A preparation method of titanium chrome brown composition
Through dry surface treatment after wet grinding and solid-phase synthesis, combined with composite dispersant and modifier, a titanium-chromium brown composition with excellent performance was prepared, which solved the pollution, energy consumption and performance problems in traditional processes and achieved the goal of achieving the It is highly efficient and environmentally friendly titanium chromium brown preparation, suitable for high-demand coatings.
Patent Information
- Application Number
- CN202411150482.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing titanium chrome brown preparation process has problems such as high pollution, high energy consumption and poor performance, and traditional pigments cannot meet the needs of the high-demand coating field.
After wet grinding and solid phase synthesis treatment, high-temperature crystal transformation is carried out, quenched cooling and added composite dispersant, modifier and polyol, titanium chromium brown composition is prepared through dry surface treatment, and the recycled waste resources are used to reduce costs. and improve performance.
It has achieved good coloring, firmness, stability, water resistance and heat resistance of titanium chrome brown, solved the problem of waste pollution, simple process, and is suitable for industrial production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention specifically relates to a method for preparing a titanium chrome brown composition. Background Art
[0002] Titanium chrome brown is yellowish yellow to reddish yellow brown. It is compatible with most thermoplastic and thermosetting resins and is an internationally recognized non-toxic and environmentally friendly pigment. Titanium chrome brown is a transition metal oxide pigment. Its main components include chromium, antimony and titanium oxides. It is easy to disperse, has good hiding power, excellent light resistance, weather resistance, heat stability, chemical resistance, no bleeding and migration. Traditional pigments, whether organic or inorganic, do not have the aforementioned comprehensive functions. Therefore, titanium chrome brown is suitable for high-demand coating fields such as exterior wall coatings, fluorocarbon coatings, architectural coatings, engineering machinery coatings and high-temperature resistant coatings. It can also be used in fields such as general plastics, special plastics, colored glass, building materials and ceramics, colored inks and colored sand and gravel.
[0003] At present, the preparation of titanium chrome brown generally adopts the traditional process, that is, various coloring oxides and additives are mixed evenly by ball milling in a certain proportion, and then calcined at high temperature and ball milled to a certain fineness. The above process has the problems of high pollution and high energy consumption, and the obtained titanium chrome brown has poor performance and limited application. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method for preparing a titanium chrome brown composition having good coloring, firmness, stability, water resistance and heat resistance, solving waste pollution, realizing resource recycling, simple process, low cost and suitable for industrial production.
[0005] The technical solution adopted by the present invention to solve the technical problem is as follows: a method for preparing a titanium chrome brown composition, comprising the following steps:
[0006] (1) Ti2O3, Cr2O3, SbFeO4 and additives are mixed, wet-ground, dried and crushed to obtain a mixture;
[0007] (2) subjecting the mixture obtained in step (1) to solid phase synthesis treatment, and then subjecting it to high temperature crystal transformation, rapid cooling, and grinding to obtain a microparticle mixture;
[0008] (3) Adding a composite dispersant, a modifier and a polyol to the particle mixture obtained in step (2), stirring and grinding the mixture to obtain a titanium chrome brown composition.
[0009] Preferably, in step (1), the mass ratio of Ti2O3, Cr2O3, SbFeO4 and the additive is 5-8:1-2:2-3:1.
[0010] Preferably, in step (1), the auxiliary agent is lithium fluoride, sodium tetraborate, potassium carbonate, cerium oxide and rubidium oxide mixed in a mass ratio of 1:0.5-1.5:0.5-1.5:0.5-1.5:0.5-1.5. The method of the present invention plays a role of embedding into the crystal lattice and reducing energy by adding lithium fluoride, plays a role of reducing the melting point of the curing reaction by adding sodium tetraborate, plays a role of improving the particle shape in the curing reaction by adding potassium carbonate, and plays a role of improving the color in the curing reaction by adding cerium oxide and rubidium oxide.
[0011] Preferably, in step (1), the wet grinding time is 30 to 50 hours. Wet grinding can fully crush the raw materials to promote uniform mixing.
[0012] Preferably, in step (1), the Ti2O3 is recovered from titanium oxide slurry. The titanium oxide slurry used in the present invention is derived from a chemical plant.
[0013] Preferably, the method for recovering Ti2O3 from titanium oxide slurry is: centrifuging the waste titanium oxide slurry, filtering the sediment, and obtaining Ti2O3. Ti2O3 is recovered based on the characteristics of components of different densities being separated in a gravity field, with heavier Ti2O3 precipitating at the bottom and impurities floating on the liquid surface.
[0014] Preferably, the mass content of titanium in the waste titanium oxide slurry is 25-35%.
[0015] Preferably, in step (1), the Cr2O3 is recovered from chromic acid mud. The chromic acid mud used in the present invention comes from a chromium salt plant.
[0016] Preferably, the method for recovering Cr2O3 from chromate-containing mud is as follows: putting chromate-containing mud into sodium chromate solution, stirring and heating to react, first adding waste acid water to react, then adding ammonia water to adjust the solution to neutrality, filtering by pressure, washing the filter residue, and roasting to obtain Cr2O3. In the preparation method of the present invention, chromate-containing mud and sodium chromate neutral solution react under heating, and acid water is added to generate insoluble chromium chromate precipitate, which is separated from other salts, thereby achieving the purpose of recovering trivalent chromium in chromate-containing mud.
[0017] Preferably, the mass content of chromium in the chromic acid mud is 16-18%.
[0018] Preferably, the mass volume ratio of the chromate-containing mud to the sodium chromate solution is 1:11-12 (kg / L).
[0019] Preferably, the molar concentration of the sodium chromate solution is 0.5-0.6 mol / L.
[0020] Preferably, the stirring and heating reaction is carried out at a temperature of 70 to 90° C. and for a time of 2 to 4 hours.
[0021] Preferably, the volume ratio of the waste acid water to the sodium chromate solution is 1 to 2:1.
[0022] Preferably, the pH value of the waste acid water is 1.5-2.0.
[0023] Preferably, the temperature of adding waste acid water to react is 80-100° C. and the time is 5-8 hours.
[0024] Preferably, the mass concentration of the ammonia water is 25-30%.
[0025] Preferably, the calcination temperature is 800-1000° C. and the calcination time is 2-4 hours.
[0026] Preferably, in step (1), the SbFeO4 is recovered from antimony smelting slag. The antimony smelting slag used in the present invention comes from an antimony smelting plant.
[0027] Preferably, the method for recovering SbFeO4 from antimony smelting slag is as follows: adding antimony smelting slag to a leaching solution, performing a leaching reaction, adding ferrous chloride, performing a precipitation reaction, filtering and separating, washing, and drying to obtain SbFeO4. Antimony in the antimony smelting slag is dissolved in an alkaline leaching solution, reacting with ferrous chloride to generate SbFeO4 precipitate, and the SbFeO4 is filtered, separated, washed, and roasted to remove impurities, thereby obtaining a SbFeO4 product with a higher purity.
[0028] Preferably, the mass content of antimony in the antimony smelting slag is 15-20%.
[0029] Preferably, the mass volume ratio of the antimony smelting slag to the leaching solution is 1:10-11 (kg / L).
[0030] Preferably, the leaching solution is a mixed solution of ammonium chloride and sodium hydroxide, wherein the molar concentration of ammonium chloride is 0.1-0.2 mol / L, and the molar concentration of sodium hydroxide is 0.2-0.5 mol / L.
[0031] Preferably, the leaching reaction temperature is 150-170° C., the total pressure is 1.3-1.5 MPa, and the time is 8-10 h. During the leaching process, the pH value of the leaching solution is adjusted to 12-14.
[0032] Preferably, the amount of ferrous chloride used is equivalent to 0.3 to 0.5 times the mass of antimony smelting slag.
[0033] Preferably, the precipitation reaction temperature is 50-60° C. and the time is 4-7 hours.
[0034] The main components of the titanium chrome brown composition obtained by the method of the present invention, titanium, chromium and antimony, are all taken from wastes. The titanium is taken from waste titanium oxide slurry, the chromium is taken from waste chromic acid mud from a chromium salt plant, and the antimony is taken from antimony smelting slag. This solves the problem of waste pollution, realizes the recycling of resources, is beneficial to environmental protection, and has great prospects for promotion.
[0035] Preferably, in step (2), the temperature of the solid phase synthesis treatment is 200-300°C, the pressure is 0.1-0.3 MPa, and the time is 2-5 hours. The method of the present invention can make Ti2O3, Cr2O3, SbFeO4 and the auxiliary agent be combined into one metal coordination compound that is difficult to synthesize in the wet mixing through solid phase synthesis treatment.
[0036] Preferably, in step (2), the temperature of the high temperature crystal transformation is 820-1150° C. and the time is 3-6 hours. The method of the present invention stabilizes the structure of the solid phase synthesis reactants by coordinating the crystal transformation.
[0037] Preferably, in step (2), rapid cooling is carried out in a rapid cooling water tower.
[0038] Preferably, in step (3), the mass ratio of the composite dispersant, the modifier and the polyol is 1:1-1.5:0.5-1.0.
[0039] Preferably, in step (3), the total mass of the composite dispersant, modifier and polyol is equivalent to 10-20% of the total mass of Ti2O3, Cr2O3, SbFeO4 and additives in step (1).
[0040] Preferably, in step (3), the grinding speed is 500-1000 r / min and the grinding time is 2-5 h. In the preparation method of the present invention, dry surface treatment is performed based on grinding, so that the average particle size of the titanium chrome brown composition is reduced, the specific surface area is increased, and the agglomerated particles of the titanium chrome brown composition are deagglomerated.
[0041] Preferably, in step (3), the composite dispersant is prepared by mixing tertiary amine salt, polyhydroxystearic acid, naphthalenesulfonic acid formaldehyde condensate salt and propylene carbonate in a mass ratio of 1:1-3:0.5-1.5:2-4. The composite dispersant used in the method of the present invention has a tertiary amine group, a hydroxyl group, a benzene ring and an ester group. Compared with a dispersant with a single group, it has a multi-component mixed structure and has a multi-polar group. The tertiary amine salt provides the tertiary amine group, the naphthalenesulfonic acid formaldehyde condensate salt provides the benzene ring, the polyhydroxystearic acid provides the hydroxyl group, and the propylene carbonate provides the ester group. The excellent dispersing effect of the tertiary amine group and the benzene ring is utilized, the dispersibility and color development of the ester group are coordinated, and the dispersibility of the ester group is combined to interact with each other, so that the dispersing effect is enhanced when the components of the titanium chrome brown composition are mixed, so that the mixed system is in a stable state.
[0042] Preferably, in step (3), the modifier is mixed with bromine, carbamate, sodium carboxymethyl cellulose and glycerol in a mass ratio of 1:0.5-1.5:1-3:0.5-1.5. The method of the present invention changes the chemical structure of titanium chrome brown by a modifier, increases the relative molecular mass of titanium chrome brown and changes the molecular structure, so as to achieve the effect of improving the stability of titanium chrome brown, which is specifically manifested as: introducing halogenated atoms by bromine to make the titanium chrome brown bright in color, and improving the coloring and fastness of the dye, grafting polar groups by carbamate to form a water-rich layer on the surface of titanium chrome brown particles, and combining sodium carboxymethyl cellulose and glycerol for condensation and moisturizing, thereby enhancing the water resistance and heat resistance of titanium chrome brown.
[0043] Preferably, in step (3), the polyol is one or more of trimethylolethane, xylitol, sorbitol or pentaerythritol, etc. The present invention adds polyols to improve the properties of titanium chrome brown, such as dispersibility, polarity, etc., so as to be suitable for different application scenarios.
[0044] The beneficial effects of the method of the present invention are as follows:
[0045] (1) The method of the present invention adopts dry surface treatment to mix the components of the titanium chrome brown composition. The dispersibility of the titanium chrome brown after dry surface treatment in water is improved, and the sedimentation rate is slowed down, the average particle size is reduced, and the specific surface area is increased. The agglomerated particles of the titanium chrome brown composition are partially deagglomerated, and are easy to disperse in the application system and have a better fineness value. The obtained titanium chrome brown has good coloring, firmness, stability, water resistance and heat resistance.
[0046] (2) The method of the present invention solves waste pollution, realizes resource recycling, and is beneficial to environmental protection;
[0047] (3) The method of the present invention has simple process, low cost and is suitable for industrial production. DETAILED DESCRIPTION
[0048] The present invention will be further described below in conjunction with the embodiments.
[0049] The chromic acid mud used in the embodiment of the present invention comes from a chromium salt plant, and the mass content of chromium is 17%; the antimony smelting slag used comes from an antimony smelting plant, and the mass content of antimony is 18%; the titanium oxide slurry used in the present invention comes from a chemical plant, and the mass content of titanium is 30%; the raw materials or chemical reagents used in the embodiment of the present invention, unless otherwise specified, are obtained through conventional commercial channels.
[0050] Example 1
[0051] (1) 50 g Ti2O3, 12 g Cr2O3, 15 g SbFeO4 and 7 g additive were mixed, wet-ground for 35 h, dried, and crushed to obtain a mixture;
[0052] The Ti2O3 is recovered from titanium oxide slurry by centrifuging the waste titanium oxide slurry, filtering the precipitate, and obtaining Ti2O3;
[0053] The Cr2O3 is recovered from the chromic acid mud, and the recovery method is as follows: 3 kg of chromic acid mud is put into 33 L of 0.5 mol / L sodium chromate solution, stirred and heated to 85°C for reaction for 2.5 hours, and then 36 L of waste acid water with a pH value of 1.5 is added, and the reaction is carried out at 80°C for 5 hours, and then ammonia water with a mass concentration of 25% is added to adjust the solution to neutrality, filter by pressure, wash the filter residue, and roast at 800°C for 2 hours to obtain Cr2O3;
[0054] The SbFeO4 is recovered from antimony smelting slag, and the recovery method is as follows: 3 kg of antimony smelting slag is added to 30 L of a mixed solution of ammonium chloride and sodium hydroxide (the molar concentration of ammonium chloride is 0.1 mol / L, and the molar concentration of sodium hydroxide is 0.2 mol / L), and the mixture is subjected to leaching reaction at 150° C. and a total pressure of 1.3 MPa for 8 hours. During the leaching process, the pH value of the leaching solution is adjusted to 13, 1 kg of ferrous chloride is added, and the mixture is subjected to precipitation reaction at 50° C. for 4 hours, and then filtered, separated, washed, and dried to obtain SbFeO4;
[0055] The auxiliary agent is formed by mixing lithium fluoride, sodium tetraborate, potassium carbonate, cerium oxide and rubidium oxide in a mass ratio of 1:0.5:0.5:0.5:0.5; in this embodiment, the addition of lithium fluoride plays a role in embedding into the crystal lattice and reducing energy, the addition of sodium tetraborate plays a role in reducing the melting point of the curing reaction, the addition of potassium carbonate plays a role in improving the particle shape in the curing reaction, and the addition of cerium oxide and rubidium oxide plays a role in improving the color in the curing reaction;
[0056] (2) The mixture obtained in step (1) is first subjected to solid phase synthesis treatment at 220° C. and 0.22 MPa for 4 h, then subjected to high temperature crystal transformation at 820° C. for 4.5 h, quenched in a quenching water tower, and ground to obtain a microparticle mixture;
[0057] (3) Add 4 g of composite dispersant, 5 g of modifier and 2 g of trimethylolethane to the microparticle mixture obtained in step (2), stir evenly, and grind at a speed of 500 r / min for 5 h to obtain a titanium chrome brown composition;
[0058] In this embodiment, the particle mixture formed by the crystal transformation is ground, and the components of the titanium chrome brown composition are mixed by dry surface treatment. The dispersibility of the titanium chrome brown composition after the dry surface treatment in water is improved, and the sedimentation rate is slowed down, the average particle size is reduced, and the specific surface area is increased. The agglomerated particles of the titanium chrome brown composition are partially depolymerized, and are easy to disperse in the application system, and have a better fineness value;
[0059] The composite dispersant is formed by mixing tertiary amine salt, polyhydroxystearic acid, naphthalenesulfonic acid formaldehyde condensate salt and propylene carbonate in a mass ratio of 1:2:1.5:3; the composite dispersant in this embodiment has a tertiary amine group, a hydroxyl group, a benzene ring and an ester group. Compared with a dispersant with a single group, the composite dispersant in this embodiment is a multi-component mixed structure with a multi-polar group. The tertiary amine salt provides the tertiary amine group, the naphthalenesulfonic acid formaldehyde condensate salt provides the benzene ring, the polyhydroxystearic acid provides the hydroxyl group, and the propylene carbonate provides the ester group. The excellent dispersing effect of the tertiary amine group and the benzene ring is used, the dispersibility and color development of the ester group are coordinated, and the dispersibility of the ester group is combined to interact with each other, so that the dispersing effect is enhanced when the components of the titanium chrome brown composition are mixed, so that the mixed system is in a stable state;
[0060] The modifier is prepared by mixing bromine, carbamate, sodium carboxymethyl cellulose and glycerol in a mass ratio of 1:1.5:2:0.5. In this embodiment, the chemical structure of titanium chrome brown is changed by the modifier, the relative molecular mass of titanium chrome brown is increased and the molecular structure is changed to achieve the effect of improving the stability of titanium chrome brown, which is specifically manifested as follows: halogenated atoms are introduced by bromine to make the titanium chrome brown color bright, and the coloring and fastness of the dye are improved; polar groups are grafted by carbamate to form a water-rich layer on the surface of titanium chrome brown particles, and sodium carboxymethyl cellulose and glycerol are combined for condensation and moisturizing, thereby enhancing the water resistance and heat resistance of titanium chrome brown.
[0061] Example 2
[0062] (1) 70 g Ti2O3, 20 g Cr2O3, 30 g SbFeO4 and 12 g additive were mixed, wet-ground for 45 h, dried, and crushed to obtain a mixture;
[0063] The Ti2O3 is recovered from titanium oxide slurry by centrifuging the waste titanium oxide slurry, filtering the precipitate, and obtaining Ti2O3;
[0064] The Cr2O3 is recovered from the chromic acid mud, and the recovery method is as follows: 2 kg of chromic acid mud is put into 24 L of 0.5 mol / L sodium chromate solution, stirred and heated to 80°C for reaction for 3 hours, and then 30 L of waste acid water with a pH value of 2 is added, and the reaction is carried out at 90°C for 6 hours, and then ammonia water with a mass concentration of 27% is added to adjust the solution to neutrality, filter by pressure, wash the filter residue, and roast at 850°C for 3 hours to obtain Cr2O3;
[0065] The SbFeO4 is recovered from antimony smelting slag, and the recovery method is: add 2kg of antimony smelting slag to 22L of a mixed solution of ammonium chloride and sodium hydroxide (the molar concentration of ammonium chloride is 0.2mol / L, and the molar concentration of sodium hydroxide is 0.3mol / L), and carry out a leaching reaction at 160°C and a total pressure of 1.38MPa for 9h. During the leaching process, adjust the pH value of the leachate to 14, add 1kg of ferrous chloride, and carry out a precipitation reaction at 55°C for 5h, filter and separate, wash, and dry to obtain SbFeO4;
[0066] The auxiliary agent is prepared by mixing lithium fluoride, sodium tetraborate, potassium carbonate, cerium oxide and rubidium oxide in a mass ratio of 1:0.6:0.8:1:0.5;
[0067] (2) The mixture obtained in step (1) is first subjected to solid phase synthesis treatment at 220° C. and 0.22 MPa for 3 h, then subjected to high temperature crystal transformation at 900° C. for 4.2 h, and then subjected to rapid cooling in a rapid cooling water tower and grinding to obtain a microparticle mixture;
[0068] (3) Add 8 g of composite dispersant, 9 g of modifier and 4 g of xylitol to the microparticle mixture obtained in step (2), stir evenly, and grind at a speed of 700 r / min for 4 h to obtain a titanium chrome brown composition;
[0069] The composite dispersant is prepared by mixing tertiary amine salt, polyhydroxystearic acid, naphthalenesulfonic acid formaldehyde condensate salt and propylene carbonate in a mass ratio of 1:1:0.5:2;
[0070] The modifier is prepared by mixing bromine, carbamate, sodium carboxymethyl cellulose and glycerol in a mass ratio of 1:1.5:3:1.5.
[0071] Example 3
[0072] (1) 60 g Ti2O3, 15 g Cr2O3, 20 g SbFeO4 and 10 g additive were mixed, wet-ground for 40 h, dried, and crushed to obtain a mixture;
[0073] The Ti2O3 is recovered from titanium oxide slurry by centrifuging the waste titanium oxide slurry, filtering the precipitate, and obtaining Ti2O3;
[0074] The Cr2O3 is recovered from the chromic acid mud, and the recovery method is as follows: 4 kg of chromic acid mud is put into 45 L of 0.55 mol / L sodium chromate solution, stirred and heated to 80°C for reaction for 3 hours, and then 60 L of waste acid water with a pH value of 1.5 is added, and the reaction is carried out at 95°C for 7 hours, and then ammonia water with a mass concentration of 30% is added to adjust the solution to neutrality, filter by pressure, wash the filter residue, and roast at 900°C for 2 hours to obtain Cr2O3;
[0075] The SbFeO4 is recovered from antimony smelting slag, and the recovery method is as follows: 1 kg of antimony smelting slag is added to 10 L of a mixed solution of ammonium chloride and sodium hydroxide (the molar concentration of ammonium chloride is 0.15 mol / L, and the molar concentration of sodium hydroxide is 0.4 mol / L), and the mixture is subjected to leaching reaction at 150° C. and a total pressure of 1.4 MPa for 8 hours. During the leaching process, the pH value of the leaching solution is adjusted to 14, 0.5 kg of ferrous chloride is added, and the mixture is subjected to precipitation reaction at 60° C. for 6 hours, filtered, separated, washed, and dried to obtain SbFeO4;
[0076] The auxiliary agent is prepared by mixing lithium fluoride, sodium tetraborate, potassium carbonate, cerium oxide and rubidium oxide in a mass ratio of 1:1:1.5:1:1.5;
[0077] (2) The mixture obtained in step (1) is first subjected to solid phase synthesis treatment at 240° C. and 0.24 MPa for 2 h, then subjected to high temperature crystal transformation at 850° C. for 4.2 h, quenched in a quenching water tower, and ground to obtain a microparticle mixture;
[0078] (3) Add 6 g of composite dispersant, 7 g of modifier and 3 g of sorbitol to the microparticle mixture obtained in step (2), stir evenly, and grind at a speed of 900 r / min for 3 h to obtain a titanium chrome brown composition;
[0079] The composite dispersant is prepared by mixing tertiary amine salt, polyhydroxystearic acid, naphthalenesulfonic acid formaldehyde condensate salt and propylene carbonate in a mass ratio of 1:2:1:3;
[0080] The modifier is prepared by mixing bromine, carbamate, sodium carboxymethyl cellulose and glycerol in a mass ratio of 1:1:2:1.
[0081] Example 4
[0082] (1) 66 g Ti2O3, 18 g Cr2O3, 25 g SbFeO4 and 11 g additive were mixed, wet-ground for 40 h, dried, and crushed to obtain a mixture;
[0083] The Ti2O3 is recovered from titanium oxide slurry by centrifuging the waste titanium oxide slurry, filtering the precipitate, and obtaining Ti2O3;
[0084] The Cr2O3 is recovered from the chromic acid mud, and the recovery method is as follows: 1 kg of chromic acid mud is put into 12 L of 0.6 mol / L sodium chromate solution, stirred and heated to 75°C for reaction for 3.5 hours, and then 14 L of waste acid water with a pH value of 1.5 is added, and the reaction is carried out at 100°C for 8 hours, and then ammonia water with a mass concentration of 28% is added to adjust the solution to neutrality, filter by pressure, wash the filter residue, and roast at 1000°C for 4 hours to obtain Cr2O3;
[0085] The SbFeO4 is recovered from antimony smelting slag, and the recovery method is: add 1.5 kg of antimony smelting slag to 15 L of a mixed solution of ammonium chloride and sodium hydroxide (the molar concentration of ammonium chloride is 0.2 mol / L, and the molar concentration of sodium hydroxide is 0.5 mol / L), and carry out a leaching reaction at 170° C. and a total pressure of 1.5 MPa for 10 hours. During the leaching process, adjust the pH value of the leachate to 14, add 0.6 kg of ferrous chloride, and carry out a precipitation reaction at 60° C. for 7 hours, filter and separate, wash, and dry to obtain SbFeO4;
[0086] The auxiliary agent is prepared by mixing lithium fluoride, sodium tetraborate, potassium carbonate, cerium oxide and rubidium oxide in a mass ratio of 1:1:1:1:1;
[0087] (2) The mixture obtained in step (1) is first subjected to solid phase synthesis treatment at 200° C. and 0.20 MPa for 5 h, then subjected to high temperature crystal transformation at 1000° C. for 4 h, and then subjected to rapid cooling in a rapid cooling water tower and grinding to obtain a microparticle mixture;
[0088] (3) Add 7 g of composite dispersant, 7 g of modifier and 6 g of pentaerythritol to the microparticle mixture obtained in step (2), stir evenly, and grind at a speed of 1000 r / min for 2 h to obtain a titanium chrome brown composition;
[0089] The composite dispersant is prepared by mixing tertiary amine salt, polyhydroxystearic acid, naphthalenesulfonic acid formaldehyde condensate salt and propylene carbonate in a mass ratio of 1:3:1.3:4;
[0090] The modifier is prepared by mixing bromine, carbamate, sodium carboxymethyl cellulose and glycerol in a mass ratio of 1:1.2:2:0.9.
[0091] Comparative Example 1
[0092] The difference between this comparative example and Example 2 is that no auxiliary agent is added in step (1). The rest is the same as Example 2.
[0093] Comparative Example 2
[0094] The difference between this comparative example and Example 2 is that in step (2), no solid phase synthesis treatment is performed. The rest is the same as Example 2.
[0095] Comparative Example 3
[0096] The difference between this comparative example and Example 2 is that in step (3), no composite dispersant and modifier are added. The rest is the same as Example 2.
[0097] According to the provisions of GB / T 5211.5-2008 "Method for Determination of Pigment Resistance", commercially available titanium chrome brown pigment was used as a control group, and the performance of the titanium chrome brown composition obtained in Examples 1 to 4 of the present invention and Comparative Examples 1 to 3 and the control group was tested. The test results are shown in Table 1:
[0098]
[0099] Note: In the table, the higher the grade from 1 to 5, the better the acid resistance, alkali resistance or oil resistance.
[0100] As can be seen from Table 1, Examples 1 to 4 of the present invention use dry surface treatment to mix the components of titanium chrome brown. The dispersibility of the titanium chrome brown after dry surface treatment in water is improved, and the sedimentation rate is slowed down and the average particle size is reduced. Since the particle size is smaller, the number of titanium chrome brown particles per unit volume is increased, which has the characteristic of a larger specific surface area, so that the agglomerated particles of titanium chrome brown are partially depolymerized, easy to disperse in the application system, and have a better fineness value. The obtained titanium chrome brown has good coloring, firmness, stability, water resistance and heat resistance.
Claims
1. A method for preparing a titanium chrome brown composition, characterized in that: The following steps are involved: (1) Ti2O3, Cr2O3, SbFeO4 and additives are mixed, wet-ground, dried and crushed to obtain a mixture; The mass ratio of Ti2O3, Cr2O3, SbFeO4 and the auxiliary agent is 5-8:1-2:2-3:1; the auxiliary agent is prepared by mixing lithium fluoride, sodium tetraborate, potassium carbonate, cerium oxide and rubidium oxide in a mass ratio of 1:0.5-1.5:0.5-1.5:0.5-1.5:0.5-1.5; the wet grinding time is 30-50h; The SbFeO4 is recovered from antimony smelting slag; the method for recovering SbFeO4 from antimony smelting slag is as follows: adding antimony smelting slag to leaching solution, performing leaching reaction, adding ferrous chloride, performing precipitation reaction, filtering and separating, washing, and drying to obtain SbFeO4; the mass content of antimony in the antimony smelting slag is 15-20%; the mass volume ratio of the antimony smelting slag to the leaching solution is 1:10-11 in kg / L; the leaching solution is a mixed solution of ammonium chloride and sodium hydroxide, The molar concentration of ammonium chloride is 0.1-0.2 mol / L, and the molar concentration of sodium hydroxide is 0.2-0.5 mol / L; the temperature of the leaching reaction is 150-170°C, the total pressure is 1.3-1.5 MPa, and the time is 8-10 hours. During the leaching process, the pH value of the leaching solution is adjusted to 12-14; the amount of ferrous chloride used is equivalent to 0.3-0.5 times the mass of antimony smelting slag; the temperature of the precipitation reaction is 50-60°C, and the time is 4-7 hours; (2) subjecting the mixture obtained in step (1) to solid phase synthesis treatment, and then subjecting it to high temperature crystal transformation, rapid cooling, and grinding to obtain a microparticle mixture; (3) adding a composite dispersant, a modifier and a polyol to the particle mixture obtained in step (2), stirring and grinding to obtain a titanium chrome brown composition; The composite dispersant is obtained by mixing tertiary amine salt, polyhydroxystearic acid, naphthalenesulfonic acid formaldehyde condensate salt and propylene carbonate; the modifier is obtained by mixing bromine, carbamate, sodium carboxymethyl cellulose and glycerol; the mass ratio of the tertiary amine salt, polyhydroxystearic acid, naphthalenesulfonic acid formaldehyde condensate salt and propylene carbonate is 1:1-3:0.5-1.5:2-4; the mass ratio of the bromine, carbamate, sodium carboxymethyl cellulose and glycerol is 1:0.5-1.5:1-3:0.5-1.5; the mass ratio of the composite dispersant, modifier and polyol is 1:1-1.5:0.5-1.0; the total mass of the composite dispersant, modifier and polyol is equivalent to 10-20% of the total mass of Ti2O3, Cr2O3, SbFeO4 and additives in step (1).
2. The method for preparing the titanium chrome brown composition according to claim 1, characterized in that: In step (1), the Ti2O3 is recovered from titanium oxide slurry; the method for recovering the Ti2O3 from the titanium oxide slurry is: centrifuging the waste titanium oxide slurry, precipitating and filtering to obtain Ti2O3; the mass content of titanium in the waste titanium oxide slurry is 25-35%.
3. The method for preparing the titanium chrome brown composition according to claim 1, characterized in that: In step (1), the Cr2O3 is recovered from the chromate-containing mud; the method for recovering the Cr2O3 from the chromate-containing mud is as follows: the chromate-containing mud is put into a sodium chromate solution, stirred and heated to react, then waste acid water is added to react, then ammonia water is added to adjust the solution to neutrality, filter-pressed, the filter residue is washed, and roasted to obtain Cr2O3; the mass content of chromium in the chromate-containing mud is 16-18%; the mass volume ratio of the chromate-containing mud to the sodium chromate solution is 1:11-12 kg / L; the chromate-containing mud is chromate-containing mud, and ... The molar concentration of the sodium chromate solution is 0.5-0.6 mol / L; the temperature of the stirring and heating reaction is 70-90°C, and the time is 2-4 hours; the volume ratio of the waste acid water to the sodium chromate solution is 1-2:1; the pH value of the waste acid water is 1.5-2.0; the temperature of the reaction of adding the waste acid water is 80-100°C, and the time is 5-8 hours; the mass concentration of the ammonia water is 25-30%; the temperature of the roasting is 800-1000°C, and the time is 2-4 hours.
4. The method for preparing the titanium chrome brown composition according to claim 1, characterized in that: In step (2), the temperature of the solid phase synthesis treatment is 200-300° C., the pressure is 0.1-0.3 MPa, and the time is 2-5 h; the temperature of the high temperature crystal transformation is 820-1150° C., and the time is 3-6 h; and rapid cooling is performed in a rapid cooling water tower.
5. The method for preparing the titanium chrome brown composition according to claim 1, characterized in that: In step (3), the grinding speed is 500-1000 r / min and the grinding time is 2-5 h; the polyol is one or more of trimethylolethane, xylitol, sorbitol or pentaerythritol.
Citation Information
Patent Citations
Metal-oxide mixed-phase titanium-chromium brown pigment and preparation process thereof
CN102532953A
Pigment-dispersed resist composition for color filters and pigment dispersion resist composition for color filter
CN112011193A
Preparation method of beta-naphthalenesulfonic acid formaldehyde condensate
CN116332805A
Near-infrared titanium gold mixed-phase pigment and preparation method thereof
CN117487380A
Superfine particle yellow pigment and its production
JP1992170323A