93 1981.50 369.30 Example 2 280 480 100 35.48 65.70 25.29 25.29 89.27 1249.78 178.54 Example 3 350 550 100 40.76 67.95 43.48 43.48 88.93 800.40 88.93 Example 4 245.71 491.43 122.86 35.48 65.70 25.29 25.29 89.27 1249.78 178.54 Example 5 280 480 100 35.48 65.70 25.29 25.29 137.96 1241.66 137.96 Comparative Example 1 648.42 0 231.58 35.48 65.70 25.29 25.29 89.27 1249.78 178.54 Comparative Example 2 324.21 555.79 0 35.48 65.70 25.29 25.29 89.27 1249.78 178.54 Comparative Example 3 880 0 0 35.48 65.70 25.29 25.29 89.27 1249.78 178.54 Comparative Example 4 280 480 100 0 101.18 25.29 25.29 89.27 1249.78 178.54 Comparative Example 5 280 480 100 35.48 65.70 25.29 25.29 101.17 1416.42 0 Comparative Example 6 280 480 100 35.48 65.70 25.29 25.29 0 1517.59 0 Comparative Example 7 280 480 100 35.48 65.70 25.29 25.29 0 0 1517.59 Comparative Example 8 280 480 100 101.18 0 25.29 25.29 89.27 1249.78 178.54
[0240] The evaluation in this embodiment was carried out according to the following method:
[0241] (1) Curing performance test
[0242] Differential scanning calorimetry, heating rate 60℃ / min, constant temperature curing at 120℃, test curing time, unit min.
[0243] (2) Water absorption test
[0244] According to GB / T1034-2008 standard, the sample specimen with a size of 50mm*50mm*1mm after curing at 120℃ was boiled in boiling water for 2 hours to test the water absorption rate in %.
[0245] (3) Moisture and heat aging test
[0246] According to GB / T15905 standard, after the packaged functional samples are cured, they are placed in a damp heat aging test box at 85°C and 85%RH for 1000 hours, and a multimeter is used to test whether the functional samples are conductive;
[0247] (4) Shrinkage test
[0248] The density of the dissolved epoxy resin solution is measured as the density before curing. After sealing, wait for it to completely cure, and measure the density in the solid state as the density after curing. Then, the shrinkage rate is calculated based on the density before curing and the density after curing.
[0249] (5) Electrical performance test:
[0250] Taking the packaging of automobile high-voltage ignition coil as an example, after the packaging is completed at 120℃, it is post-cured at 120℃ for 6 hours, and then its high-voltage resistance is tested under 6000V high voltage to see its high-voltage resistance;
[0251] Curing speed / min Damp heat aging Water absorption / % Shrinkage / % Electrical performance test Example 1 58.6 pass 1.49 1.68 pass Example 2 53.5 pass 1.11 1.25 pass Example 3 55.8 pass 1.35 1.58 pass Example 4 56.9 pass 1.25 1.22 pass Example 5 55.4 pass 1.22 1.35 pass Comparative Example 1 57.8 Failed 1.15 1.95 Failed Comparative Example 2 57.4 pass 1.09 1.69 Failed Comparative Example 3 58.5 Failed 1.05 2.34 Failed Comparative Example 4 61.5 pass 1.45 1.29 pass Comparative Example 5 58.7 Failed 0.97 2.54 pass Comparative Example 6 57.8 Failed 1.33 2.88 pass Comparative Example 7 55.8 pass 1.41 2.28 pass Comparative Example 8 67.2 pass 1.01 1.34 pass
[0252] According to Examples 1 to 5 and Comparative Examples 1 to 8, it can be found that:
[0253] Curing speed: The curing speed is between 53.5 and 67.2 minutes. The difference between the embodiments and the comparative examples is not large, but it is worth noting that the curing speed of comparative example 8 is the longest, reaching 67.2 minutes. Since the curing agent in comparative example 8 is only AP104 polyurea resin, the curing time of comparative example 4 is 61.5 minutes, and the curing efficiency is also low; AP104 polyurea resin itself has the characteristics of rapid curing under low temperature or room temperature environment, and WK305 dicyandiamide curing agent is an efficient curing accelerator that can significantly increase the curing reaction speed. Therefore, the curing agent obtained by compounding the two has a faster curing speed, can complete the curing process in a shorter time, and improve production efficiency. The coating film made of AP104 polyurea resin has fullness, leveling performance and gloss, as well as excellent physical and chemical properties. After compounding with WK305 dicyandiamide curing agent, these advantages are retained, and may be further improved due to the optimization of the curing reaction. The cured epoxy resin material has excellent properties such as high strength, high hardness, wear resistance, and corrosion resistance.
[0254] Hygrothermal aging: Most of the embodiments and comparative examples passed the hygrothermal aging test, but several comparative examples (Comparative Example 1, Comparative Example 3 and Comparative Example 5) failed the test. The epoxy resin mixtures in Comparative Example 1 and Comparative Example 3 consist of one or two components. In a humid and hot environment, the epoxy resin easily absorbs water and swells, resulting in uneven expansion between the inside and outside of the material, thereby generating internal stress. In addition, the humid and hot environment will accelerate the oxidation and degradation process of the epoxy resin, further reducing its performance. By compounding different brands of epoxy resins, the polarity, crosslinking density, molecular chain structure and other factors of the material can be adjusted, thereby improving its hygrothermal aging performance. This application uses E- The three epoxy resins, E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin, have a synergistic effect when combined. Since both E-12 and E-51 have good chemical and heat resistance, the composite epoxy resin can resist chemical corrosion and thermal aging in a hot and humid environment and maintain good performance stability. The high temperature tolerance of E-51 enables the composite epoxy resin to maintain stable performance at higher temperatures, which is particularly important for applications that need to work in a high temperature and hot and humid environment. The toughness of E-44 enables the composite epoxy resin to resist external impact and deformation in a hot and humid environment and maintain the integrity and stability of the material. This is very important for applications that need to withstand certain mechanical stresses.
[0255] Water absorption rate: the water absorption rate is between 0.97% and 1.49%. The water absorption rate of most embodiments is relatively low, among which the water absorption rate of embodiment 1 is the highest, reaching 1.49%, and the water absorption rate of comparative example 5 is the lowest. It can be seen from the data of the embodiments and comparative examples that the less the carbon fiber content, the higher the water absorption rate is relatively, and the water absorption rate of the epoxy resin material containing AP104 polyurea resin is relatively low. This is because the carbon fiber can improve the strength of the epoxy resin matrix and reduce water absorption. The water absorption of AP104 polyurea resin is relatively low. It is a high-performance polymer material with a compact molecular structure and good waterproof performance. It is not easy to absorb water and swell in water or a humid environment, and can maintain good dimensional stability and physical properties.
[0256] Shrinkage: The shrinkage is between 1.22% and 2.88%, with a large difference. The shrinkage of the examples is generally low, while the shrinkage of the comparative examples is high, especially comparative examples 3, 5, 6 and 7, all of which have shrinkages exceeding 2%. It can be seen from comparative examples 5-7 that the modified filler of the present application has a low shrinkage, and reducing one filler will greatly increase the shrinkage of the epoxy resin material.
[0257] Electrical performance test: Most of the embodiments and comparative examples passed the electrical performance test, but several comparative examples (Comparative Example 1, Comparative Example 2 and Comparative Example 3) failed to pass the test. The epoxy resin material of the present application has the characteristic of high voltage resistance.
[0258] The invention proposes a high temperature, high humidity and high pressure resistant epoxy resin material. By optimizing the chemical structure of the epoxy resin and introducing functional groups with good stability in high temperature, corrosion and high humidity environments, the high temperature, high humidity and high pressure resistance of the material are improved. A curing agent with good compatibility with the epoxy resin matrix and high reaction activity is selected to shorten the curing time and improve the production efficiency. A high temperature resistant filler is added to further improve the high temperature, humidity and high pressure resistance of the material and broaden the application range of the material. The invention also has the characteristics of low shrinkage and low water absorption. The preparation process is simple, easy to operate and suitable for industrial production.
[0259] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A high temperature, high humidity and high pressure resistant epoxy resin material, characterized in that: The epoxy resin material includes the following raw materials in percentage by mass: Epoxy resin mixture: 22-46%; Composite curing agent: 3-5%; Coupling agent: 0.01~2.00%; Accelerator: 0.01~2.00%; Modified filler: 45-74.98%; The epoxy resin mixture is composed of E-12 epoxy resin, E-51 epoxy resin and E-44 epoxy resin in a weight ratio of 2-3.5:4-5.5:1; The composite curing agent is composed of AP104 polyurea resin and WK305 dicyandiamide curing agent in a weight ratio of 2.5-3:5; The modified filler is composed of carbon fiber, silicon dioxide and silicone rubber / graphene composite material in a weight ratio of 0.01-0.5:2.5-4.5:0.5; The coupling agent is silane coupling agent KH560, and the accelerator is substituted urea accelerator UR300; The molecular weight of the E-12 epoxy resin is 1500-2000, and the viscosity of the E-12 epoxy resin is 3000-4000 mPa·s; The molecular weight of the E-51 epoxy resin is 5000-6000; The E-44 epoxy resin has an epoxy equivalent of 220-230 g / eq and a softening point of 15-20° C. The silicone rubber / graphene composite material is prepared by mixing silicone rubber in latex form and graphene in a ratio of 1-3:
1.
2. The high temperature, high humidity and high pressure resistant epoxy resin material according to claim 1, characterized in that: The carbon fiber is T300 carbon fiber.
3. A method for preparing a high temperature, high humidity and high pressure resistant epoxy resin material as claimed in any one of claims 1 to 2, characterized in that: The method comprises the following preparation steps: Step 1: Mixing ingredients: mixing the epoxy resin mixture, composite curing agent, coupling agent and accelerator according to the above proportions, and performing ultrasonic dispersion and vacuum degassing treatment to obtain a matrix resin; Step 2: Add the modified filler into the base resin, mix, grind and degas in sequence to obtain the high temperature, high humidity and high pressure resistant epoxy resin material.