A kind of thermal insulation and sound insulation coating used on building floor and preparation method thereof
Through the silicone network structure formed by acrylic resin and ethyl orthosilicate and other materials, combined with polyester fiber, ammonium polyphosphate and lignin, an efficient thermal insulation and sound insulation coating for building floors is prepared, which solves the environmental protection of existing materials. The shortcomings in waterproofness, flame retardancy and earthquake resistance have achieved diversified performance improvement and construction simplification.
Patent Information
- Application Number
- CN202411110318.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing building floor insulation materials have shortcomings in environmental protection, waterproofing, flame retardant and seismic resistance, which are difficult to meet diversified needs, and are complex in construction and high in cost.
The insulation and sound insulation coating with acrylic resin and ethyl orthosilicate as the main components is prepared by forming a three-dimensional silicone network structure and combining polyester fibers, ammonium polyphosphate and lignin and other materials to prepare good sound insulation, shock resistance and heat insulation. , a sound-silence modifier with waterproof performance, forming an efficient thermal insulation coating.
It has achieved diversified performance improvement of building floor slabs, simplified the construction process, reduced construction costs, improved sound insulation, enhanced waterproof and flame retardant performance, and is suitable for a variety of building environments to meet the needs of green buildings and energy conservation and emission reduction.
Smart Images

Figure CN118652595B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of modified organic materials, and in particular relates to a thermal insulation and sound insulation coating used on building floors and a preparation method thereof. Background Art
[0002] With the acceleration of urbanization and the increase in population density, the thermal insulation and sound insulation of building floors have become the focus of social attention. Existing building materials often have problems such as poor effect, complex construction or high cost in achieving thermal insulation and sound insulation of floors. At the same time, due to environmental factors and safety regulations, building floor materials also need to have certain earthquake resistance and waterproof properties.
[0003] At present, most of the thermal insulation and sound insulation materials on the market are concentrated on the use of traditional rock wool, foam plastics and other materials. Although these materials have certain thermal insulation and sound insulation effects, they still have the following problems: First, the materials are not environmentally friendly enough and are difficult to degrade, which imposes a burden on the environment; second, the waterproof performance is not ideal and it is easy to absorb water or moisture, affecting its thermal insulation effect and the stability of the building structure; third, in the event of fire, the flame retardant performance of some materials is poor, posing a safety hazard; fourth, the seismic performance of most thermal insulation and sound insulation materials has not been effectively considered, and they cannot withstand the impact of earthquakes.
[0004] Therefore, the development of a coating that integrates sound insulation, earthquake resistance, thermal insulation and waterproofing, especially a thermal insulation and sound insulation coating used for building floors, will be of great significance to improving the performance of existing building materials, reducing construction difficulty and improving the safety of the building environment. Especially in the context of energy conservation and emission reduction and green buildings, efficient and environmentally friendly thermal insulation and sound insulation coatings have received widespread attention and research. Summary of the invention
[0005] 1. Problems to be solved
[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a thermal insulation and sound insulation coating for use on building floors and a preparation method thereof. The coating integrates four key properties of sound insulation, earthquake resistance, thermal insulation and waterproofness, and has a significant effect on meeting the diversified needs faced by building floors.
[0007] For acrylic resin and ethyl orthosilicate, acrylic resin: as a high molecular polymer matrix, it is mainly responsible for forming a continuous coating film in the coating, providing good adhesion, flexibility and chemical resistance. Acrylic resin can be well compatible with other components (such as fillers, pigments and additives) to form a uniform and stable coating system; ethyl orthosilicate: as a commonly used cross-linking agent or prepolymer, it can generate a silicon-oxygen network structure through hydrolysis and condensation reactions. When ethyl orthosilicate reacts with water molecules in the coating formula, it will gradually form a three-dimensional siloxane network structure. This structure significantly improves the mechanical strength, heat resistance, weather resistance and waterproof properties of the coating; during the coating curing process, the chemical conversions of acrylic resin and ethyl orthosilicate are as follows: Acrylic resin curing: Acrylic resin is cured by a free radical polymerization mechanism to form a polymer network. This process usually requires the introduction of The participation of a hair dryer (catalyst) and accelerated by heating or ultraviolet light irradiation; hydrolysis and condensation of ethyl orthosilicate: ethyl orthosilicate undergoes hydrolysis reaction with water to generate silicic acid alcohol, which then forms a cross-linked siloxane (-Si-O-Si-) network through condensation reaction; this process will occur simultaneously when the coating is cured, enhancing the overall performance of the coating. At the same time, the components mentioned in the preparation method - polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran - all play a unique role in the sound-absorbing modifier and contribute to the performance of the final product. The effects of these components are analyzed below: Polyester fiber: Polyester fiber has good elasticity and wear resistance, which can improve the durability of the modifier. In sound insulation materials, polyester fiber can effectively reduce the reflection of sound waves and enhance the sound insulation effect due to its good sound absorption performance. In addition, the introduction of polyester fiber can also improve the structural strength of the mixture. Ammonium polyphosphate: Ammonium polyphosphate is a commonly used flame retardant additive. By adding it to the sound-absorbing modifier, the flame retardant properties of the final coating can be significantly improved. This is because ammonium polyphosphate will decompose at high temperatures to form phosphoric acid or polyphosphoric acid, which can form a heat-insulating protective film to prevent the spread of flames. Lignin: Lignin is a natural high molecular polymer with good chemical stability. Its addition can improve the structure of the sound-absorbing modifier and enhance its ability to absorb and scatter sound waves. In addition, as a renewable resource, the use of lignin helps to improve the environmental friendliness of the material.
[0008] Tetrahydrofuran is an organic solvent, and its role here is mainly as a reaction medium, which helps the mixing and reaction of other ingredients. During the mixing process, tetrahydrofuran can promote the uniform dispersion between polyester fiber, ammonium polyphosphate and lignin, ensuring the balanced performance of the modifier. Excess tetrahydrofuran is then removed through centrifugation and washing steps to ensure the safety of the final product. By heating and stirring the mixture under nitrogen protection, it can promote full reaction and cross-linking between the components, thereby forming a structure with good sound insulation performance. After multiple washings and vacuum drying, a pure, stable sound-absorbing modifier can be obtained. In short, this method for preparing a sound-absorbing modifier cleverly utilizes the characteristics of each component to produce a high-quality modifier that has both good sound insulation performance and flame retardant and environmental protection properties. It can be widely used in thermal insulation and sound insulation coatings on building floors to improve their comprehensive performance.
[0009] 2. Technical solution
[0010] To solve the above problems, the technical solution provided by the present invention is: a thermal insulation and sound insulation coating used on building floors, which comprises the following raw materials in parts by weight: acrylic resin: 60 parts to 100 parts.
[0011] Ethyl orthosilicate: 40 parts to 50 parts.
[0012] Noise-absorbing modifier: 10-18 parts.
[0013] Polyol: 15-20 parts.
[0014] Flame retardant: 5-10 parts.
[0015] Foam stabilizer: 2-6 parts.
[0016] Foaming agent: 0.8 parts to 2 parts.
[0017] Catalyst: 0.02 parts - 0.1 parts.
[0018] Surfactant: 0.5 parts to 2 parts.
[0019] The preparation method of the sound-absorbing modifier is as follows: polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of (10-20): (5-10): (5-10): (50-60), heated to 75°C-85°C in an oil bath under nitrogen protection, stirred continuously for 4h-8h, centrifuged at 8000rpm for 10min, the precipitate is taken, washed three times with anhydrous ethanol, and vacuum dried.
[0020] The thermal insulation and sound insulation coating used on the building floor slab mentioned above comprises the following raw materials in parts by weight: acrylic resin: 70 parts to 90 parts.
[0021] Ethyl orthosilicate: 42 parts to 48 parts.
[0022] Noise-absorbing modifier: 12-16 parts.
[0023] Polyol: 15-20 parts.
[0024] Flame retardant: 5-10 parts.
[0025] Foam stabilizer: 2-6 parts.
[0026] Foaming agent: 0.8 parts to 2 parts.
[0027] Catalyst: 0.02 parts - 0.1 parts.
[0028] Surfactant: 0.5 parts to 2 parts.
[0029] The preparation method of the sound-absorbing modifier is as follows: polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of (15-20): (5-10): (8-10): (50-60), heated to 80°C-85°C in an oil bath under nitrogen protection, stirred continuously for 4h-8h, centrifuged at 8000rpm for 10min, the precipitate is taken, washed three times with anhydrous ethanol, and vacuum dried.
[0030] The thermal insulation and sound insulation coating used on the building floor slab mentioned above comprises the following raw materials in parts by weight: 80 parts of acrylic resin.
[0031] Ethyl orthosilicate: 45 parts.
[0032] Noise-absorbing modifier: 14 parts.
[0033] Polyol: 18 parts.
[0034] Flame retardant: 8 parts.
[0035] Foam stabilizer: 4 parts.
[0036] Foaming agent: 1.4 parts.
[0037] Catalyst: 0.07 parts.
[0038] Surfactant: 1.5 parts.
[0039] The preparation method of the sound-absorbing modifier is as follows: polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of 18:8:9:55, heated to 83°C in an oil bath under nitrogen protection, stirred continuously for 6 hours, centrifuged at 8000 rpm for 10 minutes, the precipitate is taken, washed three times with anhydrous ethanol, and vacuum dried.
[0040] The thermal insulation and sound insulation coating used on the building floor slabs described above, the physical and chemical properties of the acrylic resin are as follows: density is 1.2g / cm³, refractive index is 1.50, and glass transition temperature is 107°C.
[0041] The physical and chemical properties of the ethyl orthosilicate are as follows: density is 0.93 g / cm³, and refractive index is 1.43.
[0042] In the above-mentioned thermal insulation and sound insulation coating used on building floors, the polyol is one of ethylene glycol, propylene glycol, butylene glycol, trihydroxyethanol, glycerol, tetraethylene glycol, and pentaethylene glycol.
[0043] The flame retardant is one of hexabromodiphenyl ether, magnesium hydroxide, expanded graphite and nano-alumina.
[0044] The foam stabilizer is one of Tween-20, Tween-80, Span-20 and Span-80.
[0045] The catalyst is one of hydrogen peroxide, benzoyl peroxide, diisopropyl peroxide, triethylamine, diethanolamine and pyridine.
[0046] The surfactant is one of alkylphenol polyoxyethylene ether, allyl polyoxyalkyl ether and tetraalkylammonium chloride.
[0047] The method for preparing the thermal insulation and sound insulation coating used on the building floor as described above comprises the following steps: premixing: adding acrylic resin, polyol, flame retardant, foam stabilizer and surfactant into a stirring kettle, stirring at a low speed to obtain a mixture.
[0048] Add the sound-absorbing modifier: slowly add the sound-absorbing modifier into the mixture and stir evenly.
[0049] Adding ethyl orthosilicate: slowly add ethyl orthosilicate into the mixture and stir evenly.
[0050] Adding foaming agent: adding the foaming agent into the mixture and stirring evenly.
[0051] Adding catalyst: Add the catalyst into the mixture and stir well.
[0052] Degassing: Let the mixture stand to degas, and store in a cool place.
[0053] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on building floors, the pre-mixing and stirring temperature is 80°C-90°C.
[0054] The stirring speed of the premix is 12 rpm-20 rpm.
[0055] The slow dropping speed of the noise-reducing modifier is 0.5 parts / min.
[0056] The slow dropping speed of the ethyl orthosilicate is 0.5 parts / min.
[0057] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on building floors, the standing time is 15 minutes to 30 minutes.
[0058] The degassing treatment method is centrifugation, the centrifugal speed is 10000rpm-16000rpm, the centrifugal time is 20min-40min, and the centrifugal temperature is 4°C.
[0059] 3. Beneficial effects
[0060] The coating integrates four key properties: sound insulation, earthquake resistance, thermal insulation and waterproofing. It has a significant effect in meeting the diversified needs of building floors. This integrated design not only improves the application value of the material, but also simplifies the construction process and reduces the overall construction cost. The modified organic material technology is adopted. By selecting environmentally friendly raw materials such as polyester fiber, ammonium polyphosphate, lignin, etc., it not only ensures the performance of the coating, but also takes into account the biodegradability and environmental friendliness of the material. This is particularly important in the current context of emphasizing green buildings and sustainable development. By adding a special sound-absorbing modifier, the coating can effectively absorb and scatter sound waves, significantly improving the sound insulation effect of the building, which creates a quieter space for living and working environments and improves the comfort of living and working. Moderate; the pore structure formed by materials such as acrylic resin and ethyl orthosilicate effectively reduces heat conduction and has good thermal insulation performance, which helps to reduce energy consumption and achieve energy conservation and emission reduction; the coating also has good waterproof performance, can block moisture penetration, and keep the floor dry. At the same time, by adding flame retardants such as ammonium polyphosphate, the fire safety of the material is improved and the safety performance of the building is increased; the coating has excellent physical and chemical stability, good crack resistance and aging resistance, can maintain its performance for a long time, and extend the service life of building materials. Due to its outstanding comprehensive performance, the coating can not only be used in civil buildings such as residential buildings, schools, and hospitals, but also in public buildings, industrial buildings and other environments to meet the needs of different buildings for thermal insulation and sound insulation.
[0061] In summary, the thermal insulation and sound insulation coating and preparation method provided by the present invention have the characteristics of high performance, environmental protection, durability, etc., and bring a new efficient and environmentally friendly solution to the field of building materials technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 It is a flow principle diagram of sound waves inside the thermal insulation and sound insulation coating prepared by the present invention.
[0063] Figure 2 It is a scanning electron microscope image of the thermal insulation and sound insulation coating prepared by the present invention. DETAILED DESCRIPTION
[0064] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0065] It should be noted that, in the present invention, all weight parts involved are kilograms (Kg).
[0066] Example 1
[0067] The thermal insulation and sound insulation coating used on building floors comprises the following raw materials in parts by weight: 60 parts of acrylic resin.
[0068] Ethyl orthosilicate: 50 parts.
[0069] Noise-absorbing modifier: 10 parts.
[0070] Polyol: 20 parts.
[0071] Flame retardant: 5 parts.
[0072] Foam stabilizer: 6 parts.
[0073] Foaming agent: 0.8 parts.
[0074] Catalyst: 0.1 parts.
[0075] Surfactant: 0.5 parts.
[0076] The preparation method of the sound-absorbing modifier is as follows: polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of 10:5:10:50, heated to 75°C in an oil bath under nitrogen protection, stirred continuously for 8 hours, centrifuged at 8000 rpm for 10 minutes, the precipitate is taken, washed three times with anhydrous ethanol, and vacuum dried.
[0077] The thermal insulation and sound insulation coating used on the building floor slabs described above, the physical and chemical properties of the acrylic resin are as follows: density is 1.2g / cm³, refractive index is 1.50, and glass transition temperature is 107°C.
[0078] The physical and chemical properties of the ethyl orthosilicate are as follows: density is 0.93 g / cm³, and refractive index is 1.43.
[0079] In the above-mentioned thermal insulation and sound insulation coating used on building floors, the polyol is glycerol.
[0080] The flame retardant is hexabrominated diphenyl ether.
[0081] The foam stabilizer is Tween-20.
[0082] The catalyst is benzoyl peroxide.
[0083] The surfactant is alkylphenol polyoxyethylene ether.
[0084] The method for preparing the thermal insulation and sound insulation coating used on the building floor as described above comprises the following steps: premixing: adding acrylic resin, polyol, flame retardant, foam stabilizer and surfactant into a stirring kettle, stirring at a low speed to obtain a mixture.
[0085] Add the sound-absorbing modifier: slowly add the sound-absorbing modifier into the mixture and stir evenly.
[0086] Adding ethyl orthosilicate: slowly add ethyl orthosilicate into the mixture and stir evenly.
[0087] Adding foaming agent: adding the foaming agent into the mixture and stirring evenly.
[0088] Adding catalyst: Add the catalyst into the mixture and stir well.
[0089] Degassing: Let the mixture stand to degas, and store in a cool place.
[0090] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on building floors, the pre-mixing and stirring temperature is 80°C.
[0091] The stirring speed of the premix is 20 rpm.
[0092] The slow dropping speed of the noise-reducing modifier is 0.5 parts / min.
[0093] The slow dropping speed of the ethyl orthosilicate is 0.5 parts / min.
[0094] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on the building floor, the standing time is 15 minutes.
[0095] The degassing treatment method is centrifugation, the centrifugal speed is 10000rpm, the centrifugal time is 40min, and the centrifugal temperature is 4°C.
[0096] Example 2
[0097] The thermal insulation and sound insulation coating used on building floors comprises the following raw materials in parts by weight: 100 parts of acrylic resin.
[0098] Ethyl orthosilicate: 40 parts.
[0099] Noise-absorbing modifier: 18 parts.
[0100] Polyol: 15 parts.
[0101] Flame retardant: 10 parts.
[0102] Foam stabilizer: 2 parts.
[0103] Foaming agent: 2 parts.
[0104] Catalyst: 0.02 parts.
[0105] Surfactant: 2 parts.
[0106] The preparation method of the sound-absorbing modifier is as follows: polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of 20:10:5:60, heated to 85°C in an oil bath under nitrogen protection, stirred continuously for 4 hours, centrifuged at 8000 rpm for 10 minutes, the precipitate is taken, washed three times with anhydrous ethanol, and vacuum dried.
[0107] The thermal insulation and sound insulation coating used on the building floor slabs described above, the physical and chemical properties of the acrylic resin are as follows: density is 1.2g / cm³, refractive index is 1.50, and glass transition temperature is 107°C.
[0108] The physical and chemical properties of the ethyl orthosilicate are as follows: density is 0.93 g / cm³, and refractive index is 1.43.
[0109] In the above-mentioned thermal insulation and sound insulation coating used on building floors, the polyol is butanediol.
[0110] The flame retardant is magnesium hydroxide.
[0111] The foam stabilizer is Span-20.
[0112] The catalyst is diisopropyl peroxide.
[0113] The surfactant is allyl polyoxyalkyl ether.
[0114] The method for preparing the thermal insulation and sound insulation coating used on the building floor as described above comprises the following steps: premixing: adding acrylic resin, polyol, flame retardant, foam stabilizer and surfactant into a stirring kettle, stirring at a low speed to obtain a mixture.
[0115] Add the sound-absorbing modifier: slowly add the sound-absorbing modifier into the mixture and stir evenly.
[0116] Adding ethyl orthosilicate: slowly add ethyl orthosilicate into the mixture and stir evenly.
[0117] Adding foaming agent: adding the foaming agent into the mixture and stirring evenly.
[0118] Adding catalyst: Add the catalyst into the mixture and stir well.
[0119] Degassing: Let the mixture stand to degas, and store in a cool place.
[0120] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on building floors, the pre-mixing and stirring temperature is 90°C.
[0121] The stirring speed of the premix is 12 rpm.
[0122] The slow dropping speed of the noise-reducing modifier is 0.5 parts / min.
[0123] The slow dropping speed of the ethyl orthosilicate is 0.5 parts / min.
[0124] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on the building floor, the standing time is 30 minutes.
[0125] The degassing treatment method is centrifugation, the centrifugal speed is 16000 rpm, the centrifugal time is 20 minutes, and the centrifugal temperature is 4°C.
[0126] Example 3
[0127] The thermal insulation and sound insulation coating used on building floors comprises the following raw materials in parts by weight: 70 parts of acrylic resin.
[0128] Ethyl orthosilicate: 48 parts.
[0129] Noise-absorbing modifier: 12 parts.
[0130] Polyol: 20 parts.
[0131] Flame retardant: 5 parts.
[0132] Foam stabilizer: 6 parts.
[0133] Foaming agent: 0.8 parts.
[0134] Catalyst: 0.1 parts.
[0135] Surfactant: 0.5 parts.
[0136] The preparation method of the sound-absorbing modifier is as follows: polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of 15:10:8:50, heated to 80°C in an oil bath under nitrogen protection, stirred continuously for 4 hours, centrifuged at 8000 rpm for 10 minutes, the precipitate is taken, washed three times with anhydrous ethanol, and vacuum dried.
[0137] The thermal insulation and sound insulation coating used on the building floor slabs described above, the physical and chemical properties of the acrylic resin are as follows: density is 1.2g / cm³, refractive index is 1.50, and glass transition temperature is 107°C.
[0138] The physical and chemical properties of the ethyl orthosilicate are as follows: density is 0.93 g / cm³, and refractive index is 1.43.
[0139] In the above-mentioned thermal insulation and sound insulation coating used on building floors, the polyol is trihydroxyethanol (C3H8O3).
[0140] The flame retardant is expanded graphite.
[0141] The foam stabilizer is Tween-80.
[0142] The catalyst is diethanolamine.
[0143] The surfactant is tetraalkylammonium chloride.
[0144] The method for preparing the thermal insulation and sound insulation coating used on the building floor as described above comprises the following steps: premixing: adding acrylic resin, polyol, flame retardant, foam stabilizer and surfactant into a stirring kettle, stirring at a low speed to obtain a mixture.
[0145] Add the sound-absorbing modifier: slowly add the sound-absorbing modifier into the mixture and stir evenly.
[0146] Adding ethyl orthosilicate: slowly add ethyl orthosilicate into the mixture and stir evenly.
[0147] Adding foaming agent: adding the foaming agent into the mixture and stirring evenly.
[0148] Adding catalyst: Add the catalyst into the mixture and stir well.
[0149] Degassing: Let the mixture stand to degas, and store in a cool place.
[0150] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on building floors, the pre-mixing and stirring temperature is 80°C.
[0151] The stirring speed of the premix is 12 rpm.
[0152] The slow dropping speed of the noise-reducing modifier is 0.5 parts / min.
[0153] The slow dropping speed of the ethyl orthosilicate is 0.5 parts / min.
[0154] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on the building floor, the standing time is 15 minutes.
[0155] The degassing treatment method is centrifugation, the centrifugal speed is 10000rpm, the centrifugal time is 20min, and the centrifugal temperature is 4℃.
[0156] Example 4
[0157] The thermal insulation and sound insulation coating used on building floors comprises the following raw materials in parts by weight: 90 parts of acrylic resin.
[0158] Ethyl orthosilicate: 42 parts.
[0159] Noise-absorbing modifier: 16 parts.
[0160] Polyol: 15 parts.
[0161] Flame retardant: 10 parts.
[0162] Foam stabilizer: 2 parts.
[0163] Foaming agent: 2 parts.
[0164] Catalyst: 0.02 parts.
[0165] Surfactant: 2 parts.
[0166] The preparation method of the sound-absorbing modifier is as follows: polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of 20:5:10:60, heated to 85°C in an oil bath under nitrogen protection, stirred continuously for 8 hours, centrifuged at 8000 rpm for 10 minutes, the precipitate is taken, washed three times with anhydrous ethanol, and vacuum dried.
[0167] The thermal insulation and sound insulation coating used on the building floor slabs described above, the physical and chemical properties of the acrylic resin are as follows: density is 1.2g / cm³, refractive index is 1.50, and glass transition temperature is 107°C.
[0168] The physical and chemical properties of the ethyl orthosilicate are as follows: density is 0.93 g / cm³, and refractive index is 1.43.
[0169] In the above-mentioned thermal insulation and sound insulation coating used on building floors, the polyol is butanediol.
[0170] The flame retardant is nano aluminum oxide.
[0171] The foam stabilizer is Tween-20.
[0172] The catalyst is benzoyl peroxide.
[0173] The surfactant is allyl polyoxyalkyl ether.
[0174] The method for preparing the thermal insulation and sound insulation coating used on the building floor as described above comprises the following steps: premixing: adding acrylic resin, polyol, flame retardant, foam stabilizer and surfactant into a stirring kettle, stirring at a low speed to obtain a mixture.
[0175] Add the sound-absorbing modifier: slowly add the sound-absorbing modifier into the mixture and stir evenly.
[0176] Adding ethyl orthosilicate: slowly add ethyl orthosilicate into the mixture and stir evenly.
[0177] Adding foaming agent: adding the foaming agent into the mixture and stirring evenly.
[0178] Adding catalyst: Add the catalyst into the mixture and stir well.
[0179] Degassing: Let the mixture stand to degas, and store in a cool place.
[0180] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on building floors, the pre-mixing and stirring temperature is 90°C.
[0181] The stirring speed of the premix is 20 rpm.
[0182] The slow dropping speed of the noise-reducing modifier is 0.5 parts / min.
[0183] The slow dropping speed of the ethyl orthosilicate is 0.5 parts / min.
[0184] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on the building floor, the standing time is 30 minutes.
[0185] The degassing treatment method is centrifugation, the centrifugal speed is 16000 rpm, the centrifugal time is 40 minutes, and the centrifugal temperature is 4°C.
[0186] Example 5
[0187] The thermal insulation and sound insulation coating used on building floors comprises the following raw materials in parts by weight: 80 parts of acrylic resin.
[0188] Ethyl orthosilicate: 45 parts.
[0189] Noise-absorbing modifier: 14 parts.
[0190] Polyol: 18 parts.
[0191] Flame retardant: 8 parts.
[0192] Foam stabilizer: 4 parts.
[0193] Foaming agent: 1.4 parts.
[0194] Catalyst: 0.07 parts.
[0195] Surfactant: 1.5 parts.
[0196] The preparation method of the sound-absorbing modifier is as follows: polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of 18:8:9:55, heated to 83°C in an oil bath under nitrogen protection, stirred continuously for 6 hours, centrifuged at 8000 rpm for 10 minutes, the precipitate is taken, washed three times with anhydrous ethanol, and vacuum dried.
[0197] The thermal insulation and sound insulation coating used on the building floor slabs described above, the physical and chemical properties of the acrylic resin are as follows: density is 1.2g / cm³, refractive index is 1.50, and glass transition temperature is 107°C.
[0198] The physical and chemical properties of the ethyl orthosilicate are as follows: density is 0.93 g / cm³, and refractive index is 1.43.
[0199] In the above-mentioned thermal insulation and sound insulation coating used on building floors, the polyol is glycerol.
[0200] The flame retardant is hexabrominated diphenyl ether.
[0201] The foam stabilizer is Tween-80.
[0202] The catalyst is diisopropyl peroxide (CAS No.: 54693-46-8).
[0203] The surfactant is tetraalkylammonium chloride (CAS No.: 75-57-0).
[0204] The method for preparing the thermal insulation and sound insulation coating used on the building floor as described above comprises the following steps: premixing: adding acrylic resin, polyol, flame retardant, foam stabilizer and surfactant into a stirring kettle, stirring at a low speed to obtain a mixture.
[0205] Add the sound-absorbing modifier: slowly add the sound-absorbing modifier into the mixture and stir evenly.
[0206] Adding ethyl orthosilicate: slowly add ethyl orthosilicate into the mixture and stir evenly.
[0207] Adding foaming agent: adding the foaming agent into the mixture and stirring evenly.
[0208] Adding catalyst: Add the catalyst into the mixture and stir well.
[0209] Degassing: Let the mixture stand to degas, and store in a cool place.
[0210] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on building floors, the pre-mixing and stirring temperature is 85°C.
[0211] The stirring speed of the premix is 15 rpm.
[0212] The slow dropping speed of the noise-reducing modifier is 0.5 parts / min.
[0213] The slow dropping speed of the ethyl orthosilicate is 0.5 parts / min.
[0214] In the above-mentioned method for preparing the thermal insulation and sound insulation coating used on the building floor, the standing time is 20 minutes.
[0215] The degassing treatment method is centrifugation, the centrifugal speed is 14000 rpm, the centrifugal time is 30 minutes, and the centrifugal temperature is 4°C.
[0216] Comparative Example 1
[0217] The thermal insulation and sound insulation coating used on the building floor is different from that in Example 5 in that ethyl orthosilicate is removed.
[0218] Comparative Example 2
[0219] The thermal insulation and sound insulation coating used on the building floor is different from that in Example 5 in that the ammonium polyphosphate in the sound-absorbing modifier is removed.
[0220] Comparative Example 3
[0221] The thermal insulation and sound insulation coating used on the building floor is different from that in Example 5 in that the lignin in the sound-absorbing modifier is removed.
[0222] Comparative Example 4
[0223] The thermal insulation and sound insulation coating used on the building floor is different from that in Example 5 in that the sound-absorbing modifier is removed.
[0224] Test Case
[0225] The coating prepared in Example 5 was selected, which added a core component, namely a sound-absorbing modifier, from the schematic diagram of the simulation ( Figure 1 ) It can be seen that the black line on the chain in the figure is the direction of heat propagation, and it can be seen that the heat is trapped inside the paint. The gray line across the chain in the figure is the direction of sound wave propagation. It can be seen that the sound wave is absorbed and dissipated after multiple reflections inside the paint. Figure 2 As shown, the coating shows a typical loose and porous aerogel microstructure, which plays a good role in improving the two functions of thermal insulation and sound insulation. In addition, the contact angle is as high as 142°, showing excellent waterproof performance. The measured tanδ value of the thermal insulation and sound insulation coating is 0.23, and the elasticity is relatively high. This is due to the relatively soft structure, which meets the standard of "Elastic Architectural Coatings" (JG / T 172-2005) and meets the requirements of seismic performance.
[0226] The thermal insulation and sound insulation coatings (thickness of 2 mm) prepared in Examples 1-5 and Comparative Examples 1-4 were tested for thermal conductivity using a DRM-1 thermal conductivity tester in accordance with the provisions of GB / T 10294. The sound insulation performance was tested with reference to "Ren Qinghai, Ma Yangmin, Zhang Tianfu. Study on Eucommia Gum / Chloroprene Rubber Blends and Their Sound Insulation Performance [J]. Journal of Shaanxi University of Science and Technology (Natural Science Edition), 2011, 29(01): 35-37." The initial sound intensity was 120 dB, and the sound intensity after sound insulation was observed.
[0227] Table 1 Test results
[0228] Thermal conductivity W / m∙K Sound intensity dB Example 1 0.035 32 Example 2 0.034 32 Example 3 0.034 31 Example 4 0.032 30 Example 5 0.032 29 Comparative Example 1 0.173 67 Comparative Example 2 0.037 76 Comparative Example 3 0.035 79 Comparative Example 4 0.041 85
[0229] As shown in Table 1, in general, the thermal insulation and sound insulation coating prepared by the embodiment of the present invention is better than the thermal insulation and sound insulation material prepared by the comparative example, and has better thermal insulation and sound insulation performance. After analysis as follows, comparative example 1 removes ethyl orthosilicate, which plays an important role in the coating. It can generate a pore structure during the curing process. This pore structure is very effective in reducing heat conduction; removing ethyl orthosilicate will lead to a reduction in this pore structure, thereby reducing the thermal insulation performance of the coating; ethyl orthosilicate not only affects the thermal insulation performance through the pore structure formed, but also affects the propagation of sound waves; the pore structure can increase the absorption and scattering of sound waves inside the material, thereby improving the sound insulation performance of the material; therefore, removing ethyl orthosilicate will reduce the sound insulation effect; ethyl orthosilicate will form pores after participating in the reaction, and these pores reduce the overall density of the coating; removing ethyl orthosilicate will increase the density of the coating, which is not conducive to reducing the weight of the building and reducing the amount of materials used; ethyl orthosilicate can improve the waterproof performance of the coating. In the pore structure formed by it, the presence of micropores can prevent water molecules from penetrating and improve the waterproofness of the coating; after removing ethyl orthosilicate, the waterproofness of the coating will decrease; the pore structure not only helps to keep warm and soundproof, but also makes the coating have a certain flexibility and can withstand a certain degree of deformation without breaking; therefore, removing ethyl orthosilicate will affect the durability and stability of the coating; on the whole, ethyl orthosilicate plays an important role in the performance of thermal insulation and sound insulation coatings, and its removal will cause the coating to have varying degrees of reduction in multiple performance aspects such as thermal insulation and sound insulation.
[0230] Comparative Example 2 removes ammonium polyphosphate from the sound-absorbing modifier. Ammonium polyphosphate is often used as a flame retardant in thermal insulation and sound insulation materials, and also contributes to the structure and performance of the material. The effect of removing ammonium polyphosphate from the sound-absorbing modifier on the thermal insulation and sound insulation performance can be analyzed from the following aspects: Ammonium polyphosphate is an effective inorganic flame retardant that can improve the stability and safety of the material in the event of fire. Removing ammonium polyphosphate reduces the flame retardant properties of the thermal insulation and sound insulation coating, making it more flammable under high temperature or fire conditions, and cannot effectively prevent the spread of the fire. Although the main function of ammonium polyphosphate is as a flame retardant, in the thermal insulation and sound insulation coating, the combined effect of all components jointly determines the overall performance of the material. Ammonium polyphosphate changes the pore structure or density of the coating at the microscopic level, and these slight changes in the structure will affect the propagation and absorption of sound waves. Therefore, removing ammonium polyphosphate will have a certain effect on the sound insulation performance of the coating, and the specific effect depends on the adjustment of other components and the overall formula. The removal of ammonium polyphosphate will cause changes in the internal structure of the material, affecting its thermal insulation effect. Generally speaking, the thermal insulation performance of a material is closely related to the porosity and distribution of its internal structure. However, ammonium polyphosphate has little direct effect on thermal insulation performance, and the impact after removal is not as significant as its effect on flame retardancy. When ammonium polyphosphate is added to thermal insulation and sound insulation coatings, it will increase the stiffness and stability of the material, thereby affecting the mechanical properties of the material. Removing ammonium polyphosphate will make the coating more susceptible to deformation under external forces, thereby affecting its service life and protective effect. In general, removing ammonium polyphosphate from the sound-absorbing modifier mainly affects the flame retardancy of the material, and has a certain impact on the sound insulation, thermal insulation and mechanical properties of the material, but the specific degree of impact depends on the overall formula and structural design of the material. In practical applications, the performance of the final product can be compensated or optimized by adjusting the proportion of other ingredients or adding alternative materials.
[0231] Comparative Example 3 removes lignin from the sound-absorbing modifier. Lignin plays an important role in the formula of the sound-absorbing modifier in the thermal insulation and sound insulation coating. It is a natural polymer compound with good physical and chemical stability. In the thermal insulation and sound insulation coating, lignin can provide the following benefits: Due to its unique porous structure, lignin can effectively absorb and scatter sound waves, helping to improve the sound insulation performance of the material. Removing lignin from the sound-absorbing modifier will reduce the overall sound absorption capacity of the coating, which will have an adverse effect on the sound insulation effect. Lignin also uses its porous structure in the coating to reduce heat conduction and contribute to improving the thermal insulation performance. Although the direct effect of lignin on thermal insulation performance is not as great as its effect on sound insulation performance, its presence in the coating is still of certain significance for improving the overall performance. Lignin can improve the structural strength and durability of the material. Adding lignin to the coating can improve the adhesion of the material, improve its crack resistance and aging resistance, and increase the stability and service life of the coating. Removing lignin makes the coating more fragile and its ability to resist external stress and environmental aging decreases. As a naturally derived polymer, lignin has good environmental friendliness and helps to improve the green and environmentally friendly characteristics of thermal insulation and sound insulation coatings. Eliminating lignin will affect the sustainability and biodegradability of the coating. As a relatively low-cost raw material, the use of lignin in coating formulations helps to control production costs. Removing lignin requires finding other alternative materials with similar functions, which will increase the cost of the formulation. In general, removing lignin from the sound-absorbing modifier will have a negative impact on the sound insulation effect, thermal insulation performance, mechanical stability, environmental friendliness and cost-effectiveness of the thermal insulation and sound insulation coating. In order to maintain or optimize the performance of the formulation after removing lignin, it is necessary to compensate by adjusting the proportion of other ingredients or introducing new functional materials.
[0232] Comparative Example 4 removes the muffler modifier, which plays a key role in thermal insulation and sound insulation coatings, especially in terms of sound control and sound insulation. The effects of removing the muffler modifier on thermal insulation and sound insulation coatings mainly include: muffler modifiers are specially designed to absorb, scatter or block sound waves to reduce the propagation of sound. Removing this modifier will directly weaken the sound insulation ability of the coating. This means that the building floor coated with this coating cannot effectively reduce external noise or the transmission of sound between rooms, affecting the acoustic environment inside the building. Although the muffler modifier is mainly aimed at acoustic performance, the structural characteristics of some muffler materials (such as porosity) also contribute to improving thermal insulation performance. Therefore, removing the muffler modifier indirectly affects the thermal insulation performance of the coating, especially if this modifier plays an important role in the formation of the internal structure of the material. Muffler modifiers contribute to the physical and chemical properties of the coating, including adhesion, elasticity, weather resistance, etc. Removing them leads to changes in the properties of the coating, such as reducing adhesion to the substrate, reducing durability, or changing the flexibility of the coating. With the sound-deadening modifier, thermal insulation and sound insulation coatings can be widely used in applications that require high sound insulation performance, such as residences, schools, hospitals, etc. After removal, the application scope of the coating will be limited and cannot meet the needs of specific acoustic environments. Removing the sound-deadening modifier requires redesigning the formula to achieve similar performance, which involves finding new alternative materials or increasing the proportion of other ingredients, which will increase manufacturing costs or affect the cost-effectiveness of the final product. In short, removing the sound-deadening modifier will directly affect the core functions of thermal insulation and sound insulation coatings, especially in terms of sound insulation capabilities. This change needs to be overcome through optimization and adjustment in the formulation to ensure that the coating can still meet the market requirements for high-performance architectural coatings.
[0233] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A thermal insulation and sound insulation coating used on building floors. Features: In parts by weight, the following raw materials are included: Acrylic resin: 60-100 parts; Ethyl orthosilicate: 40-50 parts; Noise-reducing agent: 10-18 parts; Polyol: 15-20 parts; Flame retardant: 5-10 parts; Foam stabilizer: 2-6 parts; Foaming agent: 0.8-2 parts; Catalyst: 0.02-0.1 parts; Surfactant: 0.5-2 parts; The preparation method of the sound-absorbing modifier is as follows: Polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of (10-20): (5-10): (5-10): (50-60), heated to 75°C-85°C in an oil bath under nitrogen protection, stirred continuously for 4h-8h, centrifuged at 8000rpm for 10min, the precipitate is collected, washed three times with anhydrous ethanol, and dried in a vacuum.
2. The thermal insulation and sound insulation coating used on building floors according to claim 1, Features: In parts by weight, the following raw materials are included: Acrylic resin: 70-90 parts; Ethyl orthosilicate: 42 parts to 48 parts; Noise-reducing agent: 12-16 parts; Polyol: 15-20 parts; Flame retardant: 5-10 parts; Foam stabilizer: 2-6 parts; Foaming agent: 0.8-2 parts; Catalyst: 0.02-0.1 parts; Surfactant: 0.5-2 parts; The preparation method of the sound-absorbing modifier is as follows: Polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of (15-20): (5-10): (8-10): (50-60), heated to 80°C-85°C in an oil bath under nitrogen protection, stirred continuously for 4h-8h, centrifuged at 8000rpm for 10min, the precipitate is collected, washed three times with anhydrous ethanol, and dried in a vacuum.
3. The thermal insulation and sound insulation coating used on building floors according to claim 2, Features: In parts by weight, the following raw materials are included: Acrylic resin: 80 parts; Ethyl orthosilicate: 45 parts; Noise-reducing agent: 14 parts; Polyol: 18 parts; Flame retardant: 8 parts; Foam stabilizer: 4 parts; Foaming agent: 1.4 parts; Catalyst: 0.07 parts; Surfactant: 1.5 parts; The preparation method of the sound-absorbing modifier is as follows: Polyester fiber, ammonium polyphosphate, lignin and tetrahydrofuran are mixed in a mass ratio of 18:8:9:55, heated to 83°C in an oil bath under nitrogen protection, stirred continuously for 6 hours, centrifuged at 8000 rpm for 10 minutes, the precipitate is taken, washed three times with anhydrous ethanol, and vacuum dried.
4. The thermal insulation and sound insulation coating used on building floors according to claim 3, Features: The physicochemical properties of the acrylic resin are as follows: The density is 1.2g / cm³, the refractive index is 1.50, and the glass transition temperature is 107℃; The physicochemical properties of the ethyl orthosilicate are as follows: The density is 0.93g / cm³ and the refractive index is 1.
43.
5. The thermal insulation and sound insulation coating used on building floors according to claim 3, Features: The polyol is one of ethylene glycol, propylene glycol, butylene glycol, trihydroxyethanol, glycerol, tetraethylene glycol, and pentaethylene glycol; The flame retardant is one of hexabromodiphenyl ether, magnesium hydroxide, expanded graphite, and nano-alumina; The foam stabilizer is one of Tween-20, Tween-80, Span-20 and Span-80; The catalyst is one of hydrogen peroxide, benzoyl peroxide, diisopropyl peroxide, triethylamine, diethanolamine and pyridine; The surfactant is one of alkylphenol polyoxyethylene ether, allyl polyoxyalkyl ether and tetraalkylammonium chloride.
6. A method for preparing the thermal insulation and sound insulation coating used on building floors as claimed in claim 1, Features: The following steps are involved: Premixing: Add acrylic resin, polyol, flame retardant, foam stabilizer and surfactant into a stirring kettle, stir evenly at a low speed to obtain a mixture; Adding the sound-absorbing modifier: slowly adding the sound-absorbing modifier into the mixture and stirring evenly; Adding ethyl orthosilicate: slowly adding ethyl orthosilicate into the mixture and stirring evenly; Adding a foaming agent: adding the foaming agent into the mixture and stirring evenly; Adding catalyst: adding the catalyst into the mixture and stirring evenly; Degassing: Let the mixture stand to degas, and store in a cool place.
7. The method for preparing the thermal insulation and sound insulation coating for use on building floors according to claim 6, Features: The premixing stirring temperature is 80°C-90°C; The stirring speed of the premix is 12 rpm-20 rpm; The slow dropping speed of the noise-reducing modifier is 0.5 parts / min; The slow dropping speed of the ethyl orthosilicate is 0.5 parts / min.
8. The method for preparing the thermal insulation and sound insulation coating for use on building floors according to claim 7, Features: The standing time is 15min-30min; The degassing treatment method is centrifugation, the centrifugal speed is 10000rpm-16000rpm, the centrifugal time is 20min-40min, and the centrifugal temperature is 4°C.