A kind of porous ceramic microbead and preparation method thereof

By using specific raw materials and adhesives, the method addresses high energy consumption and environmental impact in ceramic microbead production, achieving cost-effective, sustainable, and high-quality porous ceramic microbeads with improved plasticity and sphericity.

CN118652103BActive Publication Date: 2024-12-03XINYANG YONGKAI THERMAL INSULATION MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411154451.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The high energy consumption and carbon emissions associated with the production of porous ceramic microbeads due to the need for high-temperature foaming processes, along with the poor plasticity and sphericity of microbeads using clay as a sintering aid, hinder industrial scalability and environmental sustainability.

Method used

A method involving the use of fly ash, perlite tailings, sludge, or aluminum ash as raw materials, glass powder as a sintering aid, and ammonium bicarbonate or yeast powder as a foaming agent, combined with a specially prepared adhesive made from citric acid and magnesium-based compounds, to achieve foaming at lower temperatures (110°C to 130°C) and sintering at 700°C to 900°C, resulting in porous ceramic microbeads with improved plasticity and sphericity.

Benefits of technology

The method significantly reduces energy consumption and production costs while enhancing the sphericity and mechanical strength of porous ceramic microbeads, making them suitable for industrial production and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652103B_ABST
    Figure CN118652103B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of thermal insulation materials, specifically a porous ceramic microbead and a preparation method thereof, first preparing an adhesive, that is, mixing a citric acid solution and a magnesium-based compound in proportion; then placing the precipitated magnesium carboxylate obtained after the reaction in an oven, and heat treating it at 180-200°C for not less than 10 hours; mixing the heat-treated magnesium carboxylate with boric acid in a mass ratio of 4:1 to obtain an adhesive for preparing porous ceramic microbeads by a foaming method, and then mixing the adhesive with ceramic microbead raw materials, a sintering aid and a foaming agent, and then adding water thereto, granulating it through a granulator, and foaming it at 110-130°C for more than 10 minutes, and finally sintering it at a certain temperature to obtain porous ceramic microbeads. The prepared adhesive can greatly reduce the foaming temperature of the porous microbeads, effectively reduce production costs, and improve production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal insulation materials, in particular to porous ceramic microbeads and a preparation method thereof. Background Art

[0002] Porous ceramic microbeads are a new type of lightweight ceramic material with a porous structure inside and a dense glaze layer on the surface. They have the characteristics of low density, high strength, excellent thermal insulation and adsorption properties, and are widely used in high-performance thermal insulation materials, acoustic absorption and shock absorption, chemical catalyst carriers and special building materials. Porous ceramic microbeads use mine tailings or industrial waste as the main raw materials, and add a small amount of organic matter, carbonate and silicon carbide as high-temperature foaming agents. During the sintering process, when the temperature rises to between 1000℃-1300℃, some minerals begin to melt to form a liquid phase with appropriate viscosity. The liquid phase effectively blocks the pores on the surface of the microbeads, prevents the escape of internal gas, and gives the microbeads a certain plasticity. At this time, the foaming agent in the raw material releases gas (such as CO2, H2O, etc.), which causes the volume of the microbeads to expand, thus forming ceramic microbeads with a porous structure.

[0003] The preparation of porous ceramic microspheres usually needs to be carried out at a relatively high temperature, resulting in huge energy consumption in the entire production process, with energy consumption costs accounting for 85% of the total cost. Large amounts of energy demand usually rely on fossil fuels such as coal and natural gas, which not only increases production costs, but also causes a large amount of carbon emissions, which has a significant negative impact on the environment. In the context of the "dual carbon" goals, the development of low-temperature foaming technology has important practical significance for the production of porous ceramic microspheres. By using low-temperature foaming agents, not only can energy consumption and production costs be significantly reduced, but carbon emissions can also be reduced, driving the entire industry towards environmental protection and energy conservation.

[0004] The key to developing low-temperature foaming technology is how to make the microbead body form a liquid phase with appropriate viscosity at a lower temperature to obtain better plasticity. At present, the common practice is to add clay to the raw materials to give the microbead body a certain plasticity, and use microwave rapid heating to prepare porous ceramic body microbeads. However, the plasticity of the body given by clay is poor, resulting in the prepared porous microbeads being mostly apparent pores and poor sphericity. This technology is difficult to meet the requirements of industrial production. Dong Cheng et al. used fly ash as the main raw material, kaolin, quicklime and glass powder as auxiliary raw materials, and successfully prepared porous ceramic microbeads by microwave foaming. However, the apparent porosity of the porous ceramic microbeads was as high as 60%. Summary of the invention

[0005] To solve the above problems, the object of the present invention is to provide a method for preparing porous ceramic microbeads, which is as follows: ceramic microbead raw materials, adhesives, sintering aids and foaming agents are uniformly mixed, water is added thereto, granulated and sieved by a granulator to obtain ceramic microbead green bodies, the ceramic microbead green bodies are foamed at 110°C to 130°C for more than 10 minutes, and finally, sintered at 700°C to 900°C to obtain porous ceramic microbeads.

[0006] Furthermore, the raw material of the ceramic microbeads includes at least one of fly ash, perlite tailings, sludge, and aluminum ash.

[0007] Furthermore, the sintering aid is glass powder, which functions to reduce the temperature at which the liquid phase is formed.

[0008] Furthermore, the foaming agent includes at least one of ammonium bicarbonate, washing powder and yeast powder.

[0009] Furthermore, the mass of the added water is 18% to 60% of the total mass of the ceramic microsphere raw material, the binder, the sintering aid and the foaming agent.

[0010] Furthermore, the granulator is one of an extrusion granulator, a drum granulator, and a spray drying granulator.

[0011] The foaming mechanism occurs at 110℃~130℃. At this temperature, the magnesium carboxylate softens after heat treatment, giving the ceramic microspheres plasticity. At the same time, the foaming agent decomposes to produce a large amount of gas, which prompts the ceramic microspheres to form a porous structure. In addition, the heat-treated magnesium carboxylate undergoes an esterification reaction with boric acid to form a network structure of magnesium carboxylate borate, which gives the porous ceramic microspheres mechanical strength.

[0012] Furthermore, the adhesive is prepared by the following method: first, a citric acid solution and a magnesium-based compound are mixed and reacted in proportion, the reaction time is not less than 1 hour, the solution obtained after the reaction is placed in an oven, and heat-treated at 180-200° C. for not less than 10 hours to obtain a solid product, that is, magnesium carboxylate after heat treatment; then, the heat-treated product is mixed with boric acid at a mass ratio of 4:1, and finally an adhesive for preparing porous ceramic microspheres by a foaming method is obtained;

[0013] Furthermore, in the preparation of the adhesive, the citric acid solution is obtained by mixing citric acid monohydrate and deionized water in a mass ratio of 4:5, and heating in a water bath to 75-85° C. to fully dissolve the citric acid;

[0014] Furthermore, in the preparation of the adhesive, the magnesium-based compound is one of light-burned magnesium oxide, magnesium hydroxide or magnesium carbonate;

[0015] Furthermore, in the preparation of the adhesive, the mixing ratio of the citric acid solution and the magnesium-based compound means that when the magnesium-based compound is light-burned magnesium oxide, the mass ratio of the citric acid solution to the light-burned magnesium oxide is 1:0.29; when the magnesium-based compound is magnesium hydroxide, the mass ratio of the citric acid solution to the magnesium hydroxide is 1:0.41; when the magnesium-based compound is magnesium carbonate, the mass ratio of the citric acid solution to the magnesium carbonate is 1:0.55.

[0016] Furthermore, in the preparation of the adhesive, the citric acid solution and the magnesium-based compound react to generate a white precipitate, which is magnesium carboxylate;

[0017] Furthermore, in the preparation of the adhesive, the heat-treated magnesium carboxylate is in powder form.

[0018] The purpose of the heat treatment is to remove the crystal water and free water in the reaction product magnesium carboxylate, so that it has bonding properties; the bonding mechanism of the adhesive means that magnesium carboxylate will form magnesium carboxylate containing crystal water with bonding properties when it meets water at room temperature.

[0019] The present invention also provides a porous ceramic micro-bead obtained according to the above preparation method. The porous ceramic micro-bead has a porous structure inside and a dense glaze layer is covered on the surface.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The porous ceramic microbeads prepared by the present invention adopt a specially prepared adhesive, which can significantly reduce the foaming temperature and production cost, has the function of imparting plasticity to the porous ceramic microbead blank, and has the function of imparting strength to the porous ceramic microbead blank, can improve the sphericity of the porous ceramic microbeads, has the advantages of low apparent porosity and low bulk density, is suitable for industrial production, is environmentally friendly and non-toxic, and has a wide range of uses, and can be used to prepare coal ash porous ceramic microbeads, red mud porous ceramic microbeads, tailings porous ceramic microbeads, sludge porous ceramic microbeads, garbage porous ceramic microbeads, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The macroscopic image and SEM image of magnesium carboxylate after heat treatment in the process of preparing the adhesive in Example 1 of the present invention, wherein the image marked as (a) in the upper left corner is the macroscopic image, and the image marked as (b) in the upper left corner is the SEM image;

[0023] Figure 2 The XRD spectrum and infrared spectrum of magnesium carboxylate after heat treatment in the process of preparing the adhesive in Example 1 of the present invention, wherein the upper left corner marked with (a) is the XRD spectrum, and the upper left corner marked with (b) is the infrared spectrum;

[0024] Figure 3The XRD spectra and infrared spectra of the hydration product of the magnesium carboxylate after heat treatment and the hydration product of the prepared adhesive in Example 1 of the present invention are shown in FIG. 1 , wherein the XRD spectra are shown in the upper left corner as (a), and the infrared spectra are shown in the upper left corner as (b);

[0025] Figure 4 is the viscosity value of the hydration product of the adhesive prepared in Example 1 of the present invention at room temperature and 110° C.;

[0026] Figure 5 These are macroscopic images of porous ceramic microbeads prepared in Example 2 and Comparative Example 1, respectively, wherein the one marked with (a) in the upper left corner is prepared in Comparative Example 1, and the one marked with (b) in the upper left corner is prepared in Example 2. DETAILED DESCRIPTION

[0027] In order to better understand the content of the present invention, the present invention will be further described below in conjunction with specific embodiments and drawings. The following embodiments are implemented based on the technology of the present invention, and detailed implementation methods and operating steps are given, but the protection scope of the present invention is not limited to the following embodiments.

[0028] In the embodiments and comparative examples, the single particle strength of the porous ceramic microbeads is characterized by the following method: select 5 porous ceramic microbeads with similar particle diameters and good sphericity, and place a single porous ceramic microbead on the ground. Use a pointer-type tensile gauge to press the porous ceramic microbead, and slowly increase the pressure until the porous ceramic microbead breaks. Record the maximum load when each porous ceramic microbead breaks, and calculate and average the single particle strength of the porous ceramic microbead using formula (1).

[0029] (1)

[0030] Where: G, single particle strength of porous ceramic microspheres, unit: MPa;

[0031] Fc, maximum load of porous ceramic microbeads when broken, unit N;

[0032] H, diameter of porous ceramic microspheres, in mm.

[0033] The bulk density of porous ceramic microspheres is characterized by the following method: using a 50 ml beaker, first remove the tare weight of the beaker, then place the fired and fully cooled microspheres into the beaker and allow them to naturally accumulate until the beaker is filled; then place the microspheres in the beaker on an electronic balance for weighing and record the accurate weight reading. The bulk density of porous ceramic microspheres is calculated by the following formula.

[0034] σ=m / V

[0035] Where: σ is the bulk density of porous ceramic microspheres, unit: g / cm 3;

[0036] m is the weight of the porous ceramic microbeads measured by an electronic balance, in g;

[0037] V is the volume of the porous ceramic microspheres, in cm 3 .

[0038] The water absorption rate of porous ceramic microbeads is characterized by the following method: first, weigh the dry weight (m1) of an appropriate amount of porous ceramic microbeads, and then completely immerse the porous ceramic microbeads in water for 1 hour to ensure that the water fully penetrates. After that, remove the excess water by complete filtration, and use an electronic balance to measure the wet weight (m2) of the microbeads after removing the tare weight. The water absorption rate of porous ceramic microbeads is calculated by the following formula.

[0039] Water absorption rate = (m2-m1) / m1*100%

[0040] Embodiment 1:

[0041] The preparation method of the adhesive in this embodiment is as follows: citric acid monohydrate and deionized water are mixed in a mass ratio of 4:5, heated in a water bath to 80°C to fully dissolve the citric acid to obtain a citric acid solution, and then the citric acid solution and light-burned magnesium oxide are mixed in a mass ratio of 1:0.29 for 2 h; the solution obtained after the reaction is placed in an oven and heat-treated at 180°C for 10 hours to obtain a solid product, namely, magnesium carboxylate after heat treatment; the magnesium carboxylate and boric acid are mixed in a mass ratio of 4:1 to finally obtain an adhesive for preparing porous ceramic microbeads by a foaming method.

[0042] The preparation method of porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: fly ash 81 wt.%, glass powder 8 wt.%, binder 8 wt.%, NH4HCO3 3 wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0043] First, the above raw materials are put into a ball mill and mixed evenly, then, 18 wt.% of water is added to the evenly mixed raw materials (here, 18 wt.% means that the mass of the added water is 18% of the total mass of the raw materials), and then transferred to a drum granulator for granulation and sieved through a sieve to obtain a ceramic microbead body with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead body is placed in an oven and foamed at 110°C for 30 minutes. Finally, the foamed ceramic microbead body is transferred to a muffle furnace, the temperature is raised to 860°C and sintered for 15 minutes to obtain porous ceramic microbeads.

[0044] The test results show that the water absorption rate of the porous ceramic microspheres is 0.8%, the single particle strength is 6.2 MPa, and the bulk density is 0.42 g / cm 3 .

[0045] Embodiment 2:

[0046] The preparation method of the adhesive in this embodiment is the same as that in Embodiment 1.

[0047] The preparation method of porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: fly ash 80wt.%, glass powder 8wt.%, binder 8wt.%, NH4HCO3 4wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0048] First, the above raw materials are put into a ball mill and mixed evenly, then, 18 wt.% of water is added to the evenly mixed raw materials (here, 18 wt.% means that the mass of the added water is 18% of the total mass of the raw materials), and then transferred to a drum granulator for granulation and sieved through a sieve to obtain a ceramic microbead body with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead body is placed in an oven and foamed at 110°C for 30 minutes. Finally, the foamed ceramic microbead body is transferred to a muffle furnace, the temperature is raised to 860°C and sintered for 15 minutes to obtain porous ceramic microbeads.

[0049] The test results show that the water absorption rate of the porous ceramic microspheres is 0.6%, the single particle strength is 4.5 MPa, and the bulk density is 0.29 g / cm 3 .

[0050] Embodiment 3:

[0051] The preparation method of the adhesive in this embodiment is the same as that in Embodiment 1.

[0052] The preparation method of the porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: perlite tailings 80wt.%, glass powder 5wt.%, adhesive 10wt.%, yeast powder 5wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0053] First, the above raw materials are loaded into a ball mill and mixed evenly, and then 18 wt.% of water is added to the evenly mixed raw materials (here 18 wt.% means that the mass of the added water is 18% of the total mass of the raw materials), and then transferred to a drum granulator for granulation and sieved through a sieve to obtain a ceramic microbead body with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead body is placed in an oven and foamed at 110°C for 45 minutes. Finally, the foamed ceramic microbead body is transferred to a muffle furnace, heated to 800°C and sintered for 20 minutes to obtain porous ceramic microbeads.

[0054] The test results show that the water absorption rate of the porous ceramic microspheres is 0.5%, the single particle strength is 5.1 MPa, and the bulk density is 0.38 g / cm 3 .

[0055] Embodiment 4:

[0056] The preparation method of the adhesive in this embodiment is the same as that in Embodiment 1.

[0057] The preparation method of the porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: perlite tailings 82wt.%, glass powder 5wt.%, adhesive 8wt.%, yeast powder 5wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0058] First, the above raw materials are loaded into a ball mill and mixed evenly, and then 20 wt.% of water is added to the evenly mixed raw materials (here 20 wt.% means that the mass of the added water is 20% of the total mass of the raw materials), and then transferred to an extrusion granulator for granulation and sieved through a sieve to obtain a ceramic microbead body with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead body is placed in an oven and foamed at 110°C for 45 minutes. Finally, the foamed ceramic microbead body is transferred to a muffle furnace, heated to 800°C and sintered for 20 minutes to obtain porous ceramic microbeads.

[0059] The test results show that the water absorption rate of the porous ceramic microspheres is 0.7%, the single particle strength is 5.8 MPa, and the bulk density is 0.48 g / cm 3 .

[0060] Embodiment 5:

[0061] The preparation method of the adhesive in this embodiment is the same as that in Embodiment 1.

[0062] The preparation method of porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: aluminum ash 70wt.%, glass powder 10wt.%, adhesive 15wt.%, NH4HCO3 5wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0063] First, the above raw materials are loaded into a ball mill and mixed evenly, and then 20 wt.% of water is added to the evenly mixed raw materials (here 20 wt.% means that the mass of the added water is 20% of the total mass of the raw materials), and then transferred to an extrusion granulator for granulation and sieved through a sieve to obtain a ceramic microbead body with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead body is placed in an oven and foamed at 110°C for 60 minutes. Finally, the foamed ceramic microbead body is transferred to a muffle furnace, heated to 850°C and sintered for 15 minutes to obtain porous ceramic microbeads.

[0064] The test results show that the water absorption rate of the porous ceramic microspheres is 0.4%, the single particle strength is 4.1 MPa, and the bulk density is 0.28 g / cm 3 .

[0065] Embodiment 6:

[0066] The preparation method of the adhesive in this embodiment is the same as that in Embodiment 1.

[0067] The preparation method of porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: aluminum ash 70wt.%, glass powder 10wt.%, adhesive 15wt.%, washing powder 5wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0068] First, the above raw materials are put into a ball mill and mixed evenly, then, 60 wt.% of water is added to the evenly mixed raw materials (here 60 wt.% means that the mass of the added water is 60% of the total mass of the raw materials), and then transferred to a spray drying granulator for granulation and sieved through a sieve to obtain ceramic microbead bodies with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead bodies are placed in an oven and foamed at 110°C for 60 minutes. Finally, the foamed ceramic microbead bodies are transferred to a muffle furnace, heated to 850°C and sintered for 15 minutes to obtain porous ceramic microbeads.

[0069] The test results show that the water absorption rate of the porous ceramic microspheres is 0.6%, the single particle strength is 5.9 MPa, and the bulk density is 0.34 g / cm 3 .

[0070] Embodiment 7:

[0071] The preparation method of the adhesive in this embodiment is as follows: citric acid monohydrate and deionized water are mixed in a mass ratio of 4:5, heated in a water bath to 75°C to fully dissolve the citric acid to obtain a citric acid solution, and then the citric acid solution and magnesium hydroxide are mixed in a mass ratio of 1:0.41 for 2.5 hours; the solution obtained after the reaction is placed in an oven and heat treated at 180°C for 10 hours to obtain a solid product, magnesium carboxylate; the magnesium carboxylate and boric acid are mixed in a mass ratio of 4:1 to finally obtain an adhesive for preparing porous ceramic microbeads by a foaming method.

[0072] The preparation method of porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: fly ash 81 wt.%, glass powder 8 wt.%, binder 8 wt.%, NH4HCO3 3 wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0073] First, the above raw materials are loaded into a ball mill and mixed evenly, then, 60 wt.% of water is added to the evenly mixed raw materials (here, 60 wt.% means that the mass of the added water is 60% of the total mass of the raw materials), and then transferred to a spray drying granulator for granulation and sieved through a sieve to obtain a ceramic microbead body with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead body is placed in an oven and foamed at 120°C for 30 minutes. Finally, the foamed ceramic microbead body is transferred to a muffle furnace, heated to 860°C and sintered for 15 minutes to obtain porous ceramic microbeads.

[0074] The test results show that the water absorption rate of the porous ceramic microspheres is 0.7%, the single particle strength is 5.9 MPa, and the bulk density is 0.41 g / cm 3 .

[0075] Embodiment 8:

[0076] The preparation method of the adhesive in this embodiment is as follows: citric acid monohydrate and deionized water are mixed in a mass ratio of 4:5, heated in a water bath to 85°C to fully dissolve the citric acid to obtain a citric acid solution, and then the citric acid solution and magnesium carbonate are mixed in a mass ratio of 1:0.55 for reaction for 1.5 h; the solution obtained after the reaction is placed in an oven and heat treated at 180°C for 10 hours to obtain a solid product, magnesium carboxylate; the magnesium carboxylate and boric acid are mixed in a mass ratio of 4:1 to finally obtain an adhesive for preparing porous ceramic microbeads by a foaming method.

[0077] The preparation method of porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: fly ash 81 wt.%, glass powder 8 wt.%, binder 8 wt.%, NH4HCO3 3 wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0078] First, the above raw materials are put into a ball mill and mixed evenly, then, 60 wt.% of water is added to the evenly mixed raw materials (here 60 wt.% means that the mass of the added water is 60% of the total mass of the raw materials), and then transferred to a spray drying granulator for granulation and sieved through a sieve to obtain ceramic microbead bodies with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead bodies are placed in an oven and foamed at 130°C for 30 minutes. Finally, the foamed ceramic microbead bodies are transferred to a muffle furnace, heated to 860°C and sintered for 15 minutes to obtain porous ceramic microbeads.

[0079] The test results show that the water absorption rate of the porous ceramic microspheres is 0.8%, the single particle strength is 6.3 MPa, and the bulk density is 0.40 g / cm 3 .

[0080] Embodiment 9:

[0081] The preparation method of the adhesive in this embodiment is the same as that in Embodiment 1.

[0082] The preparation method of porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: perlite tailings 77 wt.%, glass powder 10 wt.%, adhesive 8 wt.%, yeast powder 5 wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0083] First, the above raw materials are put into a ball mill and mixed evenly, then, 18 wt.% of water is added to the evenly mixed raw materials (here, 18 wt.% means that the mass of the added water is 18% of the total mass of the raw materials), and then transferred to a drum granulator for granulation and sieved through a sieve to obtain a ceramic microbead body with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead body is placed in an oven and foamed at 110° C. for 45 minutes. Finally, the foamed ceramic microbead body is transferred to a muffle furnace, the temperature is raised to 700° C. and sintered for 30 minutes to obtain porous ceramic microbeads.

[0084] The test results show that the water absorption rate of the porous ceramic microspheres is 0.9%, the single particle strength is 6.8 MPa, and the bulk density is 0.44 g / cm 3 .

[0085] Embodiment 10:

[0086] The preparation method of the adhesive in this embodiment is the same as that in Embodiment 1.

[0087] The preparation method of porous ceramic microbeads in this embodiment is as follows: weigh the raw material components according to the following mass percentages: perlite tailings 84 wt.%, glass powder 3 wt.%, adhesive 8 wt.%, yeast powder 5 wt.%, and the particle size of the raw materials is greater than 325 mesh.

[0088] First, the above raw materials are loaded into a ball mill and mixed evenly, and then 18 wt.% of water is added to the evenly mixed raw materials (here 18 wt.% means that the mass of the added water is 18% of the total mass of the raw materials), and then transferred to a drum granulator for granulation and sieved through a sieve to obtain a ceramic microbead body with a particle size of 2.8 mm to 8 mm. Then, the ceramic microbead body is placed in an oven and foamed at 110°C for 45 minutes. Finally, the foamed ceramic microbead body is transferred to a muffle furnace, the temperature is raised to 900°C and sintered for 10 minutes to obtain porous ceramic microbeads.

[0089] The test results show that the water absorption rate of the porous ceramic microspheres is 0.6%, the single particle strength is 5.1 MPa, and the bulk density is 0.34 g / cm 3 .

[0090] Comparative Example 1:

[0091] This comparative example adopts a high temperature foaming method to prepare porous ceramic microspheres.

[0092] The preparation method of the porous ceramic microbeads in this comparative example is as follows: weigh the raw material components according to the following mass percentages: fly ash 80wt.%, glass powder 8wt.%, silicon carbide 4wt.%, and polyvinyl alcohol fiber 8wt.%.

[0093] First, the above raw materials are loaded into a ball mill and mixed evenly; then, 18 wt.% of water is added to the mixed raw materials (here, 18 wt.% means that the mass of the added water is 18% of the total mass of the raw materials), and then transferred to a drum granulator for granulation and screened through a sieve to obtain a ceramic microbead blank with a particle size of 2.8 mm to 8 mm, and the ceramic microbead blank is placed in an oven and dried at 110°C for 24 hours. Finally, the ceramic microbead blank is transferred to a muffle furnace, heated to 1220°C and sintered for 20 minutes to obtain porous ceramic microbeads. Among them, 1220°C is also the foaming temperature for preparing the porous ceramic microbeads.

[0094] The test results show that the porous ceramic microspheres have a water absorption rate of 1.2%, a single particle strength of 6.9 MPa, and a bulk density of 0.68 g / cm 3 .

[0095] Figure 1 The macroscopic image and SEM image of the magnesium carboxylate obtained after the heat treatment in the process of preparing the adhesive in Example 1 of the present invention are shown, wherein the image marked as (a) in the upper left corner is the macroscopic image, and the image marked as (b) in the upper left corner is the SEM image; Figure 1 As can be seen from the middle figure (b), magnesium carboxylate has fibrous bonding substances, which is beneficial to improving the strength of the porous ceramic microbeads.

[0096] Figure 2 The XRD spectrum and infrared spectrum of magnesium carboxylate after heat treatment in the process of preparing the adhesive in Example 1 of the present invention are shown, wherein the upper left corner is marked with (a) for the XRD spectrum and the upper left corner is marked with (b) for the infrared spectrum; Figure 2 The middle figure (a) shows that magnesium carboxylate is transformed into an amorphous substance after heat treatment, and its phase composition cannot be determined by X-ray diffraction (XRD) technology. Figure 2 The middle figure (b) shows that the magnesium carboxylate after heat treatment still contains Mg-O, CC, HO, -CO, -C=O and -CH2 bonds, indicating that it is still a magnesium carboxylate.

[0097] Figure 3It is the XRD spectrum and infrared spectrum of the hydration product of the heat-treated magnesium carboxylate and the hydration product of the prepared adhesive (heat-treated magnesium carboxylate + boric acid) in Example 1 of the present invention. Among them, the hydration product of the heat-treated magnesium carboxylate is prepared by the following method: an appropriate amount of heat-treated magnesium carboxylate is placed in a beaker, and an equal mass of deionized water is added, and then, it is rapidly stirred for 2 minutes, and the obtained mixture is placed in a constant temperature and humidity chamber (humidity: 50%, temperature 35°C) for curing for 24 hours to obtain the hydration product of the heat-treated magnesium carboxylate; the preparation method of the hydration product of the adhesive is the same as above. Figure 3 The middle figure (a) shows that the heat-treated magnesium carboxylate will rehydrate when it meets water to form a magnesium carboxylate with a crystalline structure, which gives it adhesiveness. In addition, there is a significant difference in the XRD spectrum of the hydration product of the heat-treated magnesium carboxylate and the hydration product of the adhesive, which indicates that the heat-treated magnesium carboxylate reacts with boric acid. Figure 3 It can be seen from the middle figure (b) that the stretching vibration peak of BOC appears in the hydration product of the adhesive prepared by the present invention, which further indicates that an esterification reaction occurs between boric acid and the heat-treated magnesium carboxylate.

[0098] Figure 4 is the viscosity value of the hydration product of the adhesive prepared in Example 1 of the present invention at room temperature and 110°C, wherein the room temperature is specifically 25°C. The preparation method of the hydration product of the adhesive is the same as Figure 3 From Figure 4 It can be seen that the hydration product of the adhesive is solid at room temperature and has an infinite viscosity. When the temperature is heated to 110°C, the viscosity decreases to 5267 Pa·s, which indicates that the adhesive prepared by the present invention will soften when the temperature rises to 110°C, thereby giving the ceramic microbeads plasticity.

[0099] Figure 5 The macroscopic images of porous ceramic microbeads prepared in Example 2 and Comparative Example 1, respectively, wherein the one marked with (a) in the upper left corner is prepared in Comparative Example 1, and the one marked with (b) in the upper left corner is prepared in Example 2. Figure 5 It can be seen from the middle figure (a) that the porous ceramic microbeads prepared by the high temperature foaming method in comparative example 1 do not form a porous structure, while from figure (b) it can be seen that the porous ceramic microbeads prepared in Example 2 have a porous structure inside and a structure covered with a dense glaze layer on the surface, and the sphericity of the porous ceramic microbeads is good. The dense glaze layer covering the surface of the porous ceramic microbeads will significantly reduce their water absorption rate.

[0100] Table 1 Properties of porous ceramic microbeads prepared in Examples 1 to 10 and Comparative Example 1

[0101] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 Comparative Example 1 Water absorption (%) 0.8 0.6 0.5 0.7 0.4 0.6 0.7 0.8 0.9 0.6 1.2 Single particle strength (MPa) 6.2 4.5 5.1 5.8 4.1 5.9 5.9 6.3 6.8 5.1 6.9 <![CDATA[Bulk density (g / cm 3 )]]> 0.42 0.29 0.38 0.48 0.28 0.34 0.41 0.40 0.44 0.34 0.68

[0102] In Example 2 and Comparative Example 1, the mass percentages of fly ash and glass powder used as raw materials are the same, and the raw material ratios for preparing ceramic microspheres are the same. The foaming temperature of the porous ceramic microspheres prepared by the adhesive of the present invention is 1110°C lower than that of Comparative Example 1, and the sintering temperature is significantly reduced and the sintering time is shortened, which can significantly reduce the production cost and energy consumption of preparing porous ceramic microspheres. It can also be seen from Table 1 that the porous ceramic microspheres prepared by the present invention have the characteristics of low water absorption (i.e., low apparent porosity), low bulk density, and certain single particle strength.

[0103] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing porous ceramic microbeads, characterized in that: The specific steps include: The ceramic microbead raw material, the binder, the sintering aid and the foaming agent are uniformly mixed, and water is added thereto, and the mixture is granulated and sieved by a granulator to obtain a ceramic microbead body, and the ceramic microbead body is foamed at 110° C. to 130° C. for more than 10 minutes, and finally, sintered at 700° C. to 900° C. to obtain porous ceramic microbeads; The adhesive is prepared by the following method: first, a citric acid solution and a magnesium-based compound are mixed in proportion and reacted for a reaction time of not less than 1 hour; the solution obtained after the reaction is placed in an oven and heat-treated at 180 to 200° C. for not less than 10 hours to obtain a solid product; then, the heat-treated product is mixed with boric acid in a mass ratio of 4:1 to finally obtain an adhesive.

2. The method for preparing porous ceramic microspheres according to claim 1, characterized in that: The citric acid solution is obtained by mixing citric acid monohydrate and deionized water in a mass ratio of 4:5, and heating the mixture in a water bath to 75-85° C. to fully dissolve the citric acid.

3. The method for preparing porous ceramic microspheres according to claim 1, characterized in that: The magnesium-based compound is one of light-burned magnesium oxide, magnesium hydroxide or magnesium carbonate.

4. The method for preparing porous ceramic microspheres according to claim 3, characterized in that: The citric acid solution and the magnesium-based compound are mixed in proportion. Specifically, when the magnesium-based compound is light-burned magnesium oxide, the mass ratio of the two is 1:0.29; when the magnesium-based compound is magnesium hydroxide, the mass ratio of the two is 1:0.41; when the magnesium-based compound is magnesium carbonate, the mass ratio of the two is 1:0.

55.

5. The method for preparing porous ceramic microspheres according to claim 1, characterized in that: The citric acid solution and the magnesium-based compound are mixed and reacted to generate a white precipitate, which is magnesium carboxylate.

6. The method for preparing porous ceramic microspheres according to claim 1, characterized in that: The raw material of the ceramic microbeads includes at least one of fly ash, perlite tailings, sludge, and aluminum ash; the sintering aid is glass powder; and the foaming agent includes at least one of ammonium bicarbonate, washing powder, and yeast powder.

7. The method for preparing porous ceramic microspheres according to claim 1, characterized in that: The mass of the added water is 18% to 60% of the total mass of the ceramic microsphere raw material, adhesive, sintering aid and foaming agent.

8. The method for preparing porous ceramic microspheres according to claim 1, characterized in that: The granulator is one of an extrusion granulator, a drum granulator and a spray drying granulator.

9. The porous ceramic microbeads obtained by the preparation method according to any one of claims 1 to 8.

10. The porous ceramic microbeads according to claim 9, characterized in that: The porous ceramic micro-beads have a porous structure inside and a dense glaze layer is covered on the surface.

Citation Information

Patent Citations

  • Process for production of aluminum titanate-based ceramics

    CN101910065A

  • Magnesium-based binder for sintered magnesia bricks and preparation method thereof

    CN111233489A