A flexible battery with freely designed shape and preparation method thereof
Through the design of aluminum-plated aramid and copper-plated aramid fiber electrodes and the use of gel electrolytes, the shortcomings of traditional flexible batteries in bending and shape design are solved, and flexible batteries with high energy density and multiple bends are achieved. for various shapes and angles.
Patent Information
- Application Number
- CN202411095371.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-12
AI Technical Summary
Traditional flexible batteries are prone to separation of electrode materials and current collectors when bending, folding and deforming, affecting electrochemical performance, and failing to achieve free design of shapes, limiting the application range and capacity of the battery.
Aluminum-plated aramid and copper-plated aramid as the current collector of fiber electrodes. By uniformly coating the positive and negative electrode materials, the fibrous electrodes are arranged in the desired shape, combined with gel electrolytes, the free design and high energy of flexible batteries are achieved. density.
The multiple bends and free-form design of flexible batteries are realized, which improves the energy density and safety of the batteries, and can configure larger capacity batteries in irregular spaces to meet the needs of various shapes and angles.
Smart Images

Figure CN118645704B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a flexible battery with a freely designable shape and a preparation method thereof, belonging to the technical field of battery preparation. Background Art
[0002] With the trend of intelligent and highly integrated electronic devices, the research and development of flexible electronic devices has progressed rapidly and is widely used in communications, healthcare, wearable devices and consumer electronics. As the energy supply in these flexible electronic devices, the demand for high-performance flexible batteries is becoming more and more urgent. Traditional lithium-ion battery products are rigid. When bent, folded, or deformed, it is easy to cause the electrode material and the current collector to separate, affecting the electrochemical performance, and even causing short circuits and serious safety problems. In addition, some flexible batteries are affected by the electrodes, which limits the bending ability of the battery and can only bend in the same direction at a small angle and small curvature. At the same time, there are also disadvantages such as complex production process, single shape, and low energy density.
[0003] Chinese patent application CN117832653A discloses a wearable flexible zinc-ion battery and a preparation method thereof, wherein the wearable flexible zinc-ion battery has a scorpion tail structure, the thick stack formed by the winding part on the trunk is similar to the tail section of the scorpion tail, and the non-winding part on the trunk connects the thick layer stacking of the tail section of the scorpion tail, and the non-winding part on the trunk greatly improves the battery flexibility by sacrificing a small part of the battery capacity, and the stacking part can store more energy, which can meet people's requirements for the daily endurance of wearable flexible devices; the wearable flexible zinc-ion battery with the scorpion tail structure is subjected to a smaller maximum principal stress during the deformation process, indicating that the structure can better withstand the life damage caused by bending deformation, which is conducive to the battery maintaining a stable cycle performance and extending the service life of the battery. Chinese patent application CN117747903A discloses a flexible battery pack and a preparation method thereof, and the preparation of a flexible battery pack is realized by using a flexible circuit board with a copper substrate and aluminum-plated wiring as a flexible substrate. However, these related technologies are all to make the battery as flexible as possible, but cannot realize the preparation of batteries of various shapes. If the battery can be freely designed in shape, it will be very convenient for the application of the battery. According to the design of the internal space of the electronic product, a larger capacity battery can be configured in an irregular space. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a flexible battery with freely designed shape and a preparation method, which uses flexible fiber electrodes as a substrate and satisfies different shape requirements through the free arrangement of flexible electrodes, thereby realizing the free design of the battery's appearance.
[0005] The technical solution of the present invention to solve the above technical problem is as follows: a method for preparing a flexible battery with a freely designed shape, the preparation method is:
[0006] S1, using aluminum-plated aramid as a positive electrode current collector, and uniformly coating a positive electrode material on the positive electrode current collector to obtain a positive electrode, using copper-plated aramid as a negative electrode current collector, and uniformly coating a negative electrode material on the negative electrode current collector to obtain a negative electrode;
[0007] S2. Wrap one of the negative electrode or the positive electrode with a diaphragm, then assemble the negative electrode and the positive electrode to obtain fibrous positive and negative electrodes, arrange the fibrous positive and negative electrodes according to the required battery shape, and connect the positive and negative electrodes of the fibrous positive and negative electrodes to the pole ears respectively; then load them into a packaging shell of corresponding shape, and inject gel electrolyte; finally, completely seal the shell to obtain the required flexible battery.
[0008] Furthermore, the fiber of the aluminum-coated aramid is 200D-400D, and the coating amount of the positive electrode material on the aluminum-coated aramid is 140-180 mg / m.
[0009] Furthermore, the aluminum-coated aramid fiber is A , unit is D; the coating amount of the positive electrode material on the aluminum-plated aramid is B , the unit is mg / m; B = b ±5, b =0.2 A +100.
[0010] Furthermore, the copper-plated aramid fiber is 200D-400D, and the coating amount of the negative electrode material on the copper-plated aramid is 60-90 mg / m.
[0011] Furthermore, the copper-plated aramid fiber is A’ , unit is D; the coating amount of the negative electrode material on the copper-plated aramid is B’ , the unit is mg / m; B’ = b’ ±5, b’ =0.15 A’ +30.
[0012] Furthermore, the packaging shell material is an aluminum-plastic film, and the thickness of the aluminum-plastic film is 60-150 μm.
[0013] Furthermore, the fibrous positive and negative electrodes are prepared by wrapping one of the positive electrode and the negative electrode with a separator, and then winding, twisting or arranging a single or multiple positive electrodes and negative electrodes together.
[0014] Furthermore, the positive electrode material includes lithium cobalt oxide, a conductive agent and a binder, the binder is polyvinylidene fluoride, and the mass ratio of the lithium cobalt oxide, the conductive agent and the binder is (90-95): (2-5): (3-5).
[0015] Furthermore, the negative electrode material includes graphite, a conductive agent and a binder, the binder is sodium carboxymethyl cellulose and styrene-butadiene rubber, the mass ratio of the graphite, the conductive agent and the binder is (95.5-97): (1-2): (2-2.5), and the mass ratio of the sodium carboxymethyl cellulose and styrene-butadiene rubber is (0.8-1): (1.2-1.5).
[0016] A flexible battery with a freely designable shape is prepared according to the preparation method of the present invention.
[0017] The beneficial effects of the present invention are:
[0018] The flexible battery of the present invention uses aluminum-plated aramid and copper-plated aramid as positive and negative current collectors of the fiber battery. After coating, the positive and negative electrodes are more flexible and can be folded in half, providing a good basis for designing flexible batteries. With flexible fiber electrodes as the matrix, the free arrangement of flexible fiber electrodes can meet different shape requirements, and the shape of the battery can be freely designed, including irregular and asymmetric shapes, and can also realize the design of irregular shapes at the three-dimensional level.
[0019] The battery prepared by the preparation method of the present invention has good flexibility and can be bent multiple times to different degrees and in different directions / angles; compared with traditional flexible batteries, the flexible battery of the present invention has higher energy density. Moreover, the preparation method of the present invention can configure a battery with a larger capacity in an irregular space according to the different designs of the internal space of the electronic product.
[0020] In the flexible battery preparation method described in the present invention, by controlling the relationship between the aluminum-plated aramid / copper-plated aramid fiber and the coating amount of the coating material, it is more conducive to making the fibrous positive and negative electrodes meet various bending requirements (the bending radius can be less than 0.5m, and the bending angle can reach 360°), thereby meeting the processing requirements of freely designed shape batteries.
[0021] The flexible battery of the present invention is based on gel electrolyte, does not catch fire or explode after being punctured, and has good safety. The lubricating effect of the gel electrolyte can reduce the mutual friction force of the fiber electrodes when the flexible battery is deformed. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a front view of the flexible battery in Example 1 of the present invention;
[0023] Figure 2 This is a front view of the flexible battery in Example 2 of the present invention;
[0024] Figure 3 This is a front view of the flexible battery in Example 3 of the present invention;
[0025] Figure 4This is a front view of the flexible battery in Example 4 of the present invention;
[0026] Figure 5 This is a front view of the flexible battery in Example 5 of the present invention;
[0027] Figure 6 This is a front view of the flexible battery in Example 6 of the present invention;
[0028] In the figure, 1. Fibrous positive and negative electrodes; 2. Packaging shell; 3. Tabs. DETAILED DESCRIPTION
[0029] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0031] A method for preparing a flexible battery with a freely designable shape, characterized in that the preparation method comprises:
[0032] S1, using aluminum-plated aramid as a positive electrode current collector, and uniformly coating a positive electrode material on the positive electrode current collector to obtain a positive electrode, using copper-plated aramid as a negative electrode current collector, and uniformly coating a negative electrode material on the negative electrode current collector to obtain a negative electrode;
[0033] S2. Wrap one of the negative electrode or the positive electrode with a diaphragm, then assemble the negative electrode and the positive electrode to obtain fibrous positive and negative electrodes 1, arrange the fibrous positive and negative electrodes 1 according to the required battery shape, and connect the positive electrode and the negative electrode of the fibrous positive and negative electrodes 1 to the pole ears 3 respectively; then load them into a packaging shell 2 of corresponding shape, and inject gel electrolyte; finally, completely seal the shell to obtain the required flexible battery.
[0034] Specifically, the fiber of the aluminum-coated aramid is 200D-400D, and the coating amount of the positive electrode material on the aluminum-coated aramid is 140-180 mg / m.
[0035] Specifically, the aluminum-coated aramid fiber is A , unit is D; the coating amount of the positive electrode material on the aluminum-plated aramid is B , the unit is mg / m; B = b ±5, b =0.2 A +100.
[0036] Specifically, the copper-plated aramid fiber is 200D-400D, and the coating amount of the negative electrode material on the copper-plated aramid fiber is 60-90 mg / m.
[0037] Specifically, the copper-plated aramid fiber is A’ , unit is D; the coating amount of the negative electrode material on the copper-plated aramid is B’ , the unit is mg / m; B’ = b’ ±5, b’ =0.15 A’ +30.
[0038] Specifically, the packaging shell 2 is made of an aluminum-plastic film, and the thickness of the aluminum-plastic film is 60-150 μm.
[0039] Specifically, the fibrous positive and negative electrodes 1 are prepared by wrapping one of the positive electrode and the negative electrode with a separator, and then winding, twisting or arranging a single or multiple positive electrodes and negative electrodes with each other.
[0040] Specifically, the fibrous positive and negative electrodes 1 of the flexible battery can be divided into several small pieces, which can be connected in parallel or in series.
[0041] Specifically, the fiber-shaped positive and negative electrodes 1 of the flexible battery can be freely deformed and arranged into different shapes: polygonal, circular, elliptical and other irregular shapes.
[0042] Specifically, the fiber electrodes arranged in a predetermined shape can be stacked in parallel in 1 to 10 layers, and the thickness of the finished battery is 2 to 32 mm.
[0043] Specifically, the material of the packaging shell 2 used in the embodiment of the present invention is an aluminum-plastic film, and the thickness of the aluminum-plastic film is 60-150 μm.
[0044] More specifically, the aluminum-plated aramid fiber in the embodiment of the present invention is 200D-400D, the copper-plated aramid fiber is 200D-400D, and the DC resistance value is less than 5Ω / m. The aluminum-plated aramid and the copper-plated aramid can be directly purchased.
[0045] More specifically, the gel electrolyte used in the embodiment of the present invention is obtained by adding 2% to 6% by mass of ethylene glycol dimethacrylate to lithium hexafluorophosphate and mixing them evenly.
[0046] Specifically, the positive electrode material includes lithium cobalt oxide, a conductive agent and a binder, the binder is polyvinylidene fluoride, and the mass ratio of the lithium cobalt oxide, the conductive agent and the binder is (90-95): (2-5): (3-5).
[0047] Specifically, the negative electrode material includes graphite, a conductive agent and a binder, the binder is sodium carboxymethyl cellulose and styrene-butadiene rubber, the mass ratio of the graphite, the conductive agent and the binder is (95.5-97): (1-2): (2-2.5), and the mass ratio of the sodium carboxymethyl cellulose and styrene-butadiene rubber is (0.8-1): (1.2-1.5).
[0048] More specifically, the positive electrode material is added to the solvent, and the positive electrode slurry is prepared by a slurry mixing device, and then the positive electrode slurry is coated on the surface of the aluminum-plated aramid fiber; the negative electrode material is added to the solvent, and the negative electrode slurry is prepared by a slurry mixing device, and then the negative electrode slurry is coated on the surface of the copper-plated aramid fiber. The stirring speed of the slurry mixing device is 20 rpm, and the dispersion speed is 1300 rpm.
[0049] More specifically, in the embodiment of the present invention, the conductive agent is conductive carbon black (TIMCAL, model MA-EN-CO-0005), the graphite is commercial graphite (Canrd, model MA-EN-AN-0017), the polyvinylidene fluoride is purchased from Canrd, model PVDF 900; the styrene-butadiene rubber is purchased from Canrd, model TRD.
[0050] Example 1
[0051] (1) Commercial lithium cobalt oxide, conductive agent (conductive carbon black) and binder (polyvinylidene fluoride) were added to a solvent (N-methylpyrrolidone) at a mass ratio of 90:5:5, and the positive electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 330 min. After the slurry mixing was completed, the viscosity of the positive electrode slurry was tested to be 55000 mPa.s.
[0052] (2) The positive electrode slurry of step (1) was coated on the surface of dried aluminum-coated aramid (fiber 300D) and dried to obtain a positive electrode with a coating weight of 160 mg / m2.
[0053] (3) Commercial graphite, conductive agent (conductive carbon black) and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber) were added to the solvent (N-methylpyrrolidone) in a mass ratio of 95.5:2:(1:1.5), and the negative electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 390 min. After the slurry mixing was completed, the viscosity of the negative electrode slurry was tested to be 49700 mPa.s.
[0054] (4) The negative electrode slurry of step (3) was coated on the surface of dried copper-plated aramid fiber (fiber 300D) to obtain a negative electrode with a coating weight of 80 mg / m.
[0055] (5) Wrap the negative electrode obtained in step (4) with a diaphragm, and the wrapped negative electrode can be twisted with the positive electrode obtained in step (2) to obtain fibrous positive and negative electrodes 1.
[0056] (6) Arrange the fiber-shaped positive and negative electrodes 1 prepared in step (5) in a zigzag pattern as follows: Figure 1 The structural shape shown.
[0057] (7) Connect the positive and negative electrodes of the fibrous positive and negative electrodes 1 to the electrode tabs 3 respectively.
[0058] (8) Place the converted battery into an aluminum-plastic film (100 μm thick) of corresponding shape and inject gel electrolyte.
[0059] (9) After complete sealing, the desired flexible battery is obtained.
[0060] Example 2
[0061] (1) Commercial lithium cobalt oxide, conductive agent (conductive carbon black) and binder (polyvinylidene fluoride) were added to a solvent (N-methylpyrrolidone) at a mass ratio of 90:5:5, and the positive electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 330 min. After the slurry mixing was completed, the viscosity of the positive electrode slurry was tested to be 55000 mPa.s.
[0062] (2) The positive electrode slurry of step (1) was coated on the surface of dried aluminum-coated aramid (fiber is 200D) and dried to obtain a positive electrode with a coating weight of 140 mg / m2.
[0063] (3) Commercial graphite, conductive agent (conductive carbon black) and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber) were added to the solvent (N-methylpyrrolidone) in a mass ratio of 95.5:2:(1:1.5), and the negative electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 390 min. After the slurry mixing was completed, the viscosity of the negative electrode slurry was tested to be 49700 mPa.s.
[0064] (4) The negative electrode slurry of step (3) was coated on the surface of dried copper-plated aramid fiber (fiber 400D) to a negative electrode with a coating weight of 90 mg / m.
[0065] (5) Wrap the negative electrode obtained in step (4) with a diaphragm, and the wrapped negative electrode can be twisted with the positive electrode obtained in step (2) to obtain fibrous positive and negative electrodes 1.
[0066] (6) Arrange the fiber-shaped positive and negative electrodes 1 prepared in step (5) in a zigzag pattern as follows: Figure 2 The structural shape shown.
[0067] (7) The positive and negative electrodes of the fibrous positive and negative electrodes 1 are connected to the tabs 3 respectively, and the tabs 3 are located at adjacent positions on the same side of the battery.
[0068] (8) Place the converted battery into an aluminum-plastic film (150 μm thick) of corresponding shape and inject gel electrolyte.
[0069] (9) After complete sealing, the desired flexible battery is obtained.
[0070] Example 3
[0071] (1) Commercial lithium cobalt oxide, conductive agent (conductive carbon black) and binder (polyvinylidene fluoride) were added to a solvent (N-methylpyrrolidone) at a mass ratio of 90:5:5, and the positive electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 330 min. After the slurry mixing was completed, the viscosity of the positive electrode slurry was tested to be 55000 mPa.s.
[0072] (2) The positive electrode slurry of step (1) is coated on the surface of dried aluminum-coated aramid (fiber is 400D) and dried to obtain a positive electrode with a coating weight of 180 mg / m2.
[0073] (3) Commercial graphite, conductive agent (conductive carbon black) and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber) were added to the solvent (N-methylpyrrolidone) in a mass ratio of 95.5:2:(1:1.5), and the negative electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 390 min. After the slurry mixing was completed, the viscosity of the negative electrode slurry was tested to be 49700 mPa.s.
[0074] (4) The negative electrode slurry of step (3) was coated on the surface of dried copper-plated aramid fiber (fiber 200D) to obtain a negative electrode with a coating weight of 60 mg / m.
[0075] (5) Wrap the negative electrode obtained in step (4) with a diaphragm, and the wrapped negative electrode can be twisted with the positive electrode obtained in step (2) to obtain fibrous positive and negative electrodes 1.
[0076] (6) Arrange the fiber-shaped positive and negative electrodes 1 prepared in step (5) in a zigzag pattern as follows: Figure 3 The structural shape shown.
[0077] (7) Connect the positive and negative electrodes of the fibrous positive and negative electrodes 1 to the electrode tabs 3 respectively.
[0078] (8) Place the converted battery into an aluminum-plastic film (60 μm thick) of the corresponding shape and inject gel electrolyte.
[0079] (9) After complete sealing, the desired flexible battery is obtained.
[0080] Example 4
[0081] (1) Commercial lithium cobalt oxide, conductive agent (conductive carbon black) and binder (polyvinylidene fluoride) were added to a solvent (N-methylpyrrolidone) at a mass ratio of 95:2:3, and the positive electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 330 min. After the slurry mixing was completed, the viscosity of the positive electrode slurry was tested to be 36000 mPa.s.
[0082] (2) The positive electrode slurry of step (1) was coated on the surface of dried aluminum-coated aramid (fiber 300D) and dried to obtain a positive electrode with a coating weight of 160 mg / m2.
[0083] (3) Commercial graphite, conductive agent (conductive carbon black) and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber) were added to the solvent (N-methylpyrrolidone) in a mass ratio of 97:1:(0.8:1.2), and the negative electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 390 min. After the slurry mixing was completed, the viscosity of the negative electrode slurry was tested to be 35000 mPa.s.
[0084] (4) The negative electrode slurry of step (3) was coated on the surface of dried copper-plated aramid fiber (fiber 300D) to obtain a negative electrode with a coating weight of 80 mg / m.
[0085] (5) Wrap the negative electrode obtained in step (4) with a diaphragm, and the wrapped negative electrode can be twisted with the positive electrode obtained in step (2) to obtain fibrous positive and negative electrodes 1.
[0086] (6) Arrange the fiber-shaped positive and negative electrodes 1 prepared in step (5) in a zigzag pattern as follows: Figure 4 The structural shape shown.
[0087] (7) Connect the positive and negative electrodes of the fibrous positive and negative electrodes 1 to the electrode tabs 3 respectively.
[0088] (8) Place the converted battery into an aluminum-plastic film (100 μm thick) of corresponding shape and inject gel electrolyte.
[0089] (9) After complete sealing, the desired flexible battery is obtained.
[0090] Example 5
[0091] (1) Commercial lithium cobalt oxide, conductive agent (conductive carbon black) and binder (polyvinylidene fluoride) were added to a solvent (N-methylpyrrolidone) at a mass ratio of 90:5:5, and the positive electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 330 min. After the slurry mixing was completed, the viscosity of the positive electrode slurry was tested to be 55000 mPa.s.
[0092] (2) The positive electrode slurry of step (1) is coated on the surface of dried aluminum-coated aramid (fiber is 400D) and dried to obtain a positive electrode with a coating weight of 180 mg / m2.
[0093] (3) Commercial graphite, conductive agent (conductive carbon black) and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber) were added to the solvent (N-methylpyrrolidone) in a mass ratio of 95.5:2:(1:1.5), and the negative electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 390 min. After the slurry mixing was completed, the viscosity of the negative electrode slurry was tested to be 49700 mPa.s.
[0094] (4) The negative electrode slurry of step (3) was coated on the surface of dried copper-plated aramid fiber (fiber 200D) to obtain a negative electrode with a coating weight of 60 mg / m.
[0095] (5) Wrap the negative electrode obtained in step (4) with a diaphragm, and the wrapped negative electrode can be twisted with the positive electrode obtained in step (2) to obtain fibrous positive and negative electrodes 1.
[0096] (6) Arrange the fiber-shaped positive and negative electrodes 1 prepared in step (5) in a zigzag pattern as follows: Figure 5 The structural shape shown.
[0097] (7) Connect the positive and negative electrodes of the fibrous positive and negative electrodes 1 to the electrode tabs 3 respectively.
[0098] (8) Place the converted battery into an aluminum-plastic film (100 μm thick) of corresponding shape and inject gel electrolyte.
[0099] (9) After complete sealing, the desired flexible battery is obtained.
[0100] Example 6
[0101] (1) Commercial lithium cobalt oxide, conductive agent (conductive carbon black) and binder (polyvinylidene fluoride) were added to a solvent (N-methylpyrrolidone) at a mass ratio of 90:5:5, and the positive electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 330 min. After the slurry mixing was completed, the viscosity of the positive electrode slurry was tested to be 55000 mPa.s.
[0102] (2) The positive electrode slurry of step (1) was coated on the surface of dried aluminum-coated aramid (fiber 300D) and dried to obtain a positive electrode with a coating weight of 160 mg / m2.
[0103] (3) Commercial graphite, conductive agent (conductive carbon black) and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber) were added to the solvent (N-methylpyrrolidone) in a mass ratio of 95.5:2:(1:1.5), and the negative electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 20 rpm, the dispersion speed was 1300 rpm, and the slurry mixing time was 390 min. After the slurry mixing was completed, the viscosity of the negative electrode slurry was tested to be 49700 mPa.s.
[0104] (4) The negative electrode slurry of step (3) was coated on the surface of dried copper-plated aramid fiber (fiber 200D) to obtain a negative electrode with a coating weight of 60 mg / m.
[0105] (5) Wrap the negative electrode obtained in step (4) with a diaphragm, and the wrapped negative electrode can be twisted with the positive electrode obtained in step (2) to obtain fibrous positive and negative electrodes 1.
[0106] (6) Arrange the fiber-shaped positive and negative electrodes 1 prepared in step (5) in a zigzag pattern as follows: Figure 6 The structural shape shown.
[0107] (7) The positive and negative electrodes of the fibrous positive and negative electrodes 1 are connected to the tabs 3 respectively, and the tabs 3 are located at adjacent positions on the same side of the battery.
[0108] (8) Place the converted battery into an aluminum-plastic film (100 μm thick) of corresponding shape and inject gel electrolyte.
[0109] (9) After complete sealing, the desired flexible battery is obtained.
[0110] Comparative Example 1
[0111] The flexible battery was prepared by the same method as in Example 1, except that the coating amount of the positive electrode slurry was increased. In step (2), the coating amount of the positive electrode material was 180 mg / m. B = b ±5, b =0.2 A +100 rule).
[0112] Comparative Example 2
[0113] The flexible battery was prepared by the same method as in Example 1, except that the coating amount of the negative electrode slurry was increased. In step (2), the coating amount of the negative electrode material was 90 mg / m. (Not in accordance with the requirements of the present invention)B’ = b’ ±5, b’ =0.15 A’ +30 rule).
[0114] Comparative Example 3
[0115] The flexible battery was prepared by the same method as in Example 1, except that the slurry treatment conditions in step (1) and step (3) were adjusted to increase the stirring speed and the dispersion speed. The specific process is as follows:
[0116] (1) Commercial lithium cobalt oxide, conductive agent (conductive carbon black) and binder (polyvinylidene fluoride) were added to a solvent (N-methylpyrrolidone) at a mass ratio of 90:5:5, and the positive electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 40 rpm, the dispersion speed was 1600 rpm, and the slurry mixing time was 330 min. After the slurry mixing was completed, the viscosity of the positive electrode slurry was tested to be 28000 mPa.s.
[0117] (2) The positive electrode slurry of step (1) was coated on the surface of dried aluminum-coated aramid (fiber 300D) and dried to obtain a positive electrode with a coating weight of 160 mg / m2.
[0118] (3) Commercial graphite, conductive agent (conductive carbon black) and binder (sodium carboxymethyl cellulose and styrene-butadiene rubber) were added to the solvent (N-methylpyrrolidone) in a mass ratio of 95.5:2:(1:1.5), and the negative electrode slurry was prepared by a slurry mixing equipment. The stirring speed of the slurry mixing was 40 rpm, the dispersion speed was 1600 rpm, and the slurry mixing time was 390 min. After the slurry mixing was completed, the viscosity of the negative electrode slurry was tested to be 27500 mPa.s.
[0119] (4) The negative electrode slurry of step (3) was coated on the surface of dried copper-plated aramid fiber (fiber 300D) to obtain a negative electrode with a coating weight of 80 mg / m.
[0120] (5) Wrap the negative electrode obtained in step (4) with a diaphragm, and the wrapped negative electrode can be twisted with the positive electrode obtained in step (2) to obtain fibrous positive and negative electrodes 1.
[0121] (6) Arrange the fiber-shaped positive and negative electrodes 1 prepared in step (5) in a zigzag pattern as follows: Figure 1 The structural shape shown.
[0122] (7) Connect the positive and negative electrodes of the fibrous positive and negative electrodes 1 to the electrode tabs 3 respectively.
[0123] (8) Place the converted battery into an aluminum-plastic film (115 μm thick) of the corresponding shape and inject gel electrolyte.
[0124] (9) After complete sealing, the desired flexible battery is obtained.
[0125] The flexible batteries prepared in the above embodiments and comparative examples were subjected to performance tests, and the test method involved was: using a blue electric tester to measure the charge and discharge performance, with a charge rate of 0.1C, a discharge rate of 0.2C, and a cut-off voltage of 3.0-4.4V. The flexible battery performance test results are shown in Table 1 below.
[0126] Table 1 Flexible battery performance test results
[0127]
[0128] It can be seen from the data in the above table that Examples 1-6 can prepare flexible batteries with various shape requirements using the preparation method of the present invention. The flexible batteries have high specific capacity, coulombic efficiency and charge and discharge performance. The appropriate coating process ensures the flexibility of the fiber electrode and the stability of the coating layer. During use, the coating layer will not crack or fall off.
[0129] From the data comparison between Comparative Example 1 and Example 1, it can be seen that if the coating amount of the aluminum-coated aramid fiber and the positive electrode material does not match, the thickness of the coating layer will increase, and the mutual bonding force will be weakened, resulting in partial cracking and falling off of the coating layer, thereby affecting the overall capacity performance of the battery.
[0130] From the data comparison between Comparative Example 2 and Example 1, it can be seen that if the coating amount of the copper-plated aramid fiber and the negative electrode material does not match, the thickness of the coating will increase, the mutual bonding force will be weakened, and part of the coating layer will crack and fall off, thereby affecting the overall capacity performance of the battery.
[0131] From the comparison of the data of Comparative Example 3 and Example 1, it can be seen that if the stirring speed and the dispersion speed are too fast during the preparation of the positive electrode slurry or the negative electrode slurry, the viscosity of the slurry will be reduced. The lower viscosity will cause problems such as breakage, particle aggregation and uneven coating thickness during the coating process, resulting in large-scale shedding of the coating layer of the fiber electrode during use, thereby affecting the overall performance of the battery and making it impossible to prepare a flexible battery with freely designed shape.
[0132] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0133] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A method for preparing a flexible battery with freely designed shape, It is characterized in that The preparation method is: S1, using aluminum-plated aramid as a positive electrode current collector, and uniformly coating a positive electrode material on the positive electrode current collector to obtain a positive electrode, using copper-plated aramid as a negative electrode current collector, and uniformly coating a negative electrode material on the negative electrode current collector to obtain a negative electrode; S2, wrapping one of the negative electrode or the positive electrode with a diaphragm, and then assembling the negative electrode and the positive electrode to obtain fibrous positive and negative electrodes, arranging the fibrous positive and negative electrodes according to the required battery shape, and connecting the positive electrode and the negative electrode of the fibrous positive and negative electrodes to the tabs respectively; Then, it is placed in a packaging shell of corresponding shape and injected with gel electrolyte; finally, the desired flexible battery is obtained after it is completely sealed; The aluminum-coated aramid fiber is 200D-400D, and the coating amount of the positive electrode material on the aluminum-coated aramid fiber is 140-180 mg / m; the aluminum-coated aramid fiber is A , unit is D; the coating amount of the positive electrode material on the aluminum-plated aramid is B , the unit is mg / m; B = b ±5, b =0.2 A +100; The copper-plated aramid fiber is 200D-400D, and the coating amount of the negative electrode material on the copper-plated aramid fiber is 60-90 mg / m; the copper-plated aramid fiber is A’ , unit is D; the coating amount of the negative electrode material on the copper-plated aramid is B’ , the unit is mg / m; B’ = b’ ±5, b’ =0.15 A’ +30.
2. A method for preparing a flexible battery with a freely designable shape according to claim 1, It is characterized in that The packaging shell material is an aluminum-plastic film, and the thickness of the aluminum-plastic film is 60-150 μm.
3. A method for preparing a flexible battery with a freely designable shape according to claim 1, It is characterized in that The fiber-shaped positive and negative electrodes are prepared by wrapping one of the positive electrode and the negative electrode with a separator, and then winding, twisting or arranging a single or multiple positive electrodes and negative electrodes with each other.
4. A method for preparing a flexible battery with a freely designable shape according to claim 1, It is characterized in that The positive electrode material comprises lithium cobalt oxide, a conductive agent and a binder, wherein the binder is polyvinylidene fluoride, and the mass ratio of the lithium cobalt oxide, the conductive agent and the binder is (90-95): (2-5): (3-5).
5. A method for preparing a flexible battery with a freely designable shape according to claim 1, It is characterized in that The negative electrode material comprises graphite, a conductive agent and a binder, wherein the binder is sodium carboxymethyl cellulose and styrene-butadiene rubber, the mass ratio of the graphite, the conductive agent and the binder is (95.5-97):(1-2):(2-2.5), and the mass ratio of the sodium carboxymethyl cellulose and styrene-butadiene rubber is (0.8-1):(1.2-1.5).
6. A flexible battery with freely designed shape, It is characterized in that The flexible battery is prepared according to the preparation method according to any one of claims 1 to 5.