A super flat seam beautifying agent and its flat seam construction process
By adding poly(sebacic 4,6-diynedioic acid) and formamide to graft low-density polyethylene into the epoxy resin caulking agent, a double-layer structure is formed, which solves the problem of the epoxy resin caulking agent in flat joint construction. The problem of strong adhesion is achieved, the effect of smooth surface and high adhesion strength is achieved, and the process flow is simplified.
Patent Information
- Application Number
- CN202411109796.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Due to the strong adhesion of epoxy resin caulking agent during flat joint construction, it is difficult for the scraper to form a smooth and flat cutting surface, resulting in high surface roughness, which increases the difficulty of cleaning and affects the bonding strength.
A combination of component A and component B is used. Component A includes epoxy resin, phenolic resin and functional additives. Component B includes poly(decane4,6-diynedioic acid) and formamide grafted low density. Polyethylene, through the action of light and oxygen, forms a double-layer structure of the caulking agent, which reduces the adhesion of the scraper and accelerates curing.
It achieves smooth leveling of the surface of the caulking agent by the scraper, reduces the need for polishing, improves the adhesion strength and curing speed, and enhances the oxygen and water barrier properties.
Smart Images

Figure CN118638500B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a seam beautifying agent, in particular to an ultra-flat seam beautifying agent and a flat seam construction process thereof. Background Art
[0002] Epoxy resin caulking agent is a caulking material made of epoxy resin and other materials. It was originally designed to fill the gaps on the surface of artificial stone. It has excellent chemical and physical properties, such as easy curing, strong adhesion, good chemical stability and mildew resistance. It is now widely used in decoration fields such as floor tiles and ceramic tiles.
[0003] Due to its strong adhesion, during the flat seam construction process, when the caulking agent is flattened with a scraper or other tool, there is a strong adhesion between the caulking agent and the scraper or other tool, which makes it impossible for the scraper to form a smooth and flat cutting surface during use, resulting in a high roughness of the caulking agent surface on the surface of the gap. In a flat position such as the ground that is stepped on or stacked with objects for a long time, the caulking agent with a high surface roughness is prone to adhere to a large amount of dust and other pollutants, which not only reduces the service life of the caulking agent but also increases the difficulty of cleaning the gap. Therefore, in the prior art, after the caulking agent is cured and dried, it is also necessary to use a polishing machine to grind the caulking agent to reduce the roughness of the caulking agent surface. However, after using the polishing machine, the caulking agent will be subjected to a certain degree of vibration during the polishing process, which not only reduces the bonding strength between the caulking agent and the side wall of the gap, but also affects the structural integrity of the caulking agent after drying and curing. Summary of the invention
[0004] The present invention provides an ultra-flat seam filler and a flat seam construction process thereof, which solves the problem that, when epoxy resin seam fillers are used to fill seams at flat locations such as the ground, the scraper cannot form a smooth and flat cutting surface during the leveling process of the seam filler due to the strong adhesion between the epoxy resin and tools such as scrapers, resulting in high roughness on the surface of the seam filler.
[0005] The present invention is achieved through the following technical solutions:
[0006] An ultra-flat seam beautifying agent, comprising component A and component B, wherein the mass ratio of component A to component B is 4:1;
[0007] The component A comprises the following components: epoxy resin, phenolic resin, pigment, filler, and other functional additives, wherein the mass ratio of epoxy resin to phenolic resin is 2:1, based on the total resin mass of epoxy resin and phenolic resin in component A, and the other functional additives comprise the following components in mass proportion: 8-10% of C12-14 alkyl glycidyl ether, 1-2% of acrylate leveling agent, and 1-2% of 2-pyridinethiol-1-zinc oxide;
[0008] The component B comprises the following components: poly(4,6-decanediyne dioic acid) and formamide grafted low-density polyethylene, wherein the mass ratio of poly(4,6-decanediyne dioic acid) and formamide grafted low-density polyethylene is 1.2-1.4:1;
[0009] Based on component A and component B, the super flat seam agent has the following two states:
[0010] When the super-flat seam-beautifying agent is in a light-proof and sealed environment, the super-flat seam-beautifying agent is a uniform slurry prepared by mixing component A and component B;
[0011] When the ultra-flat caulking agent is exposed to oxygen and light, the ultra-flat caulking agent changes from a uniform slurry state to an upper and lower double-layer structure, wherein the double-layer structure includes an upper colloid layer and a lower slurry layer; the poly(decane-4,6-diynedioic acid) in component B decomposes under oxygen and light conditions to produce succinic acid, and under the acidic conditions of succinic acid production, the formamide in the formamide-grafted low-density polyethylene in component B undergoes hydrolysis and debranching to produce ammonia water, formic acid and low-density polyethylene, and the caulking agent in the gap is stratified, with the upper layer being the upper colloid layer and the lower layer being the lower slurry layer; the upper colloid layer includes low-density polyethylene and ammonia water, and the mass of the ammonia water accounts for 0.8%-1% of the total mass of the upper colloid layer; the lower slurry layer includes component A, ammonia water, formic acid and succinic acid.
[0012] The present invention uses epoxy resin as a main component, adds poly (decane 4,6-diyne dioic acid) and formamide grafted low-density polyethylene, reduces the adhesion of the contact layer between the caulking agent and tools such as scrapers, and can form a smooth and low-roughness caulking agent surface when the caulking agent is leveled by tools such as scrapers, without the need for polishing, thereby simplifying the flat seam process; the component B composed of poly (decane 4,6-diyne dioic acid) and formamide grafted low-density polyethylene can be uniformly and stably mixed with the component A before the caulking agent is exposed to the air, thereby obtaining a mixture with strong adhesion to the side wall of the gap and good fluidity compound (slurry); in addition, when the seam beautifying agent of the present invention is exposed to the air for a period of time, the poly (decane 4,6-diynedioic acid) decomposes and the formamide-grafted low-density polyethylene is debranched and hydrolyzed. The above process not only does not affect the adhesion and adhesion strength between component A and the side wall of the gap, but the debranching and hydrolysis products of the formamide-grafted low-density polyethylene also increase the curing speed of the epoxy resin and the phenolic resin; the low-density polyethylene film formed on the surface of the seam beautifying agent after curing increases the overall oxygen and water barrier properties of the seam beautifying agent by virtue of its own high barrier properties, and has a protective effect on the underlying structure.
[0013] The reaction mechanism of the present invention is:
[0014] Polarity modification of formamide-grafted low-density polyethylene: Low-density polyethylene is a non-polar polymer material, which not only has very low adhesion to other substances, but is also completely incompatible with epoxy resin and phenolic resin, and cannot form a uniform mixture. Therefore, the present invention uses formamide to modify low-density polyethylene, thereby improving the polarity of low-density polyethylene. The modified formamide-grafted low-density polyethylene can be uniformly mixed with all components in component A to prepare a uniform and stable seam-beautifying agent slurry. The uniform and stable seam-beautifying agent slurry without sedimentation can uniformly fill the gaps;
[0015] Poly(4,6-decanediylene glycol) is used as a catalyst for the debranching and hydrolysis of formamide-grafted low-density polyethylene in natural environments. The catalytic principle is as follows: Poly(4,6-decanediylene glycol) is called PDDA, which is an environmentally self-degradable conjugated polymer. In a dark or anaerobic environment, PDDA remains stable. When PDDA is exposed to sunlight and air, the ultraviolet rays in the sunlight react with the conjugated double bonds and triple bonds in the PDDA molecules through a photooxidation mechanism, resulting in the breakage and decomposition of the PDDA polymer chain, producing succinic acid. Succinic acid has two carboxyl functional groups. The succinic acid has a hydrogen bond with the formamide group, which makes it highly reactive. When succinic acid contacts the formamide-grafted low-density polyethylene, the carboxyl group of succinic acid forms a hydrogen bond with the formamide group and undergoes an esterification reaction. These interactions cause the connection between the formamide group and the polyethylene main chain to become unstable, resulting in debranching, which causes the formamide to separate from the low-density polyethylene main chain. The separated formamide is hydrolyzed under acidic conditions to obtain formic acid and ammonia. Part of the ammonia dissolves in water to form ammonia water, part of the ammonia directly volatilizes, part of the ammonia water is mixed with the low-density polyethylene, and part of the ammonia water is mixed with component A.
[0016] The chemical properties of low-density polyethylene are stable. There is no chemical reaction between succinic acid, formic acid and low-density polyethylene in the natural environment. However, the carboxyl groups in succinic acid and formic acid will combine with the epoxy groups of epoxy resin to form ester bonds. Ester bonds are carbon-oxygen covalent bonds formed by the reaction of carboxylic acid and alcohol. Its structure can be expressed as R-COOR', where R and R' represent organic groups. In this structure, the carbonyl carbon atom in the carboxylic acid group is covalently bonded to the oxygen atom in the alcohol group. This specific connection method makes the oxygen atom in the ester bond have a certain negative charge, while the carbon atom has a certain positive charge; this positive and negative charge distribution is uneven. In addition, since the oxygen atom in the ester bond has a high electronegativity and a strong ability to attract electrons, this further enhances the polarity of the ester bond. That is, the ester bond has a large polarity, which makes the ester bond easy to break and participate in a variety of important chemical reactions. Then, the formation of the ester bond enhances the polarity of the entire component A system, and the adhesion of the component A system is significantly enhanced.
[0017] Based on the chemical bonds between succinic acid, formic acid and epoxy resin, succinic acid and formic acid will separate from the low-density polyethylene and enter component A.
[0018] Part of the ammonia water that enters component A reacts with succinic acid to neutralize it. Heat is released during the reaction, which increases the temperature of the caulking agent. The increase in the temperature of the caulking agent will accelerate the evaporation rate of water in the caulking agent, thereby accelerating the curing speed of the caulking agent. In addition, formic acid and succinic acid will reduce the pH value of component A. During the curing process, the phenol and aldehyde groups in the phenolic resin undergo condensation reactions to generate a cross-linked structure, causing the resin to transform from a liquid or semi-solid state to a solid state. Under acidic conditions, the reaction rate and degree of cross-linking in the phenolic resin will increase, thereby accelerating the curing process.
[0019] The low-density polyethylene obtained after the formamide grafted low-density polyethylene is debranched has a low density, which is lower than the density of epoxy resin, phenolic resin and filler. In addition, low-density polyethylene is a non-polar polymer material, and is completely incompatible with epoxy resin, phenolic resin, seasoning and other substances. As a result, low-density polyethylene and component A are stratified, and the seam beautifier contains a two-layer structure. The upper layer is a mixture of low-density polyethylene and ammonia water. During the curing process, as the ammonia water evaporates, the thickness of the upper layer structure will decrease after curing; the epoxy resin in the lower layer component expands significantly during the curing process. This is because the curing reaction of epoxy resin is usually a condensation reaction, which will produce A large amount of heat is generated and the gases of the reaction products are released. These gases remain in the reaction system, causing the gas volume to gradually increase, thereby causing the solidification volume to expand; in the present invention, due to the volatilization of ammonia in the upper colloid layer, the upper layer components shrink during the solidification process; the lower slurry layer expands due to the epoxy resin solidification, causing the lower layer components to expand during the solidification process; the present invention defines the mass ratio of poly (decane 4,6-diyne dioic acid) and formamide grafted low-density polyethylene and the ratio of epoxy resin to phenolic resin, so that the upper layer solidification shrinkage of the present invention is complementary to the lower layer solidification expansion, so that the difference between the top surface of the caulking agent and the top surface of the two side walls of the gap is within ±0.01mm. If the amount of epoxy resin added is too large, the expansion degree of the lower layer of the caulking agent during the solidification process is too large, and the upper layer solidification shrinkage cannot make up for the expansion of the epoxy resin, and finally the thickness of the caulking agent after solidification is greater than the depth of the gap.
[0020] Principle of reduced adhesion with tools such as scrapers: in the present invention, after the caulking agent is exposed to the air and stratified, the upper colloid layer is mainly low-density polyethylene, and low-density polyethylene is a non-polar polymer. Its adhesion with tools such as scrapers is very low. When the caulking agent is leveled with tools such as scrapers, what is scraped away by the scrapers is the low-density polyethylene layer of the caulking agent, and the surface layer after scraping is still the low-density polyethylene layer. The surface layer of the caulking agent after scraping is the cured low-density polyethylene film, and the surface of the cured low-density polyethylene film is smooth and flat. Compared with the surface layer of the existing caulking agent after scraping and curing, the roughness of the cured low-density polyethylene film is significantly reduced, which meets the use requirements of the caulking agent and does not require subsequent polishing.
[0021] The mass ratio of poly(decane-4,6-diynedioic acid) and formamide-grafted low-density polyethylene in the present invention affects the debranching and hydrolysis effects of the formamide-grafted low-density polyethylene; if the amount of poly(decane-4,6-diynedioic acid) added is too much, excessive succinic acid is produced, resulting in excessive acidity in component A, which will have a significant corrosive effect on the filler and affect the strength of the seam beautifier; if the amount of poly(decane-4,6-diynedioic acid) added is too little, the amount of succinic acid produced is too little, the debranching degree of the formamide-grafted low-density polyethylene is very low, and the low-density polyethylene layer cannot be produced, resulting in the inability to separate the seam beautifier into layers.
[0022] Furthermore, the mass ratio of poly(decane-4,6-diynedioic acid) to formamide-grafted low-density polyethylene in the component B is 1.3:1.
[0023] Furthermore, the filler comprises the following components in parts by weight: 50-60 parts of 30-40 μm perlite powder, 10-20 parts of 0.1-0.3 μm silica powder, and 5-8 parts of 100-120 μm white silicate cement clinker; the mass of the filler accounts for 35-40% of the total resin mass of the epoxy resin and phenolic resin in component A.
[0024] The present invention optimizes the components of the filler. Under the condition of ensuring that the overall mechanical strength of the seam beautifying agent is high, each filler component has good acid and alkali corrosion resistance, especially acid resistance, so that the filler is less affected by formic acid and succinic acid. Based on the close packing theory, the present invention optimizes the gradation of each component, so that component A forms a dense structure after curing, further improving the strength of the structure of the seam beautifying agent after curing.
[0025] Furthermore, the filler comprises the following components in parts by weight: 60 parts of 30-40 μm perlite powder, 20 parts of 0.1-0.3 μm silica powder, and 8 parts of 100-120 μm white silicate cement clinker; the mass of the filler accounts for 35% of the total resin mass of the epoxy resin and phenolic resin in component A.
[0026] Furthermore, based on the total resin mass of the epoxy resin and the phenolic resin in component A, the other functional additives include the following components in proportion by mass: 8-10% of C12-14 alkyl glycidyl ether, 1-2% of acrylate leveling agent, and 1-2% of 2-pyridinethiol-1-zinc oxide.
[0027] C12-14 alkyl glycidyl ether is a diluent, and 2-pyridinethiol-1-zinc oxide is a mildew preventer; C12-14 alkyl glycidyl ether appropriately reduces the consistency of C12-14 alkyl glycidyl ether, ensuring that component A has good fluidity and can be evenly filled in the gap.
[0028] Furthermore, the ultra-flat seam beautifying agent is prepared by the following method:
[0029] S1. Preparation of component A:
[0030] S1.1, melting the epoxy resin at a temperature of 180°C to obtain an epoxy resin glue solution;
[0031] S1.2, melting the phenolic resin at a temperature of 105°C to obtain a phenolic resin glue solution;
[0032] S1.2, after mixing the epoxy resin glue and the phenolic resin glue, cool down to 100°C, stir at 100°C for 10-20 minutes until they are evenly mixed, cool down to 80°C again after evenly mixing, add other functional additives at 80°C and continue to stir until they are evenly mixed to obtain a diluted mixed glue;
[0033] S1.3, evenly mix the solid components in the filler, then cool the mixed glue to 50-60°C, slowly add the filler to the mixed glue at 50-60°C while stirring at a speed of 280-300 rpm, continue stirring for 1-2 hours, then add the pigment and mix evenly to obtain component A;
[0034] S2, preparing component B: using formamide monomer to graft-modify low-density polyethylene to obtain formamide-grafted low-density polyethylene, then mixing the formamide-grafted low-density polyethylene with poly (decane-4,6-diynedioic acid) and adding them into an anaerobic stirring tank, and uniformly mixing at 30° C. for 30-40 minutes to obtain component B;
[0035] S3. In an anaerobic stirring tank, component A and component B are mixed to obtain a caulking agent slurry, and the caulking agent slurry is then transferred to a vacuum sealed container for standby use.
[0036] Furthermore, the formamide-grafted low-density polyethylene is prepared by the following method:
[0037] a. Low-density polyethylene with a density of 0.91 g / cm³ is used as the base polymer and formamide is used as the grafting monomer;
[0038] b. exposing the low-density polyethylene to a radiation source, wherein the radiation source is ultraviolet light, electron beam or gamma ray, and the radiation treatment is performed for 30-40 seconds;
[0039] c. After the radiation treatment of the low-density polyethylene is completed, formamide is added immediately and stirred for 20-30 minutes to carry out a grafting reaction to obtain formamide-grafted low-density polyethylene. The mass ratio of formamide to low-density polyethylene is 1:20.
[0040] The flat seam construction process based on the ultra-flat seam beautifying agent comprises the following steps:
[0041] A. Clean the gap: Use a slotter or utility knife to clean the filler in the gap, and ensure that there is no sand, dust or water in the gap. The gap is the gap on the horizontal surface;
[0042] B. Paste masking tape: Paste masking tape on both sides of the gap;
[0043] C. Preparing a seam beautifying agent: preparing component A and component B respectively, wherein component B is prepared in an anaerobic environment, and then mixing component A and component B in an anaerobic environment to prepare a seam beautifying agent slurry, and placing the seam beautifying agent slurry in a vacuum sealed container for standby use;
[0044] D. Gluing: Pour the caulking agent into the glue gun and start gluing. The caulking agent is evenly filled in the gap, and the filling thickness of the caulking agent is greater than the depth of the gap. After the caulking agent is filled in the gap, the poly (decane-4,6-diynedioic acid) in the caulking agent component B is exposed to the air, decomposes under oxygen and light conditions, and produces succinic acid; under the acidic conditions of succinic acid production, the formamide in the formamide-grafted low-density polyethylene undergoes hydrolysis and debranching, producing ammonia water, formic acid and low-density polyethylene, and the caulking agent in the gap is stratified, with the upper layer being the upper colloid layer, which includes low-density polyethylene and ammonia water, and the lower slurry layer including ammonia water, formic acid, succinic acid, and component A.
[0045] E. Pressing and leveling the seams: Use a scraper to scrape off the excess transparent glue layer on the top surface of the gap, so that the seam beautifier is flush with the surfaces on both sides of the gap;
[0046] F. Drying: After drying and curing for 12-14 hours, the caulking agent in the gap forms a solid double-layer structure. The upper structure is a transparent film after the upper colloid layer is cured, and the lower structure is a block-shaped solid after the lower slurry layer that matches the shape of the gap is cured, completing the flat seam construction.
[0047] Furthermore, the scraper in step E is a stainless steel plate.
[0048] Furthermore, after drying and curing in step F, the thickness of the upper colloid layer is 1 / 20 of the thickness of the lower block layer.
[0049] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0050] 1. The ultra-flat seam sealant of the present invention uses epoxy resin as the main component, adds poly (decane 4,6-diyne dioic acid) and formamide grafted low-density polyethylene, reduces the adhesion of the contact layer between the seam sealant and tools such as scrapers, and when the seam sealant is leveled by tools such as scrapers, a smooth, low-roughness seam sealant surface can be formed, without the need for polishing, thereby simplifying the flat seam process;
[0051] 2. In the ultra-flat seam beautifier of the present invention, when component A of the seam beautifier is exposed to the air for a period of time, poly(decane-4,6-diynediacid) decomposes and formamide-grafted low-density polyethylene is debranched and hydrolyzed. The above process not only does not affect the adhesion and adhesion strength between component A and the side wall of the gap, but the product of formamide-grafted low-density polyethylene also increases the curing speed of epoxy resin and phenolic resin;
[0052] 3. The low-density polyethylene film formed on the surface of the ultra-flat seam-beautifying agent after curing of the present invention increases the oxygen and water barrier properties of the entire seam-beautifying agent by virtue of its own high barrier properties, and has a protective effect on the underlying structure;
[0053] 4. The flat seam construction process of the present invention adopts an improved super-flat seam beautifying agent, which saves the polishing process and simplifies the process flow compared with the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:
[0055] Figure 1 It is a schematic diagram of the vertical cross-section structure of the ground gap after the seam beautification of the present invention;
[0056] Figure 2 This is a schematic diagram of the structure of the seam beautifying agent after curing of the present invention;
[0057] Figure 3 This is an infrared spectrum of the upper structure of the seam beautifying agent after stratification.
[0058] Marks and corresponding parts names in the attached drawings:
[0059] 1- ground layer, 2- low-density polyethylene membrane, 3- lower structure. DETAILED DESCRIPTION
[0060] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0061] Embodiment 1, an ultra-flat seam beautifying agent of the present invention, comprising component A and component B, wherein the mass ratio of component A to component B is 4:1;
[0062] The component A comprises the following components: epoxy resin, phenolic resin, pigment, filler, and other functional additives, wherein the mass ratio of epoxy resin to phenolic resin is 2:1, based on the total resin mass of epoxy resin and phenolic resin in component A, and the other functional additives comprise the following components in mass proportion: 8-10% of C12-14 alkyl glycidyl ether, 1-2% of acrylate leveling agent, and 1-2% of 2-pyridinethiol-1-zinc oxide;
[0063] The component B comprises the following components: poly(4,6-decanediyne dioic acid) and formamide grafted low-density polyethylene, wherein the mass ratio of poly(4,6-decanediyne dioic acid) and formamide grafted low-density polyethylene is 1.2-1.4:1;
[0064] Based on component A and component B, the super flat seam agent has the following two states:
[0065] When the super-flat seam-beautifying agent is in a light-proof and sealed environment, the super-flat seam-beautifying agent is a uniform slurry prepared by mixing component A and component B;
[0066] When the ultra-flat caulking agent is exposed to oxygen and light, the ultra-flat caulking agent changes from a uniform slurry state to an upper and lower double-layer structure, wherein the double-layer structure includes an upper colloid layer and a lower slurry layer; the poly(decane-4,6-diynedioic acid) in component B decomposes under oxygen and light conditions to produce succinic acid, and under the acidic conditions of succinic acid production, the formamide in the formamide-grafted low-density polyethylene in component B undergoes hydrolysis and debranching to produce ammonia water, formic acid and low-density polyethylene, and the caulking agent in the gap is stratified, with the upper layer being the upper colloid layer and the lower layer being the lower slurry layer; the upper colloid layer includes low-density polyethylene and ammonia water, and the mass of the ammonia water accounts for 0.8%-1% of the total mass of the upper colloid layer; the lower slurry layer includes component A, ammonia water, formic acid and succinic acid.
[0067] The filler comprises the following components in parts by weight: 60 parts of 30-40 μm perlite powder, 20 parts of 0.1-0.3 μm silica powder, and 8 parts of 100-120 μm white silicate cement clinker; the mass of the filler accounts for 35% of the total resin mass of the epoxy resin and the phenolic resin in component A.
[0068] Based on the total resin mass of the epoxy resin and the phenolic resin in component A, the other functional additives include the following components in proportion by mass: 9% of C12-14 alkyl glycidyl ether, 1.5% of acrylate leveling agent, and 1.5% of 2-pyridinethiol-1-zinc oxide.
[0069] The ultra-flat seam beautifying agent of this embodiment is prepared by the following method:
[0070] S1. Preparation of component A:
[0071] S1.1, melting the epoxy resin at a temperature of 180°C to obtain an epoxy resin glue solution;
[0072] S1.2, melting the phenolic resin at a temperature of 105°C to obtain a phenolic resin glue solution;
[0073] S1.2, after mixing the epoxy resin glue and the phenolic resin glue, cool down to 100°C, stir at 100°C for 10-20 minutes until they are evenly mixed, cool down to 80°C again after evenly mixing, add other functional additives at 80°C and continue to stir until they are evenly mixed to obtain a diluted mixed glue;
[0074] S1.3, evenly mix the solid components in the filler, then cool the mixed glue to 50-60°C, slowly add the filler to the mixed glue at 50-60°C while stirring at a speed of 280-300 rpm, continue stirring for 1-2 hours, then add the pigment and mix evenly to obtain component A;
[0075] S2, preparing component B: using formamide monomer to graft-modify low-density polyethylene to obtain formamide-grafted low-density polyethylene, then mixing the formamide-grafted low-density polyethylene with poly (decane-4,6-diynedioic acid) and adding them into an anaerobic stirring tank, and uniformly mixing at 30° C. for 30-40 minutes to obtain component B;
[0076] S3. In an anaerobic stirring tank, component A and component B are mixed to obtain a caulking agent slurry, and the caulking agent slurry is then transferred to a vacuum sealed container for standby use.
[0077] The formamide grafted low-density polyethylene described in this embodiment is prepared by the following method:
[0078] a. Low-density polyethylene with a density of 0.91 g / cm³ is used as the base polymer and formamide is used as the grafting monomer;
[0079] b. exposing the low-density polyethylene to a radiation source, wherein the radiation source is ultraviolet light, electron beam or gamma ray, and the radiation treatment is performed for 30-40 seconds;
[0080] c. After the radiation treatment of the low-density polyethylene is completed, formamide is added immediately and stirred for 20-30 minutes to carry out a grafting reaction to obtain formamide-grafted low-density polyethylene. The mass ratio of formamide to low-density polyethylene is 1:20.
[0081] The application of the seam beautifying agent in this embodiment is: based on the flat seam construction process of the above-mentioned super flat seam beautifying agent, the following steps are included:
[0082] A. Clean the gap: Use a slotter or utility knife to clean the filler in the gap, and ensure that there is no sand, dust or water in the gap. The gap is the gap on the horizontal surface;
[0083] B. Paste masking tape: Paste masking tape on both sides of the gap;
[0084] C. Preparing a seam beautifying agent: preparing component A and component B respectively, wherein component B is prepared in an anaerobic environment, and then mixing component A and component B in an anaerobic environment to prepare a seam beautifying agent slurry, and placing the seam beautifying agent slurry in a vacuum sealed container for standby use;
[0085] D. Gluing: Pour the caulking agent into the glue gun and start gluing. The caulking agent is evenly filled in the gap, and the filling thickness of the caulking agent is greater than the depth of the gap. After the caulking agent is filled in the gap, the poly (decane-4,6-diynedioic acid) in the caulking agent component B is exposed to the air, decomposes under oxygen and light conditions, and produces succinic acid. Under the acidic conditions of succinic acid production, the formamide in the formamide-grafted low-density polyethylene undergoes hydrolysis and debranching to produce ammonia water, formic acid and low-density polyethylene, and the caulking agent in the gap is layered, with the upper layer being the upper colloid layer, which includes low-density polyethylene and ammonia water, and the lower layer being the lower slurry layer, which includes ammonia water, formic acid, succinic acid, and component A.
[0086] E. Pressing and leveling the seams: Use a scraper to scrape off the excess transparent glue layer on the top surface of the gap, so that the seam beautifier is flush with the surfaces on both sides of the gap;
[0087] F. Drying: After drying and curing for 12-14 hours, the caulking agent in the gap forms a double-layer structure. The upper structure is a transparent film, and the lower structure is a block-shaped solid that matches the shape of the gap, completing the flat seam construction.
[0088] The scraper in step E is a stainless steel plate.
[0089] After drying and curing in step F, the thickness of the upper colloid layer is 1 / 20 of the thickness of the lower block layer.
[0090] like Figure 1 , Figure 2As shown, taking the gap on the ground layer 1 as the standard, after the present invention injects a caulking agent into the gap of the ground layer 1, the caulking agent is cured in the air to obtain a two-layer structure, wherein the upper structure is a low-density polyethylene film 2, and the lower layer is a lower structure 3 after the lower slurry is cured; after the upper structure and the lower structure are cured, they have an obvious stratification effect and can ensure that the main component of the upper material is the low-density polyethylene film.
[0091] like Figure 3 As shown, Figure 3 The infrared spectrum of the middle and upper structure is the upper structure of the seam beautifying agent after stratification. Figure 3 The infrared spectrum in the middle and lower part is a standard spectrum of polyethylene. The characteristic peak of the upper structure of the present invention is 2921.20cm -1 、2854.65cm -1 、1465.90cm -1 、721.38cm -1 , of which 2921.20cm -1 、2854.65cm -1 It is the asymmetric and symmetric stretching vibration absorption peak of methylene -CH2, 1465.9cm -1 -CC skeleton vibration absorption peak, 721.38cm -1 It is the rotation absorption peak of -CH; the results show that the upper layer structure of the seam beautifying agent of the present invention is a low-density polyethylene film.
[0092] Example 2 is based on Example 1, and differs from Example 1 in that the mass ratio of poly(decane-4,6-diynedioic acid) to formamide-grafted low-density polyethylene in component B is 1.2:1.
[0093] Example 3 is based on Example 1, and differs from Example 1 in that the mass ratio of poly(decane-4,6-diynedioic acid) to formamide-grafted low-density polyethylene in component B is 1.4:1.
[0094] Example 4 is based on Example 1, and is different from Example 1 in that the filler includes the following components in parts by weight: 50 parts of 30-40 μm perlite powder, 10 parts of 0.1-0.3 μm silica powder, and 5 parts of 100-120 μm white Portland cement clinker; the mass of the filler accounts for 40% of the total resin mass of the epoxy resin and phenolic resin in component A.
[0095] Example 5 is based on Example 1, and is different from Example 1 in that the filler includes the following components in parts by weight: 55 parts of 30-40 μm perlite powder, 15 parts of 0.1-0.3 μm silica powder, and 7.5 parts of 100-120 μm white Portland cement clinker; the mass of the filler accounts for 37.5% of the total resin mass of the epoxy resin and phenolic resin in component A.
[0096] Example 6 is based on Example 1, and is different from Example 1 in that, based on the total resin mass of the epoxy resin and the phenolic resin in component A, the other functional additives include the following components in proportion by mass: 8% of C12-14 alkyl glycidyl ether, 1% of an acrylate leveling agent, and 1% of 2-pyridinethiol-1-zinc oxide.
[0097] Example 7 is based on Example 1, and is different from Example 1 in that, based on the total resin mass of the epoxy resin and the phenolic resin in component A, the other functional additives include the following components in proportion by mass: 10% of C12-14 alkyl glycidyl ether, 2% of an acrylate leveling agent, and 2% of 2-pyridinethiol-1-zinc oxide.
[0098] Comparative Example 1, taking the caulking agent currently on the market as a comparative example, for example, the brand: Davco, model: Caulking Agent Color Porcelain - Waterproof and Mildew-proof Series, the product number is; 100045245722; the mildew-proof grade is level 0.
[0099] Comparative Example 2 is based on Example 1. The difference between this comparative example and Example 1 is that this comparative example does not contain phenolic resin, and the rest is the same as Example 1.
[0100] Comparative Example 3 is based on Example 1. The difference between this comparative example and Example 1 is that this comparative example does not contain component B, and the rest is the same as Example 1.
[0101] Comparative Example 4 is based on Example 1. The difference between this comparative example and Example 1 is that component B of this comparative example does not contain poly(decane-4,6-diynedioic acid), and the rest is the same as Example 1.
[0102] Comparative Example 5 is based on Example 1. The difference between this comparative example and Example 1 is that component B of this comparative example does not contain formamide-grafted low-density polyethylene, and the rest is the same as Example 1.
[0103] Comparative Example 6 is based on Example 1. The difference between this comparative example and Example 1 is that the mass ratio of epoxy resin to phenolic resin in component A of this comparative example is 1:1, and the rest is the same as Example 1.
[0104] Comparative Example 7 is based on Example 1. The difference between this comparative example and Example 1 is that the mass ratio of epoxy resin to phenolic resin in component A of this comparative example is 3:1, and the rest is the same as Example 1.
[0105] Comparative Example 8 is based on Example 1. The difference between this comparative example and Example 1 is that the mass ratio of poly(decane-4,6-diynedioic acid) and formamide-grafted low-density polyethylene in component B of this comparative example is 1.1:1.
[0106] Comparative Example 9 is based on Example 1. The difference between this comparative example and Example 1 is that the mass ratio of poly(decane-4,6-diynedioic acid) and formamide-grafted low-density polyethylene in component B of this comparative example is 1.5:1.
[0107] Comparative Example 10 is based on Example 1. The difference between this comparative example and Example 1 is that the mass ratio of component A to component B in this comparative example is 3:1.
[0108] Comparative Example 11 is based on Example 1. The difference between this comparative example and Example 1 is that the mass ratio of component A to component B in this comparative example is 5:1.
[0109] Test Example 1: The waterproof performance, mildew resistance, compressive strength, surface roughness and surface flatness of the caulking agents involved in Examples 1-7 and Comparative Examples 1-11 after curing were tested. The test results are shown in Table 1.
[0110] 1) The test method for waterproof performance is as follows: First, prepare the caulking agent sample, ensure that the caulking agent has been completely cured, and then use a special water seepage pressure test equipment after curing for 28 days. The equipment usually includes a pressure source, a pressure gauge, and a sealed test chamber. Put the caulking agent sample into the test chamber and ensure that it is completely sealed. Apply gradually increasing pressure to the test chamber through the pressure source. This pressure is applied in the form of water pressure. Observe the water seepage of the caulking agent sample: In the process of applying pressure, carefully observe whether the caulking agent sample has water seepage. The water seepage phenomenon is divided into: water drop formation, water flow or wet area for detection. As long as any of the above three situations occurs, it means that the caulking agent sample has water seepage. Record the pressure value when the water seepage phenomenon occurs. The larger the pressure value, the better the waterproof performance.
[0111] 2) The method for testing the anti-mildew performance is: through a series of testing methods such as the culture dish method and the hanging method, the caulking agent sample is exposed to a specific mold environment to observe the growth of mold on the surface of the caulking agent.
[0112] Then, the mildew resistance level is divided according to the coverage area of mildew on the surface of the caulking agent sample. Generally, the mildew resistance performance level is divided into five levels from level 0 to level 4; specifically:
[0113] Level 0: No obvious mold growth at about 50 times magnification;
[0114] Level 1: The mold is invisible or difficult to see with the naked eye, but it can be clearly seen under a magnifying glass;
[0115] Level 2: Mold is clearly visible to the naked eye, covering about 10% to 30% of the sample surface;
[0116] Level 3: Mold is clearly visible to the naked eye, covering 30% to 60% of the sample surface;
[0117] Level 4: Mold is clearly visible to the naked eye, covering more than 60% of the sample surface.
[0118] 3) The test method for compressive strength is as follows: Hardness is an important parameter for the compressive strength of the caulking agent. A Rockwell hardness tester is used to apply a certain pressure to the caulking agent sample, and then the hardness value level is determined according to the degree of deformation of the sample. The higher the hardness level, the harder it is for the caulking agent to be crushed, and the stronger its compressive strength is, which indicates that its service life may be longer. The Rockwell hardness level is used as an indicator to evaluate the compressive strength of the caulking agent.
[0119] 4) The detection method of surface roughness is as follows: the surface roughness grade division is based on the arithmetic mean deviation of the profile (Ra), which refers to the arithmetic mean of the absolute value of the profile deviation within the sampling length; according to the different ranges of Ra values, the surface roughness can be divided into different grades, ranging from Ra 0.006 to Ra 50; among them, a lower Ra value indicates a smoother surface, while a higher Ra value indicates a rougher surface; the method for obtaining the arithmetic mean deviation of the profile (Ra):
[0120] Select the test length: In practical applications, select an appropriate test length for measurement. The commonly used test length is 0.8mm.
[0121] Surface measurement: Use high-precision measuring instruments, such as optical microscopes, to scan or measure the cured surface of the caulking agent, which can accurately capture the microscopic ups and downs of the surface;
[0122] Data processing: The measuring instrument records the distance from each measuring point to the surface mean line and calculates the absolute value of these distances. Subsequently, the instrument averages these absolute values to obtain the arithmetic mean deviation (Ra) of the profile.
[0123] The surface flatness detection method is: take the floor tiles as the reference, inject the caulking agent into the gap, scrape it flat, and solidify it. Then use an electron microscope to magnify the gap between the top surface of the caulking agent and the top surface of the two sides of the gap. The gap above the gap side wall is marked as "+", and the gap below the gap side wall is marked as "-". Adjust the magnification of the microscope so that the junction between the caulking agent surface and the gap mouth can be clearly observed. Observe: Aim the microscope at the measurement area and adjust the focus to obtain a clear image. In the image, find the boundary line between the caulking agent surface and the gap mouth. Measure the spacing: Use the measurement software or tool attached to the microscope to measure the distance from the boundary line to the caulking agent surface or the edge of the gap mouth. Mark the starting point and the end point in the image and calculate the distance between them. The smaller this distance is, the better the flatness of the caulking agent is. The distance between the top surface of the caulking agent and the top surface of the two sides of the gap is used as the judgment index of the surface flatness of the caulking agent.
[0124] Table 1 Performance test structure of the seam beautifier after curing
[0125]
[0126] Combining Example 1 of the present invention with Comparative Examples 10 and 11, it can be seen that the ratio between component A and component B affects the flatness of the caulking agent after curing. After the increase of component A, the caulking agent will have obvious expansion phenomenon after curing, so that the caulking agent exceeds the gap, and a protruding part appears between the caulking agent and the gap opening surface, causing the connection interface between the caulking agent and the gap opening to be uneven. The flatness of the caulking agent described in the present invention is the flatness of the connection interface between the caulking agent and the gap opening; if component A is reduced, the caulking agent will have obvious shrinkage phenomenon after curing, so that pits appear at the interface between the caulking agent surface and the gap opening, and then the connection interface is uneven. The caulking agent in Examples 1-7 of the present invention can ensure that the spacing between the caulking agent surface and the gap opening surface is within ±0.01mm, and the best is Example 1, which can be completely flush. The spacing of ±0.01mm is difficult to detect with the naked eye, and it is basically flush from a macroscopic point of view. Therefore, the flatness of the caulking agent of the present invention after curing is very high.
[0127] Combined with the above data, each component in component A and component B and the ratio between component A and component B will have a significant impact on the hardness, waterproof performance, surface roughness and flatness of the caulking agent after curing. Example 1 in Table 1 is the best ratio; as the amount of epoxy resin added increases, the hardness of the caulking agent will first increase, and after increasing to a certain value, it will show a downward trend.
[0128] Test Example 2: The delamination phenomenon, curing time and upper layer thickness of the seam beautifying agent were tested for Examples 1-7 and Comparative Examples 1-11. The test results are shown in Table 2.
[0129] Sealant stratification phenomenon: Direct observation method is used to inject the sealant into the test mold to observe whether the sealant shows stratification phenomenon in the natural environment.
[0130] Curing time: Use existing methods to measure the time it takes for the caulking agent to completely cure.
[0131] Upper layer thickness: When measuring the upper layer thickness, the ratio of the upper layer thickness to the lower layer thickness is used as a reference value.
[0132] Table 2 Performance test results of the seam beautifier
[0133]
[0134] The proportion of the upper layer thickness will affect the strength of the overall structure of the caulking agent. If the upper layer thickness increases, the strength of the overall structure of the caulking agent will decrease. If the upper layer thickness is too thin, it will not provide a good protective effect. Therefore, the present invention preferably selects the optimal thickness ratio of 4.2%-5.2%. Combining the data in Table 1 and Table 2, the best implementation of the present invention is Example 1.
[0135] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An ultra-flat seam beautifying agent, characterized in that: It includes component A and component B, and the mass ratio of component A to component B is 4:1; The component A comprises the following components: epoxy resin, phenolic resin, pigment, filler, and other functional additives, wherein the mass ratio of epoxy resin to phenolic resin is 2:1, based on the total resin mass of epoxy resin and phenolic resin in component A, the other functional additives comprise the following components in proportion by mass: 8-10% of C12-14 alkyl glycidyl ether, 1-2% of acrylate leveling agent, and 1-2% of 2-pyridinethiol-1-zinc oxide; the filler comprises the following components in proportion by weight: 50-60 parts of 30-40 μm perlite powder, 10-20 parts of 0.1-0.3 μm silica powder, and 5-8 parts of 100-120 μm white silicate cement clinker; the mass of the filler accounts for 35-40% of the total resin mass of epoxy resin and phenolic resin in component A; The component B comprises the following components: poly(4,6-decanediyne dioic acid) and formamide grafted low-density polyethylene, wherein the mass ratio of poly(4,6-decanediyne dioic acid) and formamide grafted low-density polyethylene is 1.2-1.4:1; Based on component A and component B, the super flat seam agent has the following two states: When the super-flat seam-beautifying agent is in a light-proof and sealed environment, the super-flat seam-beautifying agent is a uniform slurry prepared by mixing component A and component B; When the super flat seam agent is exposed to oxygen and light, the super flat seam agent changes from a uniform slurry state to an upper and lower double-layer structure, wherein the double-layer structure includes an upper colloid layer and a lower slurry layer, specifically: The poly (decane-4,6-diynedioic acid) in component B decomposes under oxygen and light conditions to produce succinic acid. Under the acidic conditions of succinic acid production, the formamide in component B grafted with low-density polyethylene undergoes hydrolysis and debranching to produce ammonia water, formic acid and low-density polyethylene. The caulking agent in the gap is stratified, with the upper layer being the upper colloid layer and the lower layer being the lower slurry layer; the upper colloid layer includes low-density polyethylene and ammonia water, and the mass of the ammonia water accounts for 0.8%-1% based on the total mass of the upper colloid layer; the lower slurry layer includes component A, ammonia water, formic acid and succinic acid.
2. The ultra-flat seam sealant according to claim 1, characterized in that: The mass ratio of poly(decane-4,6-diynedioic acid) to formamide-grafted low-density polyethylene in the component B is 1.3:
1.
3. The ultra-flat seam-beautifying agent according to claim 1, characterized in that: The filler comprises the following components in parts by weight: 60 parts of 30-40 μm perlite powder, 20 parts of 0.1-0.3 μm silica powder, and 8 parts of 100-120 μm white silicate cement clinker; the mass of the filler accounts for 35% of the total mass of the epoxy resin and phenolic resin in component A.
4. The ultra-flat seam-beautifying agent according to claim 1, characterized in that: Prepared by the following method: S1. Preparation of component A: S1.1, melting the epoxy resin at a temperature of 180°C to obtain an epoxy resin glue solution; S1.2, melting the phenolic resin at a temperature of 105°C to obtain a phenolic resin glue solution; S1.2, after mixing the epoxy resin glue and the phenolic resin glue, cool down to 100°C, stir at 100°C for 10-20 minutes until they are evenly mixed, cool down to 80°C again after evenly mixing, add other functional additives at 80°C and continue to stir until they are evenly mixed to obtain a diluted mixed glue; S1.3, evenly mix the solid components in the filler, then cool the mixed glue to 50-60°C, slowly add the filler to the mixed glue at 50-60°C while stirring at a speed of 280-300 rpm, continue stirring for 1-2 hours, then add the pigment and mix evenly to obtain component A; S2, preparing component B: using formamide monomer to graft-modify low-density polyethylene to obtain formamide-grafted low-density polyethylene, then mixing the formamide-grafted low-density polyethylene with poly (decane-4,6-diynedioic acid) and adding them into an anaerobic stirring tank, and uniformly mixing at 30° C. for 30-40 minutes to obtain component B; S3. In an anaerobic stirring tank, component A and component B are mixed to obtain a uniform caulking agent slurry, and then the caulking agent slurry is transferred to a vacuum sealed container for standby use.
5. The ultra-flat seam-beautifying agent according to claim 4, characterized in that: The formamide grafted low-density polyethylene is prepared by the following method: a. Low-density polyethylene with a density of 0.91 g / cm³ is used as the base polymer and formamide is used as the grafting monomer; b. exposing the low-density polyethylene to a radiation source, wherein the radiation source is ultraviolet light, electron beam or gamma ray, and the radiation treatment is performed for 30-40 seconds; c. After the radiation treatment of the low-density polyethylene is completed, formamide is added immediately and stirred for 20-30 minutes to carry out a grafting reaction to obtain formamide-grafted low-density polyethylene. The mass ratio of formamide to low-density polyethylene is 1:
20.
6. A flat seam construction process of an ultra-flat seam beautifying agent according to any one of claims 1 to 5, characterized in that: The following steps are involved: A. Clean the gap: Use a slotter or utility knife to clean the filler in the gap, and ensure that there is no sand, dust or water in the gap. The gap is the gap on the horizontal surface; B. Paste masking tape: Paste masking tape on both sides of the gap; C. Preparing a seam beautifying agent: preparing component A and component B respectively, wherein component B is prepared in an anaerobic environment, and then mixing component A and component B in an anaerobic environment to prepare a seam beautifying agent slurry, and placing the seam beautifying agent slurry in a vacuum sealed container for standby use; D. Gluing: Pour the caulking agent into the glue gun and start gluing. The caulking agent is evenly filled in the gap, and the filling thickness of the caulking agent is greater than the depth of the gap. After the caulking agent is filled in the gap, the poly (decane-4,6-diynedioic acid) in the caulking agent component B is exposed to the air, decomposes under oxygen and light conditions, and produces succinic acid; under the acidic conditions of succinic acid production, the formamide in the formamide-grafted low-density polyethylene undergoes hydrolysis and debranching, producing ammonia water, formic acid and low-density polyethylene, and the caulking agent in the gap is layered, with the upper layer being the upper colloid layer and the lower layer being the lower slurry layer; the upper colloid layer includes low-density polyethylene and ammonia water, and the lower slurry layer includes component A, ammonia water, formic acid, and succinic acid; E. Pressing and leveling the seams: Use a scraper to scrape off the excess transparent glue layer on the top surface of the gap, so that the seam beautifier is flush with the surfaces on both sides of the gap; F. Drying: After drying and curing for 12-14 hours, the caulking agent in the gap forms a solid double-layer structure. The upper structure is a transparent film after the upper colloid layer is cured, and the lower structure is a block-shaped solid after the lower slurry layer that matches the shape of the gap is cured, completing the flat seam construction.
7. The flat seam construction process of the super flat seam beautifying agent according to claim 6 is characterized in that: The scraper in step E is a stainless steel plate.
8. The flat seam construction process of the super flat seam beautifying agent according to claim 6 is characterized in that: After drying and curing in step F, the thickness of the upper colloid layer is 1 / 20 of the thickness of the lower block layer.
Citation Information
Patent Citations
Preparation method for solid unsaturated carboxylic acid-functionalized linear low density polyethylene
CN103232575A
Low surface energy uv curable ink suitable for high-speed printing and preparation method thereof
CN110499066A
Graft polymers and method of making the same
FR1177898A
A method of preparing for a modified polyethylenehaving imporved mechanical strength for thermal sprayand a modified polyethylene thereby
KR1020030054491A