A method for preparing a back contact cell, a back contact cell and a photovoltaic module
By retaining the phosphorus silicon glass layer doped with nitrogen and/or carbon in the preparation of back contact battery and etching the opening after the front coating, the semiconductor layer is protected by using the mask layer, the passivation film layer in the preparation of back contact battery is solved. The problems of damage and poor cleanliness improve the passivation performance and open circuit voltage of the battery.
Patent Information
- Application Number
- CN202411140271.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-20
AI Technical Summary
In the existing back contact battery preparation process, the passivation film and suede on the back of the silicon wafer are susceptible to scratch damage and high temperature, resulting in a decrease in the open circuit voltage, and the cleanliness of the film layer during cleaning and removal winding and plating are poor, which affects the bluntness. .
The mask layer (first phosphorus silicon glass layer doped with nitrogen and/or carbon) is left after fleece making for front coating, and the first semiconductor layer is protected by a complete mask layer during the etching opening to prevent scraping Rub and high temperature damage, while removing the damaged layer by low concentration of alkali liquid during cleaning and removal of winding and plating, ensuring the integrity of the film layer.
It improves the passivation performance and open circuit voltage of the battery, enhances the cleanliness and corrosion resistance of the film layer, and ensures high-quality preparation of the back contact battery.
Smart Images

Figure CN118658933B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of back-contact batteries, and in particular relates to a method for preparing a back-contact battery, a back-contact battery and a photovoltaic module. Background Art
[0002] At present, the preparation process of double-sided multi-crystalline back-contact solar cells is generally to make a texture after the laser opening of the passivation film on the back of the silicon wafer, remove the damaged layer in the laser opening area and form a texture surface by texture making, and remove the mask layer, and then use the tubular PECVD (plasma enhanced chemical vapor deposition) method to coat the front side of the silicon wafer. However, in this way, first, the front side coating needs to use a graphite boat for automatic insertion. During this process, the passivation film and the velvet surface on the back of the silicon wafer will be damaged by scratching with the graphite boat, and the temperature of the front side coating process is high, which has a certain impact on the performance of the passivation film layer, resulting in a decrease in the open circuit voltage; second, the film layer formed by the tubular PECVD method has a more serious wrap-around phenomenon, which needs to be cleaned and removed, but the cleaning solution will seriously damage the passivation film layer; third, the interface in the laser opening area will be contaminated during the front side coating process (such as the dirt of the graphite boat is adsorbed on the surface of the silicon wafer, and then the impurity ions are introduced into the silicon wafer by high temperature), which cannot be completely removed by backwashing alone, the cleanliness is poor, and the passivation quality of the film layer is low.
[0003] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art that the back contact battery is easily damaged by scratches and affected by high temperature during the preparation process, which weakens the passivation performance of the battery and leads to a decrease in the open circuit voltage. A preparation method of a back contact battery, a back contact battery and a photovoltaic module are provided. The preparation method of the back contact battery can retain the mask layer after the texturing and then perform front-side coating, and then perform etching openings. First, during the front-side coating process, the first semiconductor layer is protected by the complete mask layer to prevent the first semiconductor layer from being damaged by scratches or affected by high temperature, thereby improving the passivation performance and open circuit voltage of the battery. Second, during the cleaning and removal of the wrap-around plating process, The first semiconductor layer is protected by a complete mask layer to prevent the first semiconductor layer from being corroded by the cleaning solution, thereby further improving the passivation performance and open circuit voltage of the battery. Thirdly, the second semiconductor layer is directly plated after etching and backwashing, and no high-temperature treatment is required. The interface cleanliness in the first opening area is high, and the passivation quality of the film layer is high. Fourthly, a first phosphorus silicon glass layer doped with nitrogen and / or carbon is used as a mask layer, which has a high degree of density and strong corrosion resistance, and can improve the protection effect on the first semiconductor layer. Fifthly, the thickness of the back mask layer will be increased during the front annealing process, thereby further improving the protection effect on the first semiconductor layer.
[0005] In order to achieve the above object, in a first aspect, the present invention provides a method for preparing a back contact battery, comprising the following steps:
[0006] S1. Provide double-sided polished silicon wafers;
[0007] S2. depositing a first semiconductor layer on the back side of the silicon wafer, the first semiconductor layer comprising a first tunneling oxide layer, an intrinsic polysilicon layer, a first doping layer, and a second doping layer arranged in sequence, and then annealing the first semiconductor layer to convert the second doping layer into a mask layer, wherein the second doping layer is doped with nitrogen and / or carbon, and the mask layer is a first phosphorus silicon glass layer doped with nitrogen and / or carbon;
[0008] S3 cleaning and removing the oxide layer on the front side of the silicon wafer caused by annealing in S2;
[0009] S4. A velvet surface is formed on the front side of the silicon wafer by velvet cleaning;
[0010] S5. Deposition and annealing are performed on the front side of the silicon wafer to form a passivation layer, the passivation layer comprising a second tunneling oxide layer and a third doping layer disposed in sequence;
[0011] S6. Cleaning and removing the second phosphosilicate glass layer produced by the deposition of S5 on the passivation layer, and then forming an anti-reflection layer on the passivation layer;
[0012] S7 is etching an opening on the first semiconductor layer, the mask layer and the coating layer generated by the deposition of S6 to form a first opening region;
[0013] S8. removing the damaged layer on the silicon wafer in the first opening area caused by etching in S7, and removing the plating layer at the same time, wherein the damaged layer and the plating layer are removed by texturing cleaning or polishing cleaning, and the texturing solution used in the texturing cleaning and the polishing solution used in the polishing cleaning contain potassium hydroxide or sodium hydroxide, and the mass percentage of potassium hydroxide or sodium hydroxide is less than 3%;
[0014] S9. Cleaning and removing the mask layer, and then backwashing with RCA solution;
[0015] S10. Depositing a second semiconductor layer on the back side of the silicon wafer so that a portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion of the second semiconductor layer extends into the first opening area and covers the silicon wafer, the second semiconductor layer comprising an intrinsic amorphous silicon layer and a fourth doped layer arranged in sequence.
[0016] Preferably, S2 includes:
[0017] The laughing gas is introduced and reacted to form a first tunneling oxide layer under the condition of turning on the glow, wherein the thickness of the first tunneling oxide layer is 1 nm to 2 nm;
[0018] Silane and hydrogen are introduced and reacted under the condition of turning on the glow to form an intrinsic polysilicon layer, the thickness of the intrinsic polysilicon layer is 10nm-30nm;
[0019] Silane, phosphine and hydrogen are introduced and reacted to form a first doping layer under the condition of turning on the glow, and the thickness of the first doping layer is 30nm-100nm;
[0020] Introduce silane, phosphine, hydrogen, nitrogen and / or methane, and react to form a second doping layer under the condition of turning on the glow, wherein the thickness of the second doping layer is 10nm-30nm;
[0021] Oxygen is introduced and the first semiconductor layer is subjected to high temperature annealing to convert the second doping layer into a mask layer. The thickness of the mask layer is 30nm-50nm.
[0022] Preferably, in S4, the reaction conditions for forming the first tunneling oxide layer are: the laughing gas flow rate is 8000sccm-12000sccm, the reaction time is 20s-100s, the reaction pressure is 100Pa-200Pa, and the reaction power is 3000W-10000W;
[0023] And / or, the reaction conditions for forming the intrinsic polysilicon layer are: silane flow rate is 1000sccm-3000sccm, hydrogen flow rate is 7000sccm-9000sccm, reaction time is 200s-400s, reaction pressure is 300Pa-500Pa, reaction power is 2000W-4000W;
[0024] And / or, the reaction conditions for forming the first doping layer are: silane flow rate is 1000sccm-3000sccm, phosphine flow rate is 1000sccm-2000sccm, hydrogen flow rate is 7000sccm-9000sccm, reaction time is 200s-800s, reaction pressure is 300Pa-500Pa, reaction power is 3000W-5000W;
[0025] And / or, the reaction conditions for forming the second doping layer are: silane flow rate is 1000sccm-3000sccm, phosphine flow rate is 2000sccm-3000sccm, hydrogen flow rate is 7000sccm-9000sccm, nitrogen flow rate is 1000sccm-3000sccm, methane flow rate is 500sccm-1000sccm, reaction time is 100s-300s, reaction pressure is 300Pa-500Pa, reaction power is 3000W-5000W;
[0026] And / or, the oxygen annealing conditions are: annealing pressure of 5000Pa-50000Pa, annealing temperature of 850°C-950°C, annealing time of 60min-120min, and oxygen flow rate of 2000sccm-8000sccm.
[0027] Preferably, in S3, a chain cleaning machine is used to clean and remove the oxide layer, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the hydrofluoric acid concentration is 10%-15%, the reaction temperature is 20°C-35°C, and the transmission roller speed of the chain cleaning machine is 1.2 m / min-3.0 m / min.
[0028] Preferably, in S4, the texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 2%-5%, the mass percentage of the texturing additive is 0.5%-1%, the texturing time is 8min-12min, the texturing temperature is 75℃-85℃, the corrosion depth of the front side of the silicon wafer is 3μm-4μm, and the texturing additive contains at least one of benzoic acid, aminotri(methylenephosphoric acid), polyepoxysuccinic acid and polyaspartic acid.
[0029] Preferably, in S5, a second tunneling oxide layer and a third doping layer are sequentially deposited on the silicon wafer by plasma enhanced chemical vapor deposition, and oxygen annealing is performed on them, wherein the thickness of the second tunneling oxide layer is 1nm-2nm, and the thickness of the third doping layer is 1nm-15nm.
[0030] Preferably, in S5, the oxygen annealing conditions are: annealing pressure is 5000Pa-50000Pa, annealing temperature is 850°C-900°C, annealing time is 60min-120min, and oxygen flow rate is 2000sccm-8000sccm.
[0031] Preferably, in S6, the second phosphosilicate glass layer is cleaned and removed by a chain cleaning machine, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the concentration of hydrofluoric acid is 5%-10%, the reaction temperature is 20° C.-35° C., and the transmission roller speed of the chain cleaning machine is 1.2 m / min-3.0 m / min;
[0032] And / or, an anti-reflection layer is formed on the passivation layer by plasma enhanced chemical vapor deposition, wherein the thickness of the anti-reflection layer is 70nm-120nm.
[0033] Preferably, in S8, the thickness of the damaged layer is less than or equal to 1 μm.
[0034] Preferably, in S8, if the damaged layer and the plating layer are removed by texturing cleaning, the texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1%-2%, the mass percentage of the texturing additive is 0.5%-1%, the texturing time is 4min-8min, the texturing temperature is 75°C-85°C, and the texturing additive contains at least one of benzoic acid, aminotrimethylphosphonic acid, polyepoxysuccinic acid and polyaspartic acid;
[0035] If the damaged layer and the coating layer are removed by polishing and cleaning, the polishing solution used is a mixed solution of potassium hydroxide or sodium hydroxide, a polishing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1.5%-3%, the mass percentage of the polishing additive is 1%-2%, the reaction temperature is 60℃-75℃, the reaction time is 120s-240s, and the polishing additive contains at least one of benzoic acid, aminotri(methylenephosphoric acid), polyepoxysuccinic acid and polyaspartic acid.
[0036] Preferably, in S9, a chain cleaning machine is used to clean and remove the mask layer on the back side of the silicon wafer to prevent the anti-reflection layer on the front side of the silicon wafer from being cleaned and removed, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the hydrofluoric acid concentration is 10%-15%, the reaction temperature is 20°C-35°C, and the transmission roller speed of the chain cleaning machine is 1.2 m / min-3.0 m / min.
[0037] Preferably, after S10, the method for preparing a back contact battery further comprises:
[0038] S11. Etching openings on the second semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart;
[0039] S12 forming a conductive film layer on the back side of the silicon wafer;
[0040] S13. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening region and covers the second semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;
[0041] S14. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.
[0042] In a second aspect, the present invention provides a back-contact battery, which is prepared by the above-mentioned method for preparing a back-contact battery.
[0043] In a third aspect, the present invention provides a photovoltaic module comprising the above-mentioned back contact cell.
[0044] Beneficial effects:
[0045] It has been found through research that in the preparation process of back-contact cells, if a laser opening is used and then the texture is made and the mask layer is removed, and then the front coating is performed, the passivation film layer and the velvet surface on the back of the silicon wafer will be exposed during the front coating, which is easily damaged by scratches and high temperatures, resulting in poor passivation effect and reduced open circuit voltage. The passivation film layer will also be corroded by the cleaning solution during cleaning and removal of the plating, affecting the passivation effect and open circuit voltage. The interface in the laser opening area will also be contaminated during the front coating process, which cannot be removed by backwashing alone, resulting in poor cleanliness and low passivation quality of the film layer. Based on this, further research has been conducted to propose the present invention.
[0046] The present invention adopts the above-mentioned technical scheme, especially retaining the mask layer (the first phosphorus silicon glass layer doped with nitrogen and / or carbon) after texturing and then performing front-side coating, and then etching the opening, and using the complete mask layer to protect the first semiconductor layer. First, it can prevent the first semiconductor layer from being scratched or affected by high temperature during the front-side coating process, thereby improving the passivation performance and open-circuit voltage of the battery. Second, it can prevent the first semiconductor layer from being corroded by the cleaning solution during the cleaning and removal of the wrap-around plating process, thereby further improving the passivation performance and open-circuit voltage of the battery. Third, it can make the second semiconductor layer directly plated after the etching and backwashing are completed without high-temperature treatment, thereby improving the interface cleanliness in the first opening area and improving the passivation quality of the film layer. Fourth, the first phosphorus silicon glass layer doped with nitrogen and / or carbon is used as the mask layer, which has a high degree of density and strong corrosion resistance, and can improve the protection effect on the first semiconductor layer. Fifth, the thickness of the back mask layer will be increased during the front-side annealing process, thereby further improving the protection effect on the first semiconductor layer.
[0047] Furthermore, in the prior art, by retaining a conventional mask layer (silicon nitride or silicon oxynitride) and then coating the front side, there is a problem that the corrosion resistance of the mask layer is enhanced after annealing, making it difficult to remove by corrosion. The present invention uses a first phosphorus silicon glass layer doped with nitrogen and / or carbon as a mask layer, which can effectively improve the density and corrosion resistance, and protect the first semiconductor layer from being completely corroded by the cleaning solution. Moreover, its corrosion resistance will not change significantly during the annealing process of the front film layer. Compared with silicon nitride or silicon oxynitride, the corrosion rate is faster and it is easier to remove.
[0048] At the same time, a low-concentration alkali solution is used to remove the damaged layer in the first opening area and the front winding plating layer, and the etching amount is controlled to be as low as possible, so as to prevent the secondary alkali solution corrosion from damaging the first semiconductor layer while ensuring the removal of the damaged layer in the first opening area and the front winding plating layer. The back contact battery prepared by the present invention has better passivation performance, higher open circuit voltage, higher film passivation quality, and better product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0050] Figure 1 This is a schematic diagram of the structure of a silicon wafer after double-sided polishing and cleaning according to an embodiment of the present invention;
[0051] Figure 2 This is a schematic diagram of the structure of forming a first semiconductor layer and a mask layer on the back side of a silicon wafer according to an embodiment of the present invention;
[0052] Figure 3 This is a schematic diagram of a structure in which a velvet surface is formed on the front side of a silicon wafer according to an embodiment of the present invention;
[0053] Figure 4 This is a schematic diagram of the structure of forming a passivation layer and an anti-reflection layer on the front side of a silicon wafer according to an embodiment of the present invention;
[0054] Figure 5 This is a schematic diagram of a structure in which a first opening area is formed on the back side of a silicon wafer according to an embodiment of the present invention;
[0055] Figure 6 This is a schematic diagram of the structure of removing the mask layer from the back of a silicon wafer according to an embodiment of the present invention;
[0056] Figure 7 This is a schematic diagram of a structure in which a second semiconductor layer is formed on the back side of a silicon wafer according to an embodiment of the present invention;
[0057] Figure 8 This is a schematic diagram of a structure in which a second opening area is formed on the back side of a silicon wafer according to an embodiment of the present invention;
[0058] Fig. 9 This is a schematic diagram of a structure in which a conductive film layer is formed on the back side of a silicon wafer according to an embodiment of the present invention;
[0059] Fig.10 This is a schematic diagram of a structure in which an isolation groove is formed on the back side of a silicon wafer according to an embodiment of the present invention;
[0060] Fig.11 It is a schematic diagram of the structure of forming a first electrode and a second electrode on the back side of a silicon wafer according to an embodiment of the present invention.
[0061] Description of Reference Numerals
[0062] 1-silicon wafer; 2-first tunneling oxide layer; 3-first doping layer; 4-mask layer; 5-second tunneling oxide layer; 6-third doping layer; 7-anti-reflection layer; 8-intrinsic amorphous silicon layer; 9-fourth doping layer; 10-conductive film layer; 11-first electrode; 12-second electrode; 13-intrinsic polysilicon layer. DETAILED DESCRIPTION
[0063] In the present invention, unless otherwise specified, directional words such as "up, down, left, right" are generally understood in combination with the directions shown in the drawings and actual applications.
[0064] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0065] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0066] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).
[0067] In the first aspect, the present invention provides a method for preparing a back-contact battery, which retains a mask layer after texturing and then performs front-side coating, and then performs etching to open the battery, and uses the mask layer to protect the first semiconductor layer. First, it can prevent the first semiconductor layer from being scratched or affected by high temperature during the front-side coating process, thereby improving the passivation performance and open-circuit voltage of the battery. Second, it can prevent the first semiconductor layer from being corroded by the cleaning solution during the cleaning and removal of the wrap-around plating process, thereby further improving the passivation performance and open-circuit voltage of the battery. Third, it can enable the second semiconductor layer to be directly plated after etching and backwashing, without the need for high-temperature treatment, thereby improving the interface cleanliness in the first opening area and improving the passivation quality of the film layer. Fourth, a first phosphorus silicon glass layer doped with nitrogen and / or carbon is used as a mask layer, which has a high degree of density and strong corrosion resistance, thereby improving the protection effect on the first semiconductor layer. Fifth, the thickness of the back mask layer will be increased during the front-side annealing process, thereby further improving the protection effect on the first semiconductor layer.
[0068] The method for preparing a back contact battery comprises the following steps:
[0069] S1. Provide double-sided polished silicon wafers;
[0070] S2. depositing a first semiconductor layer on the back side of the silicon wafer, the first semiconductor layer comprising a first tunneling oxide layer, an intrinsic polysilicon layer, a first doping layer, and a second doping layer arranged in sequence, and then annealing the first semiconductor layer to convert the second doping layer into a mask layer, wherein the second doping layer is doped with nitrogen and / or carbon, and the mask layer is a first phosphorus silicon glass layer doped with nitrogen and / or carbon;
[0071] S3 cleaning and removing the oxide layer on the front side of the silicon wafer caused by annealing in S2;
[0072] S4. A velvet surface is formed on the front side of the silicon wafer by velvet cleaning;
[0073] S5. Deposition and annealing are performed on the front side of the silicon wafer to form a passivation layer, the passivation layer comprising a second tunneling oxide layer and a third doping layer disposed in sequence;
[0074] S6. Cleaning and removing the second phosphosilicate glass layer produced by the deposition of S5 on the passivation layer, and then forming an anti-reflection layer on the passivation layer;
[0075] S7 is etching an opening on the first semiconductor layer, the mask layer and the coating layer generated by the deposition of S6 to form a first opening region;
[0076] S8. removing the damaged layer on the silicon wafer in the first opening area caused by etching in S7, and removing the plating layer at the same time, wherein the damaged layer and the plating layer are removed by texturing cleaning or polishing cleaning, and the texturing solution used in the texturing cleaning and the polishing solution used in the polishing cleaning contain potassium hydroxide or sodium hydroxide, and the mass percentage of potassium hydroxide or sodium hydroxide is less than 3%;
[0077] S9. Cleaning and removing the mask layer, and then backwashing with RCA solution;
[0078] S10. Depositing a second semiconductor layer on the back side of the silicon wafer so that a portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion of the second semiconductor layer extends into the first opening area and covers the silicon wafer, the second semiconductor layer comprising an intrinsic amorphous silicon layer and a fourth doped layer arranged in sequence.
[0079] It should be noted that, in S1, the silicon wafer is preferably an N-type single crystal silicon wafer, and the silicon wafer can be a Czochralski single crystal silicon wafer or a cast single crystal silicon wafer.
[0080] S2 consists of five stages:
[0081] The first stage: introduce laughing gas, and react to form a first tunneling oxide layer under the condition of turning on the glow, and the thickness of the first tunneling oxide layer is 1nm-2nm. Preferably, in the first stage, the reaction conditions for forming the first tunneling oxide layer are: laughing gas flow rate is 8000sccm-12000sccm, reaction time is 20s-100s, reaction pressure is 100Pa-200Pa, and reaction power is 3000W-10000W.
[0082] The second stage: silane and hydrogen are introduced, and reacted under the condition of turning on the glow to form an intrinsic polysilicon layer, and the thickness of the intrinsic polysilicon layer is 10nm-30nm. Preferably, in the second stage, the reaction conditions for forming the intrinsic polysilicon layer are: silane flow rate is 1000sccm-3000sccm, hydrogen flow rate is 7000sccm-9000sccm, reaction time is 200s-400s, reaction pressure is 300Pa-500Pa, and reaction power is 2000W-4000W.
[0083] The third stage: introducing silane, phosphine and hydrogen, and reacting to form a first doping layer under the condition of turning on the glow, the thickness of the first doping layer is 30nm-100nm. Preferably, in the third stage, the reaction conditions for forming the first doping layer are: silane flow rate is 1000sccm-3000sccm, phosphine flow rate is 1000sccm-2000sccm, hydrogen flow rate is 7000sccm-9000sccm, reaction time is 200s-800s, reaction pressure is 300Pa-500Pa, and reaction power is 3000W-5000W.
[0084] The fourth stage: introducing silane, phosphine, hydrogen, and nitrogen and / or methane, and reacting to form a second doping layer under the condition of turning on the glow, and the thickness of the second doping layer is 10nm-30nm. Preferably, in the fourth stage, the reaction conditions for forming the second doping layer are: silane flow rate is 1000sccm-3000sccm, phosphine flow rate is 2000sccm-3000sccm, hydrogen flow rate is 7000sccm-9000sccm, nitrogen flow rate is 1000sccm-3000sccm, methane flow rate is 500sccm-1000sccm, reaction time is 100s-300s, reaction pressure is 300Pa-500Pa, and reaction power is 3000W-5000W.
[0085] The fifth stage: oxygen is introduced and the first semiconductor layer is subjected to high temperature annealing to convert the second doped layer into a mask layer, and the thickness of the mask layer is 30nm-50nm. Among them, the mask layer is a first phosphorus silicon glass layer doped with nitrogen and / or carbon, so that the mask layer is denser and more corrosion-resistant than a conventional mask layer (silicon nitride or silicon oxynitride), thereby protecting the first semiconductor layer from being completely corroded by the cleaning solution. A reasonable thickness of the mask layer can protect the first semiconductor layer from multiple solution corrosions, which is beneficial to improving the passivation performance of the battery. Preferably, in the fifth stage, the oxygen annealing conditions are: annealing pressure of 5000Pa-50000Pa, annealing temperature of 850℃-950℃, annealing time of 60min-120min, and oxygen flow rate of 2000sccm-8000sccm.
[0086] In S3, a chain cleaning machine is used to clean and remove the oxide layer, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the concentration of hydrofluoric acid is 10%-15%, the reaction temperature is 20°C-35°C, and the transmission roller speed of the chain cleaning machine is 1.2 m / min-3.0 m / min.
[0087] In S4, the texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 2%-5%, the mass percentage of the texturing additive is 0.5%-1%, the texturing time is 8min-12min, the texturing temperature is 75℃-85℃, the corrosion depth of the front side of the silicon wafer is 3μm-4μm, and the texturing additive contains at least one of benzoic acid, aminotri(methylenephosphoric acid), polyepoxysuccinic acid and polyaspartic acid, that is, the texturing additive contains a certain film-forming protective agent.
[0088] Specifically, the etching depth is deep (3μm-4μm) to ensure that a velvet surface with low reflectivity is formed on the front side of the silicon wafer. In addition, since the velvet additive contains a certain film-forming protective agent, it can adhere to the mask layer to protect the mask layer from being corroded, thereby better protecting the first semiconductor layer.
[0089] In S5, a second tunneling oxide layer and a third doping layer are sequentially deposited on the silicon wafer by plasma enhanced chemical vapor deposition, and oxygen annealing is performed on them, wherein the thickness of the second tunneling oxide layer is 1nm-2nm, and the thickness of the third doping layer is 1nm-15nm. A front passivation layer formed by combining the second tunneling oxide layer and the third doping layer of reasonable thickness is more conducive to reducing the parasitic absorption of the front passivation film layer while ensuring the passivation effect.
[0090] Preferably, the oxygen annealing conditions are: annealing pressure of 5000Pa-50000Pa, annealing temperature of 850°C-900°C, annealing time of 60min-120min, and oxygen flow rate of 2000sccm-8000sccm.
[0091] Specifically, during the oxygen annealing process, the mask layer on the back of the silicon wafer will be further oxidized, and its thickness will increase by 5-20nm accordingly, so that the first semiconductor layer can be better protected from damage during subsequent alkaline solution corrosion. In this process, if the mask layer uses conventional silicon nitride or silicon oxynitride, its density is significantly enhanced after high-temperature annealing because its usual deposition temperature is 400℃-500℃, which makes it difficult to be corroded and removed later, affecting the preparation of the back contact battery. Therefore, the mask layer uses a first phosphorus silicon glass layer doped with nitrogen and / or carbon. After high-temperature annealing, its thickness will increase a little, but the density and corrosion resistance of the film layer will not change significantly, which is convenient for subsequent corrosion removal. Compared with conventional mask layers (silicon nitride or silicon oxynitride), the first phosphorus silicon glass layer doped with nitrogen and / or carbon has a faster corrosion rate in hydrofluoric acid, which can greatly shorten the subsequent cleaning and removal time.
[0092] In S6, a chain cleaning machine is used to clean and remove the second phosphorus silicon glass layer, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the concentration of hydrofluoric acid is 5%-10%, the reaction temperature is 20℃-35℃, and the transmission roller speed of the chain cleaning machine is 1.2m / min-3.0m / min. Thereafter, an anti-reflection layer is formed on the passivation layer by plasma enhanced chemical vapor deposition, wherein the thickness of the anti-reflection layer is 70nm-120nm. A reasonable thickness of the anti-reflection layer can reduce the surface reflection of the front side of the silicon wafer and protect the passivation film layer on the front side during the secondary cleaning, thereby improving the short-circuit current and efficiency of the battery.
[0093] In S7, laser or mask etching is used to etch openings on the first semiconductor layer, mask layer and winding coating on the back of the silicon wafer to form a first opening area, and the first semiconductor layer, mask layer and winding coating in the first opening area are etched away. The width of the first opening area W1 is 400 μm-800 μm. Laser etching is preferred, and the etching laser is an ultraviolet laser or a green laser with a power of 20 KW-100 KW and a frequency of 200 kHz-1000 kHz.
[0094] In S8, since the thickness of the damaged layer is less than or equal to 1 μm, the damaged layer can be completely removed by only ensuring that the single-side etching depth of the silicon wafer is greater than 1 μm.
[0095] Preferably, in S8, if the damaged layer and the coating layer are removed by texturing cleaning, the texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1%-2%, the mass percentage of the texturing additive is 0.5%-1%, the texturing time is 4min-8min, the texturing temperature is 75℃-85℃, and the texturing additive contains at least one of benzoic acid, aminotrimethylphosphonic acid, polyepoxysuccinic acid, and polyaspartic acid, that is, the texturing additive contains a certain film-forming protective agent, and a reasonable mass percentage of potassium hydroxide or sodium hydroxide can control the reaction rate within a lower range, which is conducive to controlling the corrosion depth and reducing the corrosiveness to the film layer. In addition, since the texturing additive contains a certain film-forming protective agent, it can adhere to the mask layer to protect the mask layer from corrosion, thereby better protecting the first semiconductor layer.
[0096] If the damaged layer and the coating layer are removed by polishing and cleaning, the polishing solution used is a mixed solution of potassium hydroxide or sodium hydroxide, a polishing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1.5%-3%, the mass percentage of the polishing additive is 1%-2%, the reaction temperature is 60°C-75°C, the reaction time is 120s-240s, and the polishing additive contains at least one of benzoic acid, aminotrimethylphosphonic acid, polyepoxysuccinic acid, and polyaspartic acid, that is, the polishing additive contains a certain film-forming protective agent, and a reasonable mass percentage of potassium hydroxide or sodium hydroxide can control the reaction rate within a lower range, which is conducive to controlling the corrosion depth and reducing the corrosiveness to the film layer. In addition, since the polishing additive contains a certain film-forming protective agent, it can adhere to the mask layer to protect the mask layer from corrosion, thereby better protecting the first semiconductor layer.
[0097] It is worth noting that compared with S4, S8 uses lower concentration alkaline solution (the mass percentage of potassium hydroxide or sodium hydroxide is less than 3%) for texturing cleaning or polishing cleaning, and controls the corrosion depth to be as small as possible to ensure that while removing the damaged layer in the first opening area and the front plating layer, secondary alkaline solution corrosion is prevented from damaging the first semiconductor layer.
[0098] In S9, a chain cleaning machine is used to clean and remove the mask layer on the back of the silicon wafer to prevent the anti-reflection layer on the front of the silicon wafer from being cleaned and removed. The cleaning liquid used is an aqueous solution containing hydrofluoric acid, the concentration of hydrofluoric acid is 10%-15%, the reaction temperature is 20℃-35℃, and the transmission roller speed of the chain cleaning machine is 1.2 m / min-3.0m / min. Afterwards, a standard RCA solution is used for backwashing to obtain a clean interface in the first opening area to ensure the cleanliness of the interface in the first opening area.
[0099] In S10, the thickness of the intrinsic amorphous silicon layer is 5nm-15nm, and the thickness of the fourth doped layer is 5nm-20nm. Specifically, the second semiconductor layer is directly plated after etching and backwashing, and does not need to be subjected to high temperature treatment, so the interface is cleaner and the passivation quality of the film layer is greatly improved.
[0100] Preferably, after S10, the method for preparing a back contact battery further comprises:
[0101] S11. Etching openings on the second semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart;
[0102] S12 forming a conductive film layer on the back side of the silicon wafer;
[0103] S13. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening region and covers the second semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;
[0104] S14. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.
[0105] It should be noted that in S11, an opening is etched on the second semiconductor layer on the back of the silicon wafer by laser or mask etching to form a second opening area, and the second semiconductor layer in the second opening area is etched away. The width of the second opening area W2 is 100 μm-300 μm. Laser etching is preferred, and the etching laser is an ultraviolet laser or a green laser, and the pulse width is less than 100 ns.
[0106] In S12, a conductive film layer is deposited on the back of the silicon wafer using physical vapor deposition technology (PVD) or activated plasma deposition technology (RPD). The thickness of the conductive film layer is 40nm-80nm. The material of the conductive film layer can be an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.
[0107] In S13, an isolation groove is formed on the conductive film layer by laser or etching. The isolation groove is used to achieve the insulation function between two adjacent parts of the conductive film layer. The isolation groove is located between the first opening area and the second opening area. The width of the isolation groove W3 is 20μm-100μm. After the isolation groove is formed, the resistance between the first semiconductor layer and the second semiconductor layer is greater than 1KΩ.
[0108] In S14, a first electrode is formed on a portion of the conductive film layer located in a first opening area on the back side of the silicon wafer by using screen printing technology, and a second electrode is formed on a portion of the conductive film layer located in a second opening area on the back side of the silicon wafer.
[0109] In a second aspect, the present invention provides a back-contact battery, which is prepared by the above-mentioned method for preparing a back-contact battery.
[0110] In a third aspect, the present invention provides a photovoltaic module comprising the above-mentioned back contact cell.
[0111] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0112] Example 1
[0113] A back contact battery is prepared by the following steps:
[0114] S1. Figure 1 As shown, the N-type single crystal silicon wafer 1 is double-sided polished and cleaned, and the silicon wafer 1 is a Czochralski single crystal silicon wafer.
[0115] S2. Figure 2As shown, a first semiconductor layer is deposited on the back of a silicon wafer 1, and the first semiconductor layer includes a first tunneling oxide layer 2, an intrinsic polysilicon layer 13, a first doping layer 3, and a second doping layer arranged in sequence, and then the first semiconductor layer is annealed to convert the second doping layer into a mask layer 4. Among them, the thickness of the first tunneling oxide layer 2 is 1.5nm, the thickness of the intrinsic polysilicon layer 13 is 20nm, the thickness of the first doping layer 3 is 80nm, the thickness of the second doping layer is 30nm, and the thickness of the mask layer 4 is 50nm. The deposition conditions of the first tunneling oxide layer 2 are: passing nitrous oxide, the nitrous oxide flow rate is 10000sccm, the reaction time is 60s, the reaction pressure is 150Pa, and the reaction power is 7000W. The deposition conditions of the intrinsic polysilicon layer 13 are: passing silane and hydrogen, the silane flow rate is 2000sccm, the hydrogen flow rate is 8000sccm, the reaction time is 300s, the reaction pressure is 400Pa, and the reaction power is 3000W. The deposition conditions of the first doping layer 3 are: silane, phosphine and hydrogen are introduced, the silane flow rate is 2000sccm, the phosphine flow rate is 1200sccm, the hydrogen flow rate is 8000sccm, the reaction time is 500s, the reaction pressure is 400Pa, and the reaction power is 4000W. The deposition conditions of the second doping layer are: silane, phosphine, hydrogen, nitrogen and methane are introduced, the silane flow rate is 2000sccm, the phosphine flow rate is 2000sccm, the hydrogen flow rate is 8000sccm, the nitrogen flow rate is 2000sccm, the methane flow rate is 700sccm, the reaction time is 200s, the reaction pressure is 400Pa, and the reaction power is 4000W. The annealing conditions are: oxygen is introduced, the annealing pressure is 10000Pa, the annealing temperature is 900℃, the annealing time is 90min, and the oxygen flow rate is 5000sccm.
[0116] S3. Clean and remove the oxide layer on the front side of the silicon wafer caused by S2 annealing, and use a chain cleaning machine to clean and remove the oxide layer. The cleaning liquid used is an aqueous solution containing hydrofluoric acid, the hydrofluoric acid concentration is 12%, the reaction temperature is 30°C, and the transmission roller speed of the chain cleaning machine is 2.0m / min.
[0117] S4. Figure 3 As shown, a velvet surface is formed on the front side of the silicon wafer 1 through texturing and cleaning, and the texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 3%, the mass percentage of the texturing additive is 0.75%, the texturing time is 10 minutes, the texturing temperature is 80°C, the corrosion depth of the front side of the silicon wafer 1 is 3.5μm, and the texturing additive contains benzoic acid and aminotri(methylene)phosphoric acid.
[0118] S5. Figure 4As shown, deposition and annealing are performed on the front side of the silicon wafer 1 to form a passivation layer, and the passivation layer includes a second tunneling oxide layer 5 and a third doping layer 6 arranged in sequence. The thickness of the second tunneling oxide layer 5 is 1.5 nm, and the thickness of the third doping layer 6 is 8 nm. The annealing conditions are: oxygen flow, annealing pressure of 10000 Pa, annealing temperature of 875°C, annealing time of 70 min, and oxygen flow rate of 5000 sccm.
[0119] S6. Figure 4 As shown, the second phosphorus-silicate glass layer generated by S5 deposition on the passivation layer is cleaned and removed, and the second phosphorus-silicate glass layer is cleaned and removed by a chain cleaning machine, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the hydrofluoric acid concentration is 7.5%, the reaction temperature is 30°C, and the transmission roller speed of the chain cleaning machine is 2.0 m / min. Then, an anti-reflection layer 7 is formed on the passivation layer, wherein the thickness of the anti-reflection layer 7 is 100 nm.
[0120] S7. Figure 5 As shown, laser etching is used to etch openings on the first semiconductor layer, the mask layer 4 and the winding coating produced by S6 deposition to form a first opening area, and the first semiconductor layer, the mask layer 4 and the winding coating in the first opening area are etched away. The width of the first opening area W1 is 600μm, and the laser used for etching is a green laser with a power of 40KW and a frequency of 600kHz.
[0121] S8. Figure 5 As shown, a texturing cleaning method is used to remove the damaged layer on the silicon wafer 1 in the first opening area caused by S7 etching, and the coating layer is removed at the same time. The texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1.5%, the mass percentage of the texturing additive is 0.75%, the texturing time is 4 minutes, the texturing temperature is 80°C, and the texturing additive contains benzoic acid and aminotri(methylene)phosphoric acid.
[0122] S9. Figure 6 As shown, the mask layer 4 is cleaned and removed by a chain cleaning machine, the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the concentration of hydrofluoric acid is 12%, the reaction temperature is 25°C, and the transmission roller speed of the chain cleaning machine is 1.6m / min. Then, RCA solution is used for backwashing, and the RCA solution is a standard RCA solution.
[0123] S10. Figure 7As shown, a second semiconductor layer is deposited on the back side of the silicon wafer 1 so that a portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer 1, and the other portion extends into the first opening area and covers the silicon wafer 1. The second semiconductor layer includes an intrinsic amorphous silicon layer 8 and a fourth doped layer 9 arranged in sequence. The thickness of the intrinsic amorphous silicon layer 8 is 10 nm, and the thickness of the fourth doped layer 9 is 12 nm.
[0124] S11. Figure 8 As shown, laser etching is used to etch openings on the second semiconductor layer to form second opening areas that are alternately arranged with the first opening areas and spaced apart, and the second semiconductor layer in the second opening areas is etched away. The width of the second opening area W2 is 200μm, and the etching laser is a green laser with a pulse width of 50ns.
[0125] S12. Fig. 9 As shown, a conductive film layer 10 is formed on the back of the silicon wafer 1 by physical vapor deposition (PVD) technology. The thickness of the conductive film layer 10 is 60 nm, and the material of the conductive film layer 10 is a tin oxide-doped indium oxide film.
[0126] S13. Fig.10 As shown, an isolation groove is opened on the conductive film layer 10 by laser etching, so that a portion of the conductive film layer 10 separated from each other extends into the first opening area and covers the second semiconductor layer, and the other portion extends into the second opening area and covers the first semiconductor layer. The width of the isolation groove is 50μm. After the isolation groove is formed, the resistance between the first semiconductor layer and the second semiconductor layer is 2KΩ.
[0127] S14. Fig.11 As shown, a first electrode 11 is formed on a portion of the conductive film layer 10 extending into the first opening region, and a second electrode 12 is formed on a portion of the conductive film layer 10 extending into the second opening region by using screen printing technology.
[0128] Example 2
[0129] The method of Example 1 is referred to, except that the thickness of the mask layer 4 is adjusted to 30 nm.
[0130] Example 3
[0131] The method of Example 1 is followed, except that the reaction conditions for forming the second doping layer in S2 are adjusted so that the silane flow rate is 1000sccm, the phosphine flow rate is 2000sccm, the hydrogen flow rate is 7000sccm, the nitrogen flow rate is 1000sccm, the methane flow rate is 500sccm, the reaction time is 180s, the reaction pressure is 400Pa, and the reaction power is 4000W.
[0132] Example 4
[0133] The method of Example 1 is referred to, except that the cleaning method in S8 is adjusted, and polishing cleaning is used to remove the damaged layer on the silicon wafer 1 in the first opening area caused by etching in S7, and the plating layer is removed at the same time. The polishing solution used is a mixed solution of potassium hydroxide or sodium hydroxide, a polishing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 2%, the mass percentage of the polishing additive is 1.5%, the reaction time is 180s, the reaction temperature is 70°C, and the polishing additive contains benzoic acid and aminotri(methylene)phosphoric acid.
[0134] Example 5
[0135] The method of Example 1 is referred to, except that the cleaning conditions in S9 are adjusted so that the hydrofluoric acid concentration is 15%, the reaction temperature is 30° C., and the transmission roller speed of the chain cleaning machine is 2 m / min.
[0136] Comparative Example 1
[0137] The method of Example 1 is referred to, except that, during the process of forming the second doping layer in S2, nitrogen and methane are not introduced.
[0138] Comparative Example 2
[0139] The method of Example 1 is referred to, except that step S4 is carried out using the texturing cleaning process of step S8, and the texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1.5%, the mass percentage of the texturing additive is 0.75%, the texturing time is 4 minutes, the texturing temperature is 80°C, the texturing additive contains benzoic acid and aminotri(methylene)phosphoric acid, and the corrosion depth of the front side of the silicon wafer 1 is 1.2μm.
[0140] Comparative Example 3
[0141] The method of Example 1 is referred to, except that step S8 is carried out using the texturing cleaning process of step S4, and the texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 3%, the mass percentage of the texturing additive is 0.75%, the texturing time is 10 minutes, the texturing temperature is 80°C, and the texturing additive contains benzoic acid and aminotri(methylene)phosphoric acid.
[0142] Test Case
[0143] The back contact cells obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in Table 1.
[0144] Table 1
[0145]
[0146] It can be seen from the above results that, compared with the comparative example, by adopting the embodiment scheme of the present invention, the mask layer 4 (the first phosphorus silicon glass layer doped with nitrogen and / or carbon) can be retained after texturing and then the front side is plated, and then the opening is etched, and the first semiconductor layer is protected by the mask layer 4. First, the first semiconductor layer can be prevented from being scratched or affected by high temperature during the front side plating process, thereby improving the passivation performance and open circuit voltage of the battery. Second, the first semiconductor layer can be prevented from being corroded by the cleaning solution during the cleaning and removal of the wrapping plating process, thereby further improving the passivation performance and open circuit voltage of the battery. Third, the second semiconductor layer can be directly plated after the etching and backwashing is completed without high temperature treatment, thereby improving the interface cleanliness in the first opening area and improving the passivation quality of the film layer. Fourth, the first phosphorus silicon glass layer doped with nitrogen and / or carbon is used as the mask layer 4, which has a high degree of density and strong corrosion resistance, thereby improving the protection effect on the first semiconductor layer. Fifth, the thickness of the back mask layer 4 will be increased during the front side annealing process, thereby further improving the protection effect on the first semiconductor layer.
[0147] At the same time, a low-concentration alkaline solution is used to remove the damaged layer in the first opening area and the coating on the front side, and the etching amount is controlled to be as low as possible to ensure that the damaged layer in the first opening area and the coating on the front side are removed while preventing secondary alkaline solution corrosion from damaging the first semiconductor layer, thereby ensuring the quality of the battery.
[0148] Furthermore, according to Example 1 and Examples 2-5, it can be seen that the preferred battery structure of the present invention is more conducive to enhancing the passivation performance of the back contact battery, increasing the open circuit voltage, improving the passivation quality of the film layer, and improving the battery conversion efficiency.
[0149] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a back contact battery, characterized in that: The following steps are involved: S1. Provide double-sided polished silicon wafers; S2. depositing a first semiconductor layer on the back side of the silicon wafer, the first semiconductor layer comprising a first tunneling oxide layer, an intrinsic polysilicon layer, a first doping layer, and a second doping layer arranged in sequence, and then annealing the first semiconductor layer to convert the second doping layer into a mask layer, wherein the second doping layer is doped with nitrogen and / or carbon, and the mask layer is a first phosphosilicate glass layer doped with nitrogen and / or carbon; S2 includes: introducing laughing gas and reacting to form the first tunneling oxide layer under the condition of turning on the glow, wherein the thickness of the first tunneling oxide layer is 1nm-2nm; Passing silane and hydrogen into the gas and reacting to form the intrinsic polysilicon layer under the condition of turning on the glow, wherein the thickness of the intrinsic polysilicon layer is 10nm-30nm; Silane, phosphine and hydrogen are introduced and reacted under the condition of turning on the glow to form the first doping layer, the thickness of the first doping layer is 30nm-100nm, and the reaction conditions for forming the first doping layer are: silane flow rate is 1000sccm-3000sccm, phosphine flow rate is 1000sccm-2000sccm, hydrogen flow rate is 7000sccm-9000sccm, reaction time is 200s-800s, reaction pressure is 300Pa-500Pa, and reaction power is 3000W-5000W; Silane, phosphine, hydrogen, nitrogen and / or methane are introduced, and the second doping layer is formed by reaction under the condition of turning on the glow, the thickness of the second doping layer is 10nm-30nm, and the reaction conditions for forming the second doping layer are: silane flow rate is 1000sccm-3000sccm, phosphine flow rate is 2000sccm-3000sccm, hydrogen flow rate is 7000sccm-9000sccm, nitrogen flow rate is 1000sccm-3000sccm, methane flow rate is 500sccm-1000sccm, reaction time is 100s-300s, reaction pressure is 300Pa-500Pa, and reaction power is 3000W-5000W; Passing oxygen and performing high-temperature annealing on the first semiconductor layer, so that the second doping layer is converted into the mask layer, wherein the thickness of the mask layer is 30nm-50nm; S3 cleaning and removing the oxide layer on the front side of the silicon wafer due to annealing S2; S4. By cleaning the velvet surface, a velvet surface is formed on the front side of the silicon wafer; S5. Deposition and annealing are performed on the front side of the silicon wafer to form a passivation layer, wherein the passivation layer comprises a second tunneling oxide layer and a third doping layer disposed in sequence; S6. Cleaning and removing the second phosphosilicate glass layer produced by the deposition of S5 on the passivation layer, and then forming an anti-reflection layer on the passivation layer; S7. Etching an opening on the first semiconductor layer, the mask layer, and the coating layer generated by the deposition in S6 to form a first opening region; S8. removing the damaged layer on the silicon wafer in the first opening area caused by etching in S7, and removing the plating layer at the same time, wherein the damaged layer and the plating layer are removed by texturing cleaning or polishing cleaning, and the texturing solution used in the texturing cleaning and the polishing solution used in the polishing cleaning contain potassium hydroxide or sodium hydroxide, and the mass percentage of potassium hydroxide or sodium hydroxide is less than 3%; S9. Cleaning and removing the mask layer, and then backwashing with RCA solution; S10. Depositing a second semiconductor layer on the back side of the silicon wafer so that a portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion extends into the first opening area and covers the silicon wafer, the second semiconductor layer comprising an intrinsic amorphous silicon layer and a fourth doping layer arranged in sequence.
2. The method for preparing a back contact battery according to claim 1, characterized in that: In S2, the reaction conditions for forming the first tunneling oxide layer are: the laughing gas flow rate is 8000sccm-12000sccm, the reaction time is 20s-100s, the reaction pressure is 100Pa-200Pa, and the reaction power is 3000W-10000W; And / or, the reaction conditions for forming the intrinsic polysilicon layer are: silane flow rate is 1000sccm-3000sccm, hydrogen flow rate is 7000sccm-9000sccm, reaction time is 200s-400s, reaction pressure is 300Pa-500Pa, and reaction power is 2000W-4000W; And / or, the high temperature annealing conditions are: annealing pressure of 5000Pa-50000Pa, annealing temperature of 850°C-950°C, annealing time of 60min-120min, and oxygen flow rate of 2000sccm-8000sccm.
3. The method for preparing a back contact battery according to claim 1, characterized in that: In S3, a chain cleaning machine is used to clean and remove the oxide layer, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the hydrofluoric acid concentration is 10%-15%, the reaction temperature is 20°C-35°C, and the transmission roller speed of the chain cleaning machine is 1.2 m / min-3.0 m / min.
4. The method for preparing a back contact battery according to claim 1, characterized in that: In S4, the texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 2%-5%, the mass percentage of the texturing additive is 0.5%-1%, the texturing time is 8min-12min, the texturing temperature is 75℃-85℃, the corrosion depth of the front side of the silicon wafer is 3μm-4μm, and the texturing additive contains at least one of benzoic acid, aminotri(methylenephosphoric acid), polyepoxysuccinic acid and polyaspartic acid.
5. The method for preparing a back contact battery according to claim 1, characterized in that: In S5, the second tunneling oxide layer and the third doping layer are sequentially deposited on the silicon wafer by plasma enhanced chemical vapor deposition, and oxygen annealing is performed on them, wherein the thickness of the second tunneling oxide layer is 1nm-2nm, and the thickness of the third doping layer is 1nm-15nm.
6. The method for preparing a back contact battery according to claim 5, characterized in that: In S5, the oxygen annealing conditions are: annealing pressure is 5000Pa-50000Pa, annealing temperature is 850°C-900°C, annealing time is 60min-120min, and oxygen flow rate is 2000sccm-8000sccm.
7. The method for preparing a back contact battery according to claim 1, characterized in that: In S6, the second phosphorus silicon glass layer is cleaned and removed by a chain cleaning machine, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the concentration of hydrofluoric acid is 5%-10%, the reaction temperature is 20° C.-35° C., and the transmission roller speed of the chain cleaning machine is 1.2 m / min-3.0 m / min; And / or, an anti-reflection layer is formed on the passivation layer by plasma enhanced chemical vapor deposition, wherein the thickness of the anti-reflection layer is 70nm-120nm.
8. The method for preparing a back contact battery according to claim 1, characterized in that: In S8, the thickness of the damaged layer is less than or equal to 1 μm.
9. The method for preparing a back contact battery according to claim 8, characterized in that: In S8, if the damaged layer and the winding plating layer are removed by texturing cleaning, the texturing liquid used is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1%-2%, the mass percentage of the texturing additive is 0.5%-1%, the texturing time is 4min-8min, the texturing temperature is 75°C-85°C, and the texturing additive contains at least one of benzoic acid, aminotrimethylphosphonic acid, polyepoxysuccinic acid and polyaspartic acid; If the damaged layer and the coating layer are removed by polishing and cleaning, the polishing solution used is a mixed solution of potassium hydroxide or sodium hydroxide, a polishing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1.5%-3%, the mass percentage of the polishing additive is 1%-2%, the reaction temperature is 60°C-75°C, the reaction time is 120s-240s, and the polishing additive contains at least one of benzoic acid, aminotri(methylenephosphoric acid), polyepoxysuccinic acid and polyaspartic acid.
10. The method for preparing a back contact battery according to claim 1, characterized in that: In S9, a chain cleaning machine is used to clean and remove the mask layer on the back side of the silicon wafer to prevent the anti-reflection layer on the front side of the silicon wafer from being cleaned and removed, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the hydrofluoric acid concentration is 10%-15%, the reaction temperature is 20°C-35°C, and the transmission roller speed of the chain cleaning machine is 1.2 m / min-3.0 m / min.
11. The method for preparing a back contact battery according to claim 1, characterized in that: After S10, the method for preparing the back contact battery further includes: S11. Etching openings on the second semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart from each other; S12 forming a conductive film layer on the back side of the silicon wafer; S13. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening area and covers the second semiconductor layer, and another portion extends into the second opening area and covers the first semiconductor layer; S14. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.
12. A back contact battery, characterized in that: The back contact battery is prepared by the method for preparing a back contact battery as described in any one of claims 1 to 11.
13. A photovoltaic module, characterized in that: Comprising a back contact cell as described in claim 12.