A low-damage ITO etching solution

By using a combination of nitric acid, sulfuric acid, oxalic acid, copper layer protective agent, surfactant and konjac glucomannan in the ITO etching solution, a dense protective film is formed, which solves the corrosion of the copper layer and PR glue caused by the existing ITO etching solution. The black shadow problem on the surface enables more efficient ITO layer etching and copper layer protection.

CN118638554BActive Publication Date: 2024-10-29HEFEI SINOPISE MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411127628.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-29
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The existing ITO etching solution cannot effectively avoid the black shadow phenomenon on the surface of the PR glue, cannot meet the needs of the production line, and causes secondary corrosion to the copper layer, resulting in excessive side corrosion.

Method used

Using a low-damage ITO etching solution formula, including nitric acid, sulfuric acid, oxalic acid, copper layer protective agent, surfactant, inorganic nitrate and konjac glucomannan, by strictly controlling the content of nitric acid, sulfuric acid and the role of copper layer protective agent, Form a dense protective film to reduce the corrosion of the copper layer by the ITO etching solution.

Benefits of technology

It effectively avoids black shadows on the surface of the PR glue, reduces the loss of the copper layer, improves the etching effect of the ITO layer, ensures the protection of the copper layer, and meets the application needs in the display panel field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118638554B_ABST
    Figure CN118638554B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of etching solutions, and specifically discloses a low-damage ITO etching solution. The low-damage ITO etching solution comprises the following raw materials in weight percentage: 5-10% nitric acid, 3-10% sulfuric acid, 0.1-0.5% oxalic acid, 0.3-1% copper layer protective agent, 0.1-2% surfactant, 0.5-1.5% inorganic nitrate, 0.01-0.5% konjac glucomannan, and the balance is water; in the ITO etching solution of the present invention, konjac glucomannan has a stable three-dimensional network structure, forms a complex with copper ions and adheres to the copper surface, has strong film-forming property, and can reduce the erosion of the copper layer by the ITO etching solution; it can interact with the copper layer protective agent to form a dense protective film on the surface of the metal copper layer, effectively avoiding the phenomenon of black shadows on the surface of PR glue.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of etching liquid, and more specifically, to a low-damage ITO etching liquid. Background Art

[0002] In capacitive touch screens, a double-layer structure of copper and ITO (indium tin oxide) is often used to design the sensor. Due to the difference in the chemical properties of copper and ITO, different etching solutions and conditions are required when etching them. Usually, a two-step etching method is used to etch the copper layer first and then the ITO layer. Existing ITO etching solutions are mainly divided into oxalic acid, sulfonic acid, and aluminic acid. Oxalic acid is prone to crystallization, which affects production line production; aluminic acid cannot effectively protect the upper metal layer, resulting in corrosion of other metal layers while etching ITO, resulting in large side etching.

[0003] After etching the copper and ITO double-layer sample with sulfonic acid ITO etching solution, the sample was observed through an optical microscope, and black shadows were found on the surface of the PR glue. After analysis, it was mainly because when etching the ITO layer, the ITO etching solution would cause slight etching of the copper layer, resulting in poor adhesion between the copper layer and the PR glue, causing the PR glue to fall off; and when the concentration of copper ions in the ITO etching solution on the production line exceeds 500ppm, the copper ions will undergo an oxidation-reduction reaction with metallic copper, which will further aggravate the corrosion of the copper layer.

[0004] At present, CN114507528A discloses a sulfuric acid-based ITO etching solution, comprising the following raw materials in percentage by weight: 10-20 parts of sulfuric acid, 5-15 parts of nitric acid, 20-30 parts of acetic acid, 0.01-2 parts of inorganic chloride, 0.1-2 parts of surfactant, and water; wherein the surfactant includes at least one of polyoxyethylene fatty amine, polyoxyethylene fatty diamine and fatty alcohol polyoxyethylene ether ammonium sulfate; the ITO etching solution solves the ITO residue problem and side etching phenomenon on the surface of the substrate; but it is still difficult to avoid the phenomenon of black shadows on the surface of the PR glue, and it cannot meet the needs of the production line. Based on the above statement, the present invention proposes a low-damage ITO etching solution. Summary of the invention

[0005] In order to solve the problems that the existing ITO etching solution cannot avoid the phenomenon that black shadows appear on the surface of PR glue and cannot meet the needs of the production line, the present invention provides a low-damage ITO etching solution.

[0006] The present invention provides a low-damage ITO etching solution, which adopts the following technical solution:

[0007] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5-10% nitric acid, 3-10% sulfuric acid, 0.1-0.5% oxalic acid, 0.3-1% copper layer protective agent, 0.1-2% surfactant, 0.5-1.5% inorganic nitrate, 0.01-0.5% konjac glucomannan, and the balance is water.

[0008] Preferably, the low-damage ITO etching solution comprises the following raw materials in weight percentage: 9% nitric acid, 5% sulfuric acid, 0.1% oxalic acid, 0.5% copper layer protective agent, 1.5% surfactant, 1.2% inorganic nitrate, 0.5% konjac glucomannan, and the balance is water.

[0009] By adopting the above technical scheme, the present invention strictly controls the contents of nitric acid, sulfuric acid and oxalic acid in the ITO etching solution to achieve preliminary regulation of the etching speed of the ITO layer by the ITO etching solution; in the etching process, most of the nitric acid, sulfuric acid and oxalic acid in the ITO etching solution are consumed by ITO, reducing the problem of secondary corrosion of the copper layer by the ITO etching solution; oxalic acid can not only provide acidity, but also can be used as a complexing agent to protect the copper layer; in addition, the konjac glucomannan in the ITO etching solution of the present invention has a stable three-dimensional network structure, forms a complex with copper ions and adheres to the copper surface, has strong film-forming property, and can reduce the erosion of the copper layer by the ITO etching solution; and can interact with the copper layer protective agent to form a dense protective film on the surface of the metal copper layer, effectively avoiding the phenomenon of black shadows on the surface of the PR glue.

[0010] Preferably, the copper layer protective agent is prepared by the following method:

[0011] S1. Add rosin acid to p-xylene, evacuate, heat to 80-100°C, slowly add N-phenylethylenediamine through a constant pressure dropping funnel, and complete the addition within 10-20 minutes, then heat to 110-120°C for reaction for 2-3 hours, and then heat to 180-200°C for dehydration for 2-4 hours until no water precipitates, and terminate the reaction; cool to room temperature, pour the reaction solution into water, adjust the pH value to 7-8 with 30wt% sodium hydroxide solution, precipitate solid, filter under reduced pressure, and vacuum dry to obtain compound A;

[0012] S2. Compound A obtained in step S1 and 1,4-dichlorobenzyl are added to ethanol, and the mixture is refluxed at 80-90° C. for 3-4 hours. After the reaction is completed, the solvent is removed by distillation under reduced pressure, and acetone is added for recrystallization and purification to obtain a copper layer protective agent.

[0013] Preferably, in step S1, the mass ratio of rosin acid, N-phenylethylenediamine and p-xylene is 30:13-15:40-50.

[0014] Preferably, in step S2, the mass ratio of compound A, 1,4-dichlorobenzyl and ethanol is 76-80:17:80-100.

[0015] By adopting the above technical scheme, the present invention uses rosin acid, N-phenylethylenediamine and 1,4-dichlorobenzyl as raw materials to prepare a copper layer protective agent, and the chemical reaction process is as follows:

[0016] ;

[0017] The lone pair electrons of C=N and CN in the copper layer protective agent molecule of the present invention and the large π bond on the phenyl group can combine with the empty d orbital of the copper atom on the metal surface to form a coordination bond, thereby being adsorbed on the surface of the metal copper to form a protective film, preventing the contact between the ITO etching solution and the metal copper, and hindering the transfer of charges or substances related to the corrosion reaction; and the multi-center adsorption generated by the bisimidazoline structure of the copper layer protective agent molecule can make the formed protective film more compact, with a faster film forming rate and a better protective effect; at the same time, the tricyclic diterpenoid structure in the copper layer protective agent molecule can penetrate into the tiny pores and cracks on the surface of the copper layer to form a dense hydrophobic filling layer, the filling layer has a strong bonding force with the copper layer, is not easy to fall off, better prevents the penetration of the ITO etching solution, improves the overall protective effect of the copper layer, and further effectively improves the phenomenon of black shadows on the surface of the PR glue.

[0018] Preferably, the surfactant is Triton X-100 and / or sophorolipid.

[0019] Preferably, the surfactant is obtained by mixing Triton X-100 and sophorolipids in a mass ratio of 2:1.

[0020] By adopting the above technical scheme, the surfactant of the present invention is Triton X-100 and / or sophorolipid, which has excellent emulsification and dispersion performance, good lubrication performance and vibration and drag reduction performance, can significantly reduce the surface tension at the liquid-air interface, generate stable bubbles, and can improve the wetting and corrosion uniformity of the etching solution on the ITO layer, so that the etching surface is smoother, without residue and side corrosion; at the same time, the surfactant can also undergo characteristic adsorption on the surface of the copper layer, blocking the ionization process of copper, and acting together with other components in the ITO etching solution to reduce the loss of the copper layer; further preferably, a mixture of Triton X-100 and sophorolipid in a specific ratio is used as the surfactant, which improves the compatibility with the copper layer protective agent and promotes the stability of the ITO etching solution.

[0021] Preferably, the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1-6.

[0022] By adopting the above technical scheme, the inorganic nitrate of the present invention is a mixture of ammonium nitrate and potassium nitrate, and the two have a synergistic effect, which can control the etching speed of the ITO layer, avoid violent etching reaction, cause excessive etching, and further reduce the contact area between the copper layer and the etching solution, thereby effectively protecting the copper layer; at the same time, ammonium ions and potassium ions are used as impurity ions to inhibit crystal growth, reduce residual phenomena, and maintain the cleanliness of the etched surface.

[0023] The present invention also provides a method for preparing a low-damage ITO etching solution, which adopts the following technical solution:

[0024] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0025] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0026] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir for 5-10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0027] By adopting the above technical scheme, the preparation method of the ITO etching solution of the present invention has simple steps and low cost, is safe and environmentally friendly, and is suitable for industrial production. The obtained ITO etching solution has good application prospects and large-scale industrial promotion potential in the field of display panels.

[0028] In summary, the present invention has the following beneficial effects:

[0029] The ITO etching solution of the present invention comprises nitric acid, sulfuric acid, oxalic acid, a copper layer protective agent, a surfactant, an inorganic nitrate and konjac glucomannan. The components interact and assist each other, and can not only effectively etch the ITO layer, but also form a uniform and dense protective film on the surface of the metal copper layer, effectively avoiding the phenomenon of black shadows on the surface of the PR glue, so that the ITO etching solution of the present invention has a wide application prospect in the field of display panel etching. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a SEM image of the sample after being treated with the ITO etching solution in Example 1 of the present invention;

[0031] Figure 2 This is a SEM image of the sample after being treated with the ITO etching solution in Comparative Example 1 of the present invention;

[0032] Figure 3 This is an optical microscope image of a sample after being treated with the ITO etching solution in Example 1 of the present invention;

[0033] Figure 4This is an optical microscope image of the sample after being treated with the ITO etching solution in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below with reference to the embodiments.

[0035] The materials and reagents used in the examples of the present invention, unless otherwise specified, can be obtained from commercial sources; wherein abietic acid: CAS No. 514-10-3, purchased from Shanghai Yuanye Biological Co., Ltd. (HPLC ≥ 90%); N-phenylethylenediamine: CAS No. 1664-40-0, purchased from Shanghai Yuanye Biological Co., Ltd. (HPLC> 98%); Triton X-100: molecular formula: C 8 H 17 C 6 H 4 (OCH 2 CH 2 ) n OH (n≈10), CAS No. 9002-93-1, purchased from Shanghai McLean Biochemical Technology Co., Ltd. (97%); Sophorolipids: CAS No. 148409-20-5, purchased from Shanghai McLean Biochemical Technology Co., Ltd. (HPLC≥95%); Konjac Glucomannan: CAS No. 37220-17-0, purchased from Shanghai Yuanye Biological Co., Ltd. (purity ≥95%).

[0036] Preparation Examples 1-3 provide methods for preparing copper layer protective agents.

[0037] Preparation Example 1

[0038] Copper layer protective agent is prepared by the following method:

[0039] S1. Add 30 g of rosin acid to 40 g of p-xylene, evacuate, heat to 80 ° C, slowly add 13 g of N-phenylethylenediamine through a constant pressure dropping funnel, and complete the addition in 10 minutes. Then heat to 110 ° C for reaction for 3 hours, and then heat to 180 ° C for dehydration for 4 hours until no water precipitates. End the reaction; cool to room temperature, pour the reaction solution into 250 mL of water, adjust the pH value to 7 with 30 wt% sodium hydroxide solution, precipitate solid, filter under reduced pressure, and vacuum dry to obtain compound A;

[0040] S2. Add 76 g of the compound A obtained in step S1 and 17 g of 1,4-dichlorobenzyl into 80 g of ethanol, and reflux at 80° C. for 4 h. After the reaction, remove the solvent by distillation under reduced pressure, add acetone for recrystallization and purification, and obtain a copper layer protective agent.

[0041] Preparation Example 2

[0042] Copper layer protective agent is prepared by the following method:

[0043] S1. Add 30 g of rosin acid to 45 g of p-xylene, evacuate, heat to 90°C, slowly drop 14 g of N-phenylethylenediamine through a constant pressure dropping funnel, complete the dropwise addition in 15 min, then heat to 115°C for reaction for 2.5 h, and then heat to 190°C for dehydration for 3 h until no water precipitates, terminate the reaction; cool to room temperature, pour the reaction solution into 250 mL of water, adjust the pH value to 7.5 with 30 wt% sodium hydroxide solution, precipitate a solid, filter under reduced pressure, and dry in vacuo to obtain compound A;

[0044] S2. Add 78 g of the compound A obtained in step S1 and 17 g of 1,4-dichlorobenzyl into 90 g of ethanol, and reflux at 85° C. for 3.5 h. After the reaction is completed, remove the solvent by distillation under reduced pressure, add acetone for recrystallization and purification, and obtain a copper layer protective agent.

[0045] Preparation Example 3

[0046] Copper layer protective agent is prepared by the following method:

[0047] S1. Add 30 g of rosin acid to 50 g of p-xylene, evacuate, heat to 100 ° C, slowly add 15 g of N-phenylethylenediamine through a constant pressure dropping funnel, and complete the addition in 20 minutes. Then heat to 120 ° C for reaction for 2 hours, and then heat to 200 ° C for dehydration for 2 hours until no water precipitates. End the reaction; cool to room temperature, pour the reaction solution into 250 mL of water, adjust the pH value to 8 with 30 wt% sodium hydroxide solution, precipitate solid, filter under reduced pressure, and vacuum dry to obtain compound A;

[0048] S2. Add 80 g of the compound A obtained in step S1 and 17 g of 1,4-dichlorobenzyl into 100 g of ethanol, and reflux at 90° C. for 3 h. After the reaction, remove the solvent by distillation under reduced pressure, add acetone for recrystallization and purification, and obtain a copper layer protective agent.

[0049] Embodiment 1-6 provides a low-damage ITO etching solution and a preparation method thereof.

[0050] Example 1

[0051] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.1% oxalic acid, 0.3% copper layer protective agent, 0.1% surfactant, 0.5% inorganic nitrate, 0.01% konjac glucomannan, and the balance is water;

[0052] The copper layer protective agent is prepared by Preparation Example 1; the surfactant is sophorolipid; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1;

[0053] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0054] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0055] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0056] Example 2

[0057] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 8% nitric acid, 6% sulfuric acid, 0.25% oxalic acid, 0.5% copper layer protective agent, 1% surfactant, 1% inorganic nitrate, 0.5% konjac glucomannan, and the balance is water;

[0058] The copper layer protective agent is prepared by Preparation Example 2; the surfactant is sophorolipid; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 1:2;

[0059] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0060] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0061] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 500 r / min for 8 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0062] Example 3

[0063] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 10% nitric acid, 3% sulfuric acid, 0.5% oxalic acid, 1% copper layer protective agent, 2% surfactant, 1.5% inorganic nitrate, 0.3% konjac glucomannan, and the balance is water;

[0064] The copper layer protective agent is prepared by Preparation Example 3; the surfactant is obtained by mixing Triton X-100 and sophorolipids in a mass ratio of 1:1; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 1:3;

[0065] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0066] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0067] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 600 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0068] Example 4

[0069] Example 4 is different from Example 1 only in that the surfactant is Triton X-100, as follows:

[0070] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.1% oxalic acid, 0.3% copper layer protective agent, 0.1% surfactant, 0.5% inorganic nitrate, 0.01% konjac glucomannan, and the balance is water;

[0071] The copper layer protective agent is prepared by Preparation Example 1; the surfactant is sophorolipid; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1;

[0072] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0073] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0074] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0075] Example 5

[0076] Example 5 is different from Example 1 only in that the surfactant is obtained by mixing Triton X-100 and sophorolipids in a mass ratio of 2:1, as follows:

[0077] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.1% oxalic acid, 0.3% copper layer protective agent, 0.1% surfactant, 0.5% inorganic nitrate, 0.01% konjac glucomannan, and the balance is water;

[0078] The copper layer protective agent is prepared by Preparation Example 1; the surfactant is obtained by mixing Triton X-100 and sophorolipids in a mass ratio of 2:1; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1;

[0079] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0080] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0081] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0082] Example 6

[0083] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 9% nitric acid, 5% sulfuric acid, 0.1% oxalic acid, 0.5% copper layer protective agent, 1.5% surfactant, 1.2% inorganic nitrate, 0.5% konjac glucomannan, and the balance is water;

[0084] The copper layer protective agent is prepared by Preparation Example 1; the surfactant is obtained by mixing Triton X-100 and sophorolipids in a mass ratio of 2:1; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1;

[0085] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0086] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0087] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 600 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0088] In order to verify the comprehensive performance of the low-damage ITO etching solution prepared in Examples 1-6 of the present invention, comparative examples 1-7 are set, which are as follows:

[0089] Comparative Example 1

[0090] Comparative Example 1 is different from Example 1 only in that no copper layer protective agent is added, as follows:

[0091] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.1% oxalic acid, 0.1% surfactant, 0.5% inorganic nitrate, 0.01% konjac glucomannan, and the balance is water;

[0092] The surfactant is a sophorolipid; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1;

[0093] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0094] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0095] Step (2): Continue to add surfactant and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 min until all materials are evenly mixed to obtain a low-damage ITO etching solution.

[0096] Comparative Example 2

[0097] Comparative Example 2 is different from Example 1 only in that the copper layer protective agent is replaced by an equal mass of benzimidazole, as follows:

[0098] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.1% oxalic acid, 0.3% benzimidazole, 0.1% surfactant, 0.5% inorganic nitrate, 0.01% konjac glucomannan, and the balance is water;

[0099] The surfactant is a sophorolipid; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1;

[0100] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0101] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0102] Step (2): Continue to add benzimidazole, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 min until all materials are evenly mixed to obtain a low-damage ITO etching solution.

[0103] Comparative Example 3

[0104] Comparative Example 3 is different from Example 1 only in that an equal amount of dodecyltrimethylammonium bromide is used to replace the sophorolipid, as follows:

[0105] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.1% oxalic acid, 0.3% copper layer protective agent, 0.1% surfactant, 0.5% inorganic nitrate, 0.01% konjac glucomannan, and the balance is water;

[0106] The copper layer protective agent is prepared by Preparation Example 1; the surfactant is dodecyltrimethylammonium bromide; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1;

[0107] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0108] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0109] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0110] Comparative Example 4

[0111] Comparative Example 4 is different from Example 1 only in that no konjac glucomannan is added, specifically as follows:

[0112] A low-damage ITO etching solution, comprising the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.1% oxalic acid, 0.3% copper layer protective agent, 0.1% surfactant, 0.5% inorganic nitrate, and the balance is water;

[0113] The copper layer protective agent is prepared by Preparation Example 1; the surfactant is sophorolipid; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1;

[0114] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0115] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0116] Step (2): Continue to add the copper layer protective agent and surfactant to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0117] Comparative Example 5

[0118] Comparative Example 5 is different from Example 1 only in that oxalic acid is not added, specifically as follows:

[0119] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.3% copper layer protective agent, 0.1% surfactant, 0.5% inorganic nitrate, 0.01% konjac glucomannan, and the balance is water;

[0120] The copper layer protective agent is prepared by Preparation Example 1; the surfactant is sophorolipid; the inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1;

[0121] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0122] Step (1): Weigh water, nitric acid, sulfuric acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0123] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0124] Comparative Example 6

[0125] Comparative Example 6 is different from Example 1 only in that the inorganic nitrate is only ammonium nitrate, as follows:

[0126] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.1% oxalic acid, 0.3% copper layer protective agent, 0.1% surfactant, 0.5% inorganic nitrate, 0.01% konjac glucomannan, and the balance is water;

[0127] Wherein, the copper layer protective agent is prepared by Preparation Example 1; the surfactant is sophorolipid; the inorganic nitrate is ammonium nitrate;

[0128] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0129] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0130] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0131] Comparative Example 7

[0132] Comparative Example 7 is different from Example 1 only in that the inorganic nitrate is only potassium nitrate, as follows:

[0133] A low-damage ITO etching solution comprises the following raw materials in percentage by weight: 5% nitric acid, 10% sulfuric acid, 0.1% oxalic acid, 0.3% copper layer protective agent, 0.1% surfactant, 0.5% inorganic nitrate, 0.01% konjac glucomannan, and the balance is water;

[0134] Wherein, the copper layer protective agent is prepared by Preparation Example 1; the surfactant is sophorolipid; the inorganic nitrate is potassium nitrate;

[0135] A method for preparing a low-damage ITO etching solution comprises the following steps:

[0136] Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution;

[0137] Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir at a speed of 400 r / min for 10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

[0138] In order to verify the comprehensive performance of the low-damage ITO etching solutions prepared in Examples 1-6 and Comparative Examples 1-7 of the present invention, the following performance tests were performed respectively.

[0139] 100 mL of the ITO etching solution obtained in Examples 1-6 and Comparative Examples 1-7 were taken respectively, 0.06 g of copper powder was added, and after stirring at 40°C for 30 min, the content of copper ions in the etching solution was detected by ICP-OES; at the same time, the ITO etching solution obtained in Examples 1-6 and Comparative Examples 1-7 was used to treat the sample (the copper layer thickness was 5000Å, and the ITO layer thickness was 500Å); an optical microscope was used to observe the surface of the PR glue on the sample at a magnification of 100 times for black shadows; a SEM electron microscope was used to observe the microscopic morphology of the sample; the specific results are shown in Table 1, Figure 1-4 As shown, Figure 1 , Figure 2 They are SEM images of Example 1 and Comparative Example 1 respectively; Figure 3 , 4 They are optical microscope images of Example 1 and Comparative Example 1 respectively.

[0140] Table 1:

[0141]

[0142] It can be seen from Table 1 that the ITO etching solution of Examples 1-6 has significantly lower etching ability on copper powder than that of Comparative Examples 1-7, and there is no black shadow on the surface of the PR glue, which fully demonstrates that the ITO etching solution of the present invention causes less loss to the copper layer, effectively protects the copper layer, and improves the etching effect.

[0143] Comparison of Example 1 with Comparative Examples 1 and 2 shows that the copper layer protective agent of the present invention has a significant protective effect on the copper layer and is better than benzimidazole.

[0144] Comparing Example 1 with Comparative Example 3, it is shown that the preferred surfactant of the present invention is better than dodecyltrimethylammonium bromide; further comparing Example 1 with Examples 4 and 5, it is shown that the preferred two-component surfactant of the present invention is more helpful in reducing the loss of the copper layer by the ITO etching solution than the single-component surfactant.

[0145] Comparison of Example 1 and Comparative Example 4 shows that adding konjac glucomannan to the ITO etching solution can reduce the corrosion of the ITO etching solution on the copper layer.

[0146] Comparison of Example 1 and Comparative Example 5 shows that when oxalic acid is added to the ITO etching solution, the oxalic acid can play a role in complexing copper ions.

[0147] Comparison of Example 1 with Comparative Examples 6 and 7 shows that the mixture of ammonium nitrate and potassium nitrate is an inorganic nitrate, which is beneficial to protecting the copper layer.

[0148] Depend on Figure 1-4 It can be seen that the sample treated with the ITO etching solution of Example 1 ( Figure 1 , Figure 3 ), it was found that the ITO layer could be effectively etched, and the copper layer was not damaged. The PR glue was closely attached to the surface of the copper layer, and no black shadow appeared on the surface of the PR glue; while the sample treated with the ITO etching solution without adding the copper layer protective agent in Comparative Example 1 ( Figure 2 , Figure 4 ), it was found that the copper layer incision had obvious corrosion phenomenon, the PR glue fell off from the surface of the copper layer, and there was no photosensitive material in the gap, resulting in a black shadow on the surface of the PR glue.

[0149] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

Claims

1. A low-damage ITO etching solution, characterized in that: The method comprises the following raw materials in weight percentage: 5-10% nitric acid, 3-10% sulfuric acid, 0.1-0.5% oxalic acid, 0.3-1% copper layer protective agent, 0.1-2% surfactant, 0.5-1.5% inorganic nitrate, 0.01-0.5% konjac glucomannan, and the balance is water; The copper layer protective agent is prepared by the following method: S1. Add rosin acid to p-xylene, evacuate, heat to 80-100°C, slowly add N-phenylethylenediamine through a constant pressure dropping funnel, and complete the addition within 10-20 minutes, then heat to 110-120°C for reaction for 2-3 hours, and then heat to 180-200°C for dehydration for 2-4 hours until no water precipitates, and then cool to room temperature, pour the reaction solution into water, adjust the pH value to 7-8 with 30wt% sodium hydroxide solution, precipitate solid, filter under reduced pressure, and vacuum dry to obtain compound A; S2, adding compound A obtained in step S1 and 1,4-dichlorobenzyl to ethanol, reflux at 80-90° C. for 3-4 hours, and after the reaction, removing the solvent by distillation under reduced pressure, adding acetone for recrystallization and purification, to obtain a copper layer protective agent; In step S1, the mass ratio of rosin acid, N-phenylethylenediamine and p-xylene is 30:13-15:40-50; In step S2, the mass ratio of compound A, 1,4-dichlorobenzyl and ethanol is 76-80:17:80-100; The surfactant is obtained by mixing Triton X-100 and sophorolipids in a mass ratio of 2:1; The inorganic nitrate is obtained by mixing ammonium nitrate and potassium nitrate in a mass ratio of 2:1-6.

2. The low damage ITO etching solution according to claim 1, characterized in that The invention comprises the following raw materials in weight percentage: 9% nitric acid, 5% sulfuric acid, 0.1% oxalic acid, 0.5% copper layer protective agent, 1.5% surfactant, 1.2% inorganic nitrate, 0.5% konjac glucomannan, and the balance is water.

3. A method for preparing a low-damage ITO etching solution as claimed in claim 1 or 2, characterized in that: The following steps are involved: Step (1): Weigh water, nitric acid, sulfuric acid, oxalic acid, and inorganic nitrate respectively and add them into a container in sequence to obtain a mixed solution; Step (2): Continue to add the copper layer protective agent, surfactant, and konjac glucomannan to the mixed solution obtained in step (1), and stir for 5-10 minutes until all the materials are evenly mixed to obtain a low-damage ITO etching solution.

Citation Information

Patent Citations

  • Etchant and method for manufacturing display device using the same

    CN104651839A

  • Metal label manufacturing method based on etching process

    CN114836757A