Biodegradable resin particles

Through the copolymerization of polyacrylic acid with modified starch, iron hydroxyoxide, sodium alginate, and carboxymethylcellulose, and the use of gamma ray irradiation, the problems of short service life and low mechanical strength of existing biodegradable materials are solved, and the problem of low mechanical strength of existing biodegradable materials is achieved. The high mechanical properties and water resistance of biodegradable resin particles are obtained.

CN118652512BActive Publication Date: 2024-11-15FUJIAN DELV NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110138.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-15
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing biodegradable materials have a short service life and are low in mechanical strength, which limits their wide application in industrial and living fields.

Method used

Polyacrylic acid is used as a carrier to form active sites by copolymerization with modified starch, iron hydroxyoxide, sodium alginate, and carboxymethylcellulose by γ-ray irradiation, thereby enhancing the biodegradability and mechanical properties of the material.

Benefits of technology

The high mechanical properties and water resistance of biodegradable resin particles are achieved, and the biodegradation speed and structural density of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a biodegradable resin particle, and relates to the technical field of biodegradable materials. The invention utilizes the effects of high-speed shearing and oxalic acid to modify starch, thereby converting it into small molecules with relatively short molecular chains, forming orderly self-association, and in this process, adding agar, cooling and directional arrangement to form a three-dimensional network structure, thereby achieving biodegradability and enhancing the water resistance and mechanical properties of the matrix, utilizing oxyhydroxide, sodium alginate, and carboxymethyl cellulose under the induction of gamma rays to undergo graft copolymerization with polyacrylic acid as a carrier, wherein the oxyhydroxide is fixed in the matrix through complexation, accelerating the biodegradation progress of the matrix, and enhancing the mechanical properties, while the compatibility between sodium alginate and starch molecules reduces the gaps between the matrix skeletons, making the structure more compact, thereby improving the water resistance and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biodegradable materials, in particular to biodegradable resin particles. Background Art

[0002] Resin material is a kind of polymer compound and a common industrial raw material. It is widely used in plastic products, coatings, adhesives, synthetic fibers and other fields. In life, we cannot do without polymer materials. With the development of industrial level and strict requirements on materials, polymer materials have a better development prospect. Biodegradable materials generally refer to polymer materials that have certain usability and can be decomposed into harmless substances such as water and carbon dioxide by microorganisms in nature, so that they can be recycled into nature for reuse. The degradation process is roughly as follows: first, a large number of microorganisms infiltrate the surface of the material to reproduce and produce a large number of hydrolases, which cut off the polymer chain segments in the process of hydrolysis with the material; then the degradation products are consumed and metabolized by microorganisms to finally produce carbon dioxide and water. However, general biodegradable materials generally have a short service life and low mechanical strength, which is not conducive to the promotion of biodegradable materials. Summary of the invention

[0003] The object of the present invention is to provide a biodegradable resin particle to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing biodegradable resin particles, comprising the following preparation steps:

[0005] (1) Mix oxalic acid and dimethyl sulfoxide, stir at 50-100 rpm for 15-30 min, add corn starch and deionized water, heat to 100-130°C, continue stirring for 5-15 min, add benzene, toluene and pyridine, perform high-speed shearing, then add agar, stir at 100-250 rpm for 1-3 h, cool to room temperature, add ethanol, stir at 50-100 rpm until precipitation occurs, let stand for 20-40 min, filter, take the solid, wash with ethanol and deionized water three times each, dry at 30-50°C for 6-9 h, crush, and sieve to obtain intermediate A;

[0006] (2) Sodium alginate, carboxymethyl cellulose, ferric oxide dispersion and deionized water are mixed, heated to 60-80°C in a nitrogen atmosphere, stirred at 50-100 rpm for 20-40 min, cooled to room temperature, polyacrylic acid is added, and the pH of the solution is adjusted to 7-8 with a 20 wt % sodium hydroxide aqueous solution, heated to 50-80°C, stirred at 100-200 rpm for 1-3 h, N,N-methylenebisacrylamide is added, and stirring is continued for 15 min, then placed in a γ-ray radiation field for irradiation, then soaked in methanol for 3-6 h, dried at 50-80°C for 4-8 h, crushed, and passed through a 10-20 mesh sieve to obtain copolymer particles;

[0007] (3) The copolymer particles, the intermediate A and acetyl tributyl citrate are mixed and extruded to obtain biodegradable resin particles.

[0008] Furthermore, the high-speed shearing rate in step (1) is 400-800 rpm and the time is 10-25 min.

[0009] Furthermore, the mesh size of the sieve in step (1) is 60-130 meshes.

[0010] Furthermore, in step (1), the mass ratio of oxalic acid, dimethyl sulfoxide, corn starch, deionized water, benzene, toluene, pyridine, agar, and ethanol is 3:5:3~8:10~30:2:1:0.1:1~2:20.

[0011] Furthermore, the preparation method of the oxyhydroxide dispersion in step (2) is as follows: oxyhydroxide and deionized water are mixed in a mass ratio of 1:30-60, and ultrasonically dispersed at 21 kHz for 10-30 minutes to obtain the dispersion.

[0012] Furthermore, the molecular weight of the polyacrylic acid in step (2) is 2000.

[0013] Furthermore, the irradiation parameters of step (2) are: radiation dose of 3-10 kGy, temperature of 60-80° C., and time of 1-3 min.

[0014] Furthermore, in step (2), the mass ratio of the sodium alginate, carboxymethyl cellulose, ferric oxyhydroxide dispersion, deionized water, polyacrylic acid, and N,N-methylenebisacrylamide is 1:1:0.6:10-50:4-15:0.1.

[0015] Furthermore, the temperature of the extrusion granulation in step (3) is 130-150°C.

[0016] Furthermore, in step (3), the mass ratio of the copolymer particles, the intermediate A, and acetyl tributyl citrate is 10:2-4:0.5.

[0017] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0018] The resin particles of the invention are prepared by using polyacrylic acid as a carrier, and modified starch, ferric hydroxide oxide, sodium alginate and carboxymethyl cellulose through irradiation polymerization to achieve the effects of biodegradation, water resistance and high mechanical properties.

[0019] Firstly, the starch is modified by high-speed shearing and oxalic acid above the gelatinization temperature, wherein the carboxyl group in the oxalic acid undergoes an esterification reaction with the hydroxyl group on the starch molecular chain, and the glycosidic bonds in the starch are broken by high-temperature hydrolysis, so that its macromolecules become small molecules with relatively short molecular chains, thereby increasing the number of molecular chains and releasing them from the gelatinized starch granules, and at a high shear rate, the short molecular chains aggregated in the starch are destroyed at this time, so that the molecular chains are no longer entangled but are more easily oriented, forming an orderly self-association, so that the number of remaining free hydroxyl groups that can combine with water molecules through hydrogen bonds is relatively reduced, and in this process, agar is added, and its molecules are oriented to form a three-dimensional network structure as the mixture cools, and intermolecular hydrogen bonds are formed, so that the starch molecules are evenly fixed in the grid, thereby assisting the matrix to enhance the water resistance and mechanical properties, while achieving biodegradability.

[0020] Secondly, ferric hydroxide, sodium alginate and carboxymethyl cellulose are grafted and copolymerized with polyacrylic acid as a carrier under the induction of gamma rays. Irradiation increases the number of free radicals generated in the mixture and forms active sites for initiating polymerization in the matrix. The ferric hydroxide produces a complexation between its hydroxyl group and the carboxyl group of the acrylic acid side chain, so that the ferric hydroxide particles are firmly fixed in the matrix, providing an electron channel for the release of microbial cells, promoting long-distance electron transfer between bacteria or cooperative metabolism between different species, and accelerating the biodegradation progress of the matrix. Its rigidity can also enhance the mechanical properties of the matrix. Hydrogen bonds are formed between the components in carboxymethyl cellulose and sodium alginate, thereby reducing the number of remaining hydroxyl groups in the matrix and weakening the association of hydroxyl groups with water through hydrogen bonds, thereby improving the water resistance of the matrix. At the same time, the good compatibility between sodium alginate and starch molecules reduces the gaps between the matrix skeletons, making the structure denser, thereby improving the water resistance and mechanical properties. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0022] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the test methods of various indicators of the biodegradable resin particles prepared in the following examples:

[0023] The biodegradable resin pellets were heat-pressed at 150°C to form a film with a thickness of 500 μm.

[0024] Biodegradation: The same size of the embodiment and the comparative example were taken according to ISO 16929, and the biodegradation rate of the samples was tested on the 30th day.

[0025] Water resistance: Take the same size of the embodiment and the comparative example, immerse the sample in deionized water at 25°C according to GB / T1034, take it out after 24 hours, and test its water absorption rate.

[0026] Mechanical properties: The yield stress and Elmendorf tear strength of the examples and comparative examples of the same size were tested according to JIS K7127 and ISO 6383-2, respectively.

[0027] Example 1; (1) oxalic acid and dimethyl sulfoxide were mixed, stirred at 50 rpm for 15 min, corn starch and deionized water were added, the temperature was raised to 100°C, stirring was continued for 5 min, benzene, toluene and pyridine were added, high-speed shearing was performed at a rate of 400 rpm for 10 min, agar was then added, stirred at 100 rpm for 1 h, cooled to room temperature, ethanol was added, stirred at 50 rpm until precipitation occurred, allowed to stand for 20 min, filtered, solids were taken, and then washed with ethanol and deionized water three times each in turn, dried at 30°C for 6 h, crushed, and passed through a 60-mesh sieve to obtain intermediate A; the mass ratio of oxalic acid, dimethyl sulfoxide, corn starch, deionized water, benzene, toluene, pyridine, agar, and ethanol was 3:5:3:10:2:1:0.1:1:20;

[0028] (2) Mix ferric hydroxide and deionized water in a mass ratio of 1:30, and perform ultrasonic dispersion at 21 kHz for 10 min to obtain a ferric hydroxide dispersion. Mix sodium alginate, carboxymethyl cellulose, ferric hydroxide dispersion, and deionized water, heat to 60 °C in a nitrogen atmosphere, stir at 50 rpm for 20 min, cool to room temperature, add polyacrylic acid with a molecular weight of 2000, and adjust the solution pH to 7 with 20 wt% sodium hydroxide aqueous solution, heat to 50 °C, stir at 100 rpm for 1 h, add N, N -methylenebisacrylamide, continue stirring for 15 minutes, then place in the radiation field of gamma rays for irradiation, the radiation dose is 3kGy, the temperature is 60°C, the time is 1 minute, then soak in methanol for 3 hours, dry at 50°C for 4 hours, crush, pass through a 10-mesh sieve to obtain copolymer particles; the mass ratio of sodium alginate, carboxymethyl cellulose, ferric oxyhydroxide dispersion, deionized water, polyacrylic acid with a molecular weight of 2000, and N,N-methylenebisacrylamide is 1:1:0.6:10:4:0.1;

[0029] (3) The copolymer particles, the intermediate A and acetyl tributyl citrate are mixed and extruded and granulated at 150° C. to obtain biodegradable resin particles; the mass ratio of the copolymer particles, the intermediate A and acetyl tributyl citrate is 10:2:0.5.

[0030] Example 2; (1) oxalic acid and dimethyl sulfoxide were mixed, stirred at 75 rpm for 22 min, corn starch and deionized water were added, the temperature was raised to 110°C, stirring was continued for 8 min, benzene, toluene and pyridine were added, high-speed shearing was performed at a rate of 600 rpm for 19 min, agar was then added, stirred at 170 rpm for 2 h, cooled to room temperature, ethanol was added, stirred at 75 rpm until precipitation occurred, allowed to stand for 30 min, filtered, solids were taken, and then washed with ethanol and deionized water three times each, dried at 40°C for 8 h, crushed, and passed through a 90-mesh sieve to obtain intermediate A; the mass ratio of oxalic acid, dimethyl sulfoxide, corn starch, deionized water, benzene, toluene, pyridine, agar, and ethanol was 3:5:5:20:2:1:0.1:1.5:20;

[0031] (2) Mix ferric hydroxide and deionized water in a mass ratio of 1:45, and perform ultrasonic dispersion at 21 kHz for 20 min to obtain a ferric hydroxide dispersion. Mix sodium alginate, carboxymethyl cellulose, ferric hydroxide dispersion, and deionized water, heat to 70°C in a nitrogen atmosphere, stir at 75 rpm for 30 min, cool to room temperature, add polyacrylic acid with a molecular weight of 2000, and adjust the solution pH to 7.5 with 20 wt% sodium hydroxide aqueous solution, heat to 65°C, stir at 150 rpm for 2 h, add N,N- Methylenebisacrylamide, continue stirring for 15 minutes, then place in the radiation field of gamma rays for irradiation, the radiation dose is 6kGy, the temperature is 70°C, the time is 2 minutes, then soak in methanol for 4.5 hours, dry at 70°C for 6 hours, crush, pass through a 12-mesh sieve to obtain copolymer particles; the mass ratio of sodium alginate, carboxymethyl cellulose, ferric oxide dispersion, deionized water, polyacrylic acid with a molecular weight of 2000, and N,N-methylenebisacrylamide is 1:1:0.6:30:10:0.1;

[0032] (3) The copolymer particles, the intermediate A and acetyl tributyl citrate are mixed and extruded and granulated at 150° C. to obtain biodegradable resin particles; the mass ratio of the copolymer particles, the intermediate A and acetyl tributyl citrate is 10:3:0.5.

[0033] Example 3; (1) oxalic acid and dimethyl sulfoxide were mixed, stirred at 100 rpm for 30 min, corn starch and deionized water were added, the temperature was raised to 130°C, stirring was continued for 15 min, benzene, toluene and pyridine were added, high-speed shearing was performed at a rate of 800 rpm for 25 min, agar was then added, stirred at 250 rpm for 3 h, cooled to room temperature, ethanol was added, stirred at 100 rpm until precipitation occurred, allowed to stand for 40 min, filtered, solids were taken, and then washed with ethanol and deionized water three times each, dried at 50°C for 9 h, crushed, and passed through a 130-mesh sieve to obtain intermediate A; the mass ratio of oxalic acid, dimethyl sulfoxide, corn starch, deionized water, benzene, toluene, pyridine, agar, and ethanol was 3:5:8:30:2:1:0.1:2:20;

[0034] (2) Mix ferric hydroxide and deionized water in a mass ratio of 1:60, and disperse them ultrasonically at 21 kHz for 30 minutes to obtain a ferric hydroxide dispersion; mix sodium alginate, carboxymethyl cellulose, ferric hydroxide dispersion, and deionized water, heat to 80°C in a nitrogen atmosphere, stir at 100 rpm for 40 minutes, cool to room temperature, add polyacrylic acid with a molecular weight of 2000, and adjust the solution pH to 8 with 20 wt% sodium hydroxide aqueous solution, heat to 80°C, stir at 200 rpm for 3 hours, and add N,N- Methylenebisacrylamide, continue stirring for 15 minutes, then place in the radiation field of gamma rays for irradiation, the radiation dose is 10kGy, the temperature is 80℃, the time is 3min, then soak in methanol for 6h, dry at 80℃ for 8h, crush, pass through a 20-mesh sieve to obtain copolymer particles; the mass ratio of sodium alginate, carboxymethyl cellulose, ferric oxide dispersion, deionized water, polyacrylic acid with a molecular weight of 2000, and N,N-methylenebisacrylamide is 1:1:0.6:50:15:0.1;

[0035] (3) The copolymer particles, the intermediate A and acetyl tributyl citrate are mixed and extruded and granulated at 150° C. to obtain biodegradable resin particles; the mass ratio of the copolymer particles, the intermediate A and acetyl tributyl citrate is 10:4:0.5.

[0036] Comparative Example 1; The difference between Comparative Example 1 and Example 2 is that step (1) is different. Step (1) is changed to: oxalic acid and dimethyl sulfoxide are mixed, stirred at 75 rpm for 22 minutes, corn starch and deionized water are added, the temperature is raised to 110°C, and stirring is continued for 8 minutes. Benzene, toluene and pyridine are added, and stirring is continued at 100 rpm for 5 hours. Then agar is added, and stirring is continued at 170 rpm for 2 hours. The mixture is cooled to room temperature, ethanol is added, and stirring is continued at 75 rpm until precipitation occurs. The mixture is allowed to stand for 30 minutes, filtered, and the solid is taken. The solid is then washed with ethanol and deionized water three times each in sequence, dried at 40°C for 8 hours, crushed, and passed through a 90-mesh sieve to obtain intermediate A. The mass ratio of oxalic acid, dimethyl sulfoxide, corn starch, deionized water, benzene, toluene, pyridine, agar, and ethanol is 3:5:5:20:2:1:0.1:1.5:20. The remaining steps are the same as those in Example 2.

[0037] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (1) is different. Step (1) is changed to: corn starch and deionized water are heated to 110°C, stirred at 75 rpm for 8 min, agar is added, stirred at 170 rpm for 2 h, cooled to room temperature, dried at 40°C for 8 h, crushed, and passed through a 90-mesh sieve to obtain intermediate A; the mass ratio of corn starch, deionized water, and agar is 5:20:1.5; the remaining steps are the same as in Example 2.

[0038] Comparative Example 3; The difference between Comparative Example 3 and Example 2 is that step (1) is different. Step (1) is changed to: oxalic acid and dimethyl sulfoxide are mixed, stirred at 75 rpm for 22 minutes, corn starch and deionized water are added, the temperature is raised to 110°C, stirring is continued for 8 minutes, benzene, toluene and pyridine are added, high-speed shearing is performed at a rate of 600 rpm for 19 minutes, the mixture is cooled to room temperature, ethanol is added, stirred at 75 rpm until precipitation occurs, the mixture is allowed to stand for 30 minutes, filtered, the solid is taken, and then washed with ethanol and deionized water three times each in turn, dried at 40°C for 8 hours, crushed, and passed through a 90-mesh sieve to obtain intermediate A; the mass ratio of oxalic acid, dimethyl sulfoxide, corn starch, deionized water, benzene, toluene, pyridine and ethanol is 3:5:5:20:2:1:0.1:20; the remaining steps are the same as Example 2.

[0039] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that step (2) is different. Step (2) is changed to: sodium alginate, carboxymethyl cellulose and deionized water are mixed, heated to 70°C under a nitrogen atmosphere, stirred at 75 rpm for 30 min, cooled to room temperature, polyacrylic acid with a molecular weight of 2000 is added, and the solution pH is adjusted to 7.5 with 20 wt% sodium hydroxide aqueous solution, heated to 65°C, stirred at 150 rpm for 2 h, N,N-methylenebisacrylamide is added, and stirring is continued for 15 min. Subsequently, the mixture is placed in a γ-ray radiation field for irradiation, wherein the radiation dose is 6 kGy, the temperature is 70°C, and the time is 2 min. Subsequently, the mixture is soaked in methanol for 4.5 h, dried at 70°C for 6 h, crushed, and passed through a 12-mesh sieve to obtain copolymer particles. The mass ratio of the sodium alginate, carboxymethyl cellulose, deionized water, polyacrylic acid with a molecular weight of 2000, and N,N-methylenebisacrylamide is 1:1:30:10:0.1. The remaining steps are the same as those in Example 2.

[0040] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that step (2) is different, and step (2) is changed to: ferric hydroxide and deionized water are mixed in a mass ratio of 1:45, and ultrasonically dispersed at 21kHz for 20min to obtain a ferric hydroxide dispersion; carboxymethyl cellulose, ferric hydroxide dispersion, and deionized water are mixed, heated to 70°C under a nitrogen atmosphere, stirred at 75rpm for 30min, cooled to room temperature, polyacrylic acid with a molecular weight of 2000 is added, and the pH of the solution is adjusted to 7.5 with a 20wt% sodium hydroxide aqueous solution, heated to 65°C, and stirred at 150r The mixture was stirred for 2 h, N,N-methylenebisacrylamide was added, and stirring was continued for 15 min. The mixture was then placed in a γ-ray radiation field for irradiation at a dose of 6 kGy, a temperature of 70 ° C, and a time of 2 min. Subsequently, the mixture was soaked in methanol for 4.5 h, dried at 70 ° C for 6 h, crushed, and passed through a 12-mesh sieve to obtain copolymer particles. The mass ratio of the carboxymethyl cellulose, the oxyhydroxide dispersion, the deionized water, the polyacrylic acid with a molecular weight of 2000, and the N,N-methylenebisacrylamide was 1:0.6:30:10:0.1. The remaining steps were the same as those in Example 2.

[0041] Comparative Example 6: The difference between Comparative Example 6 and Example 2 is that step (2) is different, and step (2) is changed to: ferric hydroxide and deionized water are mixed in a mass ratio of 1:45, and ultrasonic dispersion is performed at 21kHz for 20min to obtain a ferric hydroxide dispersion; sodium alginate, ferric hydroxide dispersion and deionized water are mixed, heated to 70°C under a nitrogen atmosphere, stirred at 75rpm for 30min, cooled to room temperature, polyacrylic acid with a molecular weight of 2000 is added, and the pH of the solution is adjusted to 7.5 with a 20wt% sodium hydroxide aqueous solution, heated to 65°C, and stirred at 150r The mixture was stirred for 2 h, N,N-methylenebisacrylamide was added, and stirring was continued for 15 min. The mixture was then placed in a γ-ray radiation field for irradiation at a radiation dose of 6 kGy, a temperature of 70 ° C, and a time of 2 min. Subsequently, the mixture was soaked in methanol for 4.5 h, dried at 70 ° C for 6 h, crushed, and passed through a 12-mesh sieve to obtain copolymer particles. The mass ratio of the sodium alginate, the ferric oxyhydroxide dispersion, the deionized water, the polyacrylic acid with a molecular weight of 2000, and the N,N-methylenebisacrylamide was 1:0.6:30:10:0.1. The remaining steps were the same as those in Example 2.

[0042] Comparative Example 7: The difference between Comparative Example 7 and Example 2 is that step (2) is different, and step (2) is changed to: ferric hydroxide and deionized water are mixed in a mass ratio of 1:45, and ultrasonically dispersed at 21kHz for 20min to obtain a ferric hydroxide dispersion; sodium alginate, carboxymethyl cellulose, ferric hydroxide dispersion, and deionized water are mixed, heated to 70°C under a nitrogen atmosphere, stirred at 75rpm for 30min, cooled to room temperature, polyacrylic acid with a molecular weight of 2000 is added, and 20wt% The solution pH was adjusted to 7.5 with sodium hydroxide aqueous solution, the temperature was raised to 65°C, stirred at 150 rpm for 2 h, N,N-methylenebisacrylamide was added, stirring was continued for 2 h, dried at 70°C for 6 h, crushed, and passed through a 12-mesh sieve to obtain copolymer particles; the mass ratio of the sodium alginate, carboxymethyl cellulose, ferric oxyhydroxide dispersion, deionized water, polyacrylic acid with a molecular weight of 2000, and N,N-methylenebisacrylamide was 1:1:0.6:30:10:0.1; the remaining steps were the same as in Example 2.

[0043] Comparative Example 8: The difference between Comparative Example 8 and Example 2 is that step (3) is different. Step (3) is changed to: the copolymer particles, agar, and acetyl tributyl citrate are mixed, and extrusion granulation is performed at 150° C. to obtain biodegradable resin particles; the mass ratio of the copolymer particles, agar, and acetyl tributyl citrate is 10:3:0.5; the remaining steps are the same as in Example 2.

[0044] Effect example

[0045] The following Table 1 shows the performance analysis results of the biodegradable resin particles of Examples 1 to 3 of the present invention and Comparative Examples 1 to 8.

[0046] Table 1

[0047]

[0048] From the comparison of the experimental results of the embodiment and the comparative example in Table 1, it can be found that the present invention utilizes starch to be modified by high-speed shearing and the action of oxalic acid above the gelatinization temperature, wherein the carboxyl group in the oxalic acid reacts with the hydroxyl group on the starch molecular chain to undergo an esterification reaction, and under the action of high-temperature hydrolysis, the starch macromolecules are transformed into small molecules with relatively short molecular chains, and under a high shear rate, the short molecular chains aggregated in the starch are destroyed, so that the molecular chains are no longer entangled but are more easily oriented, forming an orderly self-association, so that the number of remaining free hydroxyl groups that can be combined with water molecules through hydrogen bonds is relatively reduced, and in this process, agar is added, and its molecules are arranged in a directional manner as the mixture is cooled to form a three-dimensional network structure, and the starch molecules are evenly fixed in the grid, thereby assisting the matrix to enhance the water resistance and strength. The invention discloses a novel nanostructured carbon foam, which is a kind of nanostructured carbon foam, and has the advantages of good mechanical properties and biodegradability. It utilizes ferric oxyhydroxide, sodium alginate and carboxymethyl cellulose to undergo graft copolymerization with polyacrylic acid as a carrier under the induction of gamma rays. Irradiation increases the number of free radicals generated by the mixture, and forms active sites for initiating polymerization in the matrix. The ferric oxyhydroxide and acrylic acid produce a complexation, so that the ferric oxyhydroxide particles are fixed in the matrix, providing an electron channel for the release of microbial cells and accelerating the biodegradation progress of the matrix. Its rigidity can also enhance the mechanical properties of the matrix. Hydrogen bonds are formed between the components in carboxymethyl cellulose and sodium alginate, which improves the water resistance of the matrix. At the same time, the good compatibility between sodium alginate and starch molecules reduces the gap between the matrix skeleton and makes the structure denser, thereby improving the water resistance and mechanical properties.

[0049] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing biodegradable resin particles, characterized in that: The method comprises the following preparation steps: (1) oxalic acid and dimethyl sulfoxide were mixed, stirred at 50-100 rpm for 15-30 min, corn starch and deionized water were added, the temperature was raised to 100-130°C, stirring was continued for 5-15 min, benzene, toluene and pyridine were added, and high-speed shearing was performed at a shear rate of 400-800 rpm for 10-25 min, agar was then added, and stirring was performed at 100-250 rpm for 1-3 h, cooled to room temperature, ethanol was added, and stirring was performed at 50-100 rpm until precipitation occurred, and the mixture was allowed to stand for 20-40 min, filtered, and the solid was taken out, and then washed with ethanol and deionized water three times each, dried at 30-50°C for 6-9 h, crushed, and sieved to obtain intermediate A; (2) Sodium alginate, carboxymethyl cellulose, ferric oxide dispersion and deionized water are mixed, heated to 60-80°C in a nitrogen atmosphere, stirred at 50-100 rpm for 20-40 min, cooled to room temperature, polyacrylic acid is added, and the pH of the solution is adjusted to 7-8 with a 20 wt % sodium hydroxide aqueous solution, heated to 50-80°C, stirred at 100-200 rpm for 1-3 h, N,N-methylenebisacrylamide is added, and stirring is continued for 15 min, then placed in a γ-ray radiation field for irradiation, then soaked in methanol for 3-6 h, dried at 50-80°C for 4-8 h, crushed, and passed through a 10-20 mesh sieve to obtain copolymer particles; (3) The copolymer particles, the intermediate A and acetyl tributyl citrate are mixed and extruded to obtain biodegradable resin particles.

2. The method for preparing biodegradable resin particles according to claim 1, characterized in that: The mesh size of the sieve in step (1) is 60-130 meshes.

3. The method for preparing biodegradable resin particles according to claim 1, characterized in that: The mass ratio of oxalic acid, dimethyl sulfoxide, corn starch, deionized water, benzene, toluene, pyridine, agar and ethanol in step (1) is 3:5:3~8:10~30:2:1:0.1:1~2:

20.

4. The method for preparing biodegradable resin particles according to claim 1, characterized in that: The preparation method of the oxyhydroxide dispersion in step (2) is as follows: oxyhydroxide and deionized water are mixed in a mass ratio of 1:30-60, and ultrasonically dispersed at 21 kHz for 10-30 minutes to obtain the dispersion.

5. The method for preparing biodegradable resin particles according to claim 1, characterized in that: The molecular weight of the polyacrylic acid in step (2) is 2000.

6. The method for preparing biodegradable resin particles according to claim 1, characterized in that: The irradiation parameters of step (2) are as follows: radiation dose of 3-10 kGy, temperature of 60-80°C, and time of 1-3 min.

7. The method for preparing biodegradable resin particles according to claim 1, characterized in that: The mass ratio of the sodium alginate, carboxymethyl cellulose, ferric oxyhydroxide dispersion, deionized water, polyacrylic acid and N,N-methylenebisacrylamide in step (2) is 1:1:0.6:10-50:4-15:0.

1.

8. The method for preparing biodegradable resin particles according to claim 1, characterized in that: The temperature of the extrusion granulation in step (3) is 130-150°C.

9. The method for preparing biodegradable resin particles according to claim 1, characterized in that: The mass ratio of the copolymer particles, the intermediate A and acetyl tributyl citrate in step (3) is 10:2-4:0.5.