A high temperature fiber filter tube and preparation method thereof

Through the method of winding molding of high-aluminum aluminum silicate fiber cotton and spraying composite adhesive, the problems of waste of water and insufficient performance for high-temperature fiber filter pipes are solved, the porosity and toughness of the product are improved, the breathability resistance is reduced, and the air permeability is achieved Efficient water resource utilization and production efficiency.

CN118662982BActive Publication Date: 2024-11-05SHANDONG RES & DESIGN ACADEMY OF IND CERAMICS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411146993.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-05
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing high-temperature fiber filter tube preparation method requires a large amount of water resources, resulting in waste and pollution of water resources, and the product has low porosity, large air permeability and poor toughness.

Method used

The fiber web is prepared by high-aluminum aluminum silicate fiber cotton. The fiber web is wound and molded by vacuum mold and sprayed with composite adhesive. The molding speed and temperature are controlled, combined with electric oven drying, which reduces water and drying time, and improves the strength of the fiber web and Porosity.

Benefits of technology

The strength, porosity, and air permeability resistance of high-temperature fiber filter tubes are improved, which reduces water resource consumption and drying time, and improves production efficiency and product performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118662982B_ABST
    Figure CN118662982B_ABST
Patent Text Reader

Abstract

The present invention provides a high-temperature fiber filter tube and a preparation method thereof, which belongs to the technical field of filter materials for gaseous fluids. The preparation method includes preparing a fiber net, winding and forming, and drying; the winding method is to wind the fiber net on a vacuum mold, and during the molding process, the fiber net is sizing by synchronously spraying an aqueous dispersion of a composite binder, and the vacuum mold is sucked at the same time; the aqueous dispersion of the composite binder, in terms of mass percentage, includes the following components: silica sol 24-26wt%, boric acid 9-11wt%; cellulose 2.6-3.2wt%, corn starch 0.8-1.2wt%; alpha alumina 2.7-3.3wt%, zirconium oxide 0.8-1.2wt%, small-particle magnesium oxide 0.7-1.3wt%, and water supplementation 100%. The present invention prepares a high-temperature fiber filter tube with high strength, large porosity, small air permeability resistance and strong toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-temperature fiber filter tube and a preparation method thereof, belonging to the technical field of filter materials for gaseous fluids. Background Art

[0002] The high-temperature fiber filter tube has the function of dust removal and filtration, and has the advantages of high filtration efficiency and wide application range. The high-temperature fiber filter tube is loaded with denitrification catalyst by spraying, impregnation, etc., and can have the functions of dust removal and denitrification at the same time, and can be used for the treatment of high-temperature flue gas.

[0003] Most of the existing high-temperature fiber filter tubes are prepared by vacuum filtration and sintering-free method. The specific method is to use ceramic fiber as raw material to prepare ultra-low concentration ceramic fiber slurry, and then filter and shape it through an external mold or an internal mold, and obtain a high-temperature fiber filter tube after drying and curing. This preparation method consumes a large amount of water to disperse the ceramic fiber to obtain a low-concentration ceramic fiber slurry, which not only causes a serious waste of water resources, but also the binder and other components in the slurry are difficult to recycle, and will cause water pollution problems after discharge. In addition, this method requires a long drying time, and the prepared high-temperature fiber filter tube has the disadvantages of low porosity, large air permeability resistance, and poor toughness. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a high-temperature fiber filter tube and a preparation method thereof, to achieve the following invention objectives: reduce water consumption, shorten drying time, ensure the strength of the high-temperature fiber filter tube, increase porosity, reduce air permeability resistance, and improve toughness.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A method for preparing a high-temperature fiber filter tube, the method comprising preparing a fiber web, winding and forming, and drying, as follows:

[0007] (1) Preparation of fiber web

[0008] Select high-aluminum aluminum silicate fiber cotton (aluminum content 52-55wt%, aluminum silicon content ≥99wt%) with a diameter of 3-5μm; then loosen and comb the fiber cotton to obtain a fiber web with a thickness of 4±0.5mm to ensure that the fiber web will not be broken due to being too thin, and will not affect the gluing due to being too thick.

[0009] (2) Winding

[0010] Then the fiber web is wound on the vacuum mold and the winding angle is set to 67-73°. When the molding starts, the winding speed is controlled to 72-77r / min to avoid breaking the fiber web due to too fast speed. When the wall thickness is about 2 / 3, the speed is adjusted to 48-52r / min to prevent the sizing effect from being affected due to too fast increase in wall thickness.

[0011] During the fiber web forming process, the fiber web is sizing by spraying the aqueous dispersion of the composite binder synchronously to ensure that the mass ratio of the fiber web to the composite binder is 3:1.5-1.7; during the sizing process, the pressure of the spray gun fan is controlled to be 0.46-0.52MPa, the flow rate is 0.57-0.64MPa, and the atomization pressure is 0.86-0.9MPa;

[0012] At the same time, the vacuum mold suction pressure is controlled at 0.18-0.22MPa to ensure the suction effect;

[0013] The high-temperature filter tube blank is formed into an outer diameter of 149.4-150.6 mm, a wall thickness of 14.7-15.3 mm, and a length of 2.9-3.1 m.

[0014] The aqueous dispersion of the composite binder includes the following components by mass percentage: 24-26wt% silica sol, 9-11wt% boric acid; 2.6-3.2wt% cellulose, 0.8-1.2wt% corn starch; 2.7-3.3wt% α-alumina, 0.8-1.2wt% zirconium oxide, 0.7-1.3wt% small-particle magnesium oxide, and water makes up 100%.

[0015] The solid content of the silica sol is 30%;

[0016] The viscosity of the cellulose is 20000 mPa·s;

[0017] The particle size of the α-alumina is 0.7 μm;

[0018] The particle size of the zirconium oxide is 1 μm;

[0019] The particle size of the small-particle magnesium oxide is 1 μm.

[0020] (3) Drying

[0021] The formed green body is dried in an electric oven. The specific drying process is as follows: heating from room temperature to 77-81°C within 0.7-1.2h, then to 98-103°C within 1.8-2.2h, and kept warm for 1.8-2.2h, then to 118-123°C within 0.7-1.2h, and kept warm for 1-2h to obtain a high-temperature fiber filter tube.

[0022] The present invention can effectively avoid the breaking of the fiber web and the delamination and cracking of the high-temperature fiber filter tube by selecting fiber cotton, controlling the thickness of the fiber web and the angle and speed of winding, and adopting a specific composite adhesive and dosage. While ensuring the strength of the high-temperature fiber filter tube, the porosity thereof is increased, the air permeability resistance is reduced, and the toughness is improved.

[0023] Compared with the prior art, the present invention achieves the following beneficial effects:

[0024] (1) The present invention simultaneously performs fiber mesh winding and adhesive spraying to prepare a high-temperature fiber filter tube with high strength, greater porosity, smaller air resistance, and stronger toughness. The high-temperature fiber filter tube prepared by the present invention has a flexural strength of 1.8-2MPa, a compressive strength of 4.2-4.5MPa, a porosity of 81.5-82%, an air resistance of 30-35 pa, a displacement of 90-93mm when the tension is 60N, a tension of 95-98N when broken, and a displacement of 129-133mm;

[0025] (2) The present invention adopts a dry molding process, which does not require a large amount of water for slurry dispersion and has a short drying time of 6-8.8 hours. It does not require high-temperature firing, effectively shortens the product turnover cycle, improves production efficiency, and saves a lot of water and energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the preparation method of the high temperature fiber filter tube of the present invention. DETAILED DESCRIPTION

[0027] Example 1

[0028] The following steps are involved:

[0029] (1) Preparation of fiber web

[0030] Select high-aluminum aluminum silicate fiber cotton (aluminum content 52-55wt%, aluminum silicon content ≥99wt%) with a diameter of 3-5μm; then loosen and comb the fiber cotton to obtain a fiber web with a thickness of 4±0.5mm to ensure that the fiber web will not be broken due to being too thin, and will not affect the gluing due to being too thick.

[0031] (2) Winding

[0032] Then the fiber web is wound on the vacuum mold and the winding angle is set to 70°. When the molding starts, the winding speed is controlled to 75r / min to avoid breaking the fiber web due to too fast speed. When the wall thickness is about 2 / 3, the speed is adjusted to 50r / min to prevent the sizing effect from being affected due to too fast increase in wall thickness.

[0033] During the fiber web forming process, the fiber web is sizing by spraying the aqueous dispersion of the composite binder simultaneously to ensure that the mass ratio of the fiber web to the composite binder is 3:1.6; during the sizing process, the pressure of the spray gun fan is controlled to be 0.5MPa, the flow rate is 0.6MPa, and the atomization pressure is 0.88MPa;

[0034] At the same time, the vacuum mold suction pressure is controlled at 0.2MPa to ensure the suction effect;

[0035] The high-temperature filter tube blank is formed into an outer diameter of 150mm, a wall thickness of 15mm and a length of 3m.

[0036] The aqueous dispersion of the composite binder includes the following components by mass percentage: 25wt% silica sol, 10wt% boric acid, 3wt% cellulose, 2wt% corn starch, 3wt% α-alumina, 1wt% zirconium oxide, 1wt% small-particle magnesium oxide, and water makes up to 100%.

[0037] The solid content of the silica sol is 30%;

[0038] The viscosity of the cellulose is 20000 mPa·s;

[0039] The particle size of the α-alumina is 0.7 μm;

[0040] The particle size of the zirconium oxide is 1 μm;

[0041] The particle size of the small-particle magnesium oxide is 1 μm.

[0042] (3) Drying

[0043] The formed green body is dried in an electric oven. The specific drying process is as follows: heating from room temperature to 80°C within 1 hour, then to 100°C within 2 hours, keeping warm for 2 hours, then to 120°C within 1 hour, keeping warm for 1.5 hours, to obtain a high-temperature fiber filter tube.

[0044] Example 2

[0045] The following steps are involved:

[0046] (1) Preparation of fiber web

[0047] Select high-aluminum aluminum silicate fiber cotton (aluminum content 52-55wt%, aluminum silicon content ≥99wt%) with a diameter of 3-5μm; then loosen and comb the fiber cotton to obtain a fiber web with a thickness of 4±0.5mm to ensure that the fiber web will not be broken due to being too thin, and will not affect the gluing due to being too thick.

[0048] (2) Winding

[0049] Then the fiber web is wound on the vacuum mold and the winding angle is set to 67°. When the molding starts, the winding speed is controlled to 72r / min to avoid breaking the fiber web due to too fast speed. When the wall thickness is about 2 / 3, the speed is adjusted to 48r / min to prevent the sizing effect from being affected due to too fast increase in wall thickness.

[0050] During the fiber web forming process, the fiber web is sizing by spraying the aqueous dispersion of the composite binder simultaneously to ensure that the mass ratio of the fiber web to the composite binder is 3:1.5; during the sizing process, the pressure of the spray gun fan is controlled to be 0.46MPa, the flow rate is 0.57MPa, and the atomization pressure is 0.86MPa;

[0051] At the same time, the vacuum mold suction pressure is controlled at 0.18MPa to ensure the suction effect;

[0052] The high-temperature filter tube blank is formed into an outer diameter of 149.4 mm, a wall thickness of 14.7 mm, and a length of 2.9 m.

[0053] The aqueous dispersion of the composite binder includes the following components, by mass percentage: 24wt% silica sol, 9wt% boric acid, 2.6wt% cellulose, 0.8wt% corn starch, 2.7wt% alpha alumina, 0.8wt% zirconium oxide, 0.7wt% small-particle magnesium oxide, and water makes up 100%.

[0054] The solid content of the silica sol is 30%;

[0055] The viscosity of the cellulose is 20000 mPa·s;

[0056] The particle size of the α-alumina is 0.7 μm;

[0057] The particle size of the zirconium oxide is 1 μm;

[0058] The particle size of the small-particle magnesium oxide is 1 μm.

[0059] (3) Drying

[0060] The formed green body is dried in an electric oven. The specific drying process is as follows: heating from room temperature to 77°C within 0.7h, then to 98°C within 1.8h, keeping warm for 1.8h, then to 118°C within 0.7h, keeping warm for 2h, to obtain a high-temperature fiber filter tube.

[0061] Example 3

[0062] The following steps are involved:

[0063] (1) Preparation of fiber web

[0064] Select high-aluminum aluminum silicate fiber cotton (aluminum content 52-55wt%, aluminum silicon content ≥99wt%) with a diameter of 3-5μm; then loosen and comb the fiber cotton to obtain a fiber web with a thickness of 4±0.5mm to ensure that the fiber web will not be broken due to being too thin, and will not affect the gluing due to being too thick.

[0065] (2) Winding

[0066] Then the fiber web was wound on the vacuum mold and the winding angle was set to 73°. When the molding started, the winding speed was controlled to 77r / min to avoid breaking the fiber web due to too fast speed. When the wall thickness was about 2 / 3, the speed was adjusted to 52r / min to prevent the sizing effect from being affected due to too fast increase in wall thickness.

[0067] During the fiber web forming process, the fiber web is sizing by spraying the aqueous dispersion of the composite binder simultaneously, ensuring that the mass ratio of the fiber web to the composite binder is 3:1.7; during the sizing process, the pressure of the spray gun fan is controlled to be 0.52MPa, the flow rate is 0.64MPa, and the atomization pressure is 0.9MPa;

[0068] At the same time, the vacuum mold suction pressure is controlled at 0.22MPa to ensure the suction effect;

[0069] The high-temperature filter tube blank is formed into an outer diameter of 150.6 mm, a wall thickness of 15.3 mm, and a length of 3.1 m.

[0070] The aqueous dispersion of the composite binder includes the following components, by mass percentage: 26wt% silica sol, 11wt% boric acid, 3.2wt% cellulose, 1.2wt% corn starch, 3.3wt% α-alumina, 1.2wt% zirconium oxide, 1.3wt% small-particle magnesium oxide, and water makes up 100%.

[0071] The solid content of the silica sol is 30%;

[0072] The viscosity of the cellulose is 20000 mPa·s;

[0073] The particle size of the α-alumina is 0.7 μm;

[0074] The particle size of the zirconium oxide is 1 μm;

[0075] The particle size of the small-particle magnesium oxide is 1 μm.

[0076] (3) Drying

[0077] The formed green body is dried in an electric oven. The specific drying process is as follows: heating from room temperature to 81°C within 1.2 hours, then to 103°C within 2.2 hours, and kept warm for 2.2 hours, then to 123°C within 1.2 hours, and kept warm for 1 hour to obtain a high-temperature fiber filter tube.

[0078] Comparative Example 1

[0079] The same high-aluminum aluminum silicate fiber cotton as in Example 1 was used as the raw material, and shearing was performed to obtain the processed aluminum silicate fiber with an aspect ratio of 100; then 10 kg of aluminum silicate fiber, 1 kg of cellulose, 150 kg of silica sol, and 250 kg of water were mixed, and the speed of the disperser was adjusted to 850 r / min, and stirred for 40 min until uniform dispersion was obtained to obtain a slurry. The slurry was placed in a vacuum mold for suction filtration molding, and the suction pressure was controlled to 0.1 MPa and the centrifugal speed was 70 r / min; when the pressure dropped to 0.05 MPa, the suction and centrifugation were stopped, and the demoulding and drying were performed, and the drying temperature was 130°C for 20 hours to obtain a high-temperature filter tube with an outer diameter of 150 mm, a wall thickness of 15 mm, and a length of 3 m.

[0080] The silica sol has a pH of 5 and a silicon dioxide content of 30%.

[0081] Comparative Example 2

[0082] On the basis of Example 1, the addition of α-alumina, zirconium oxide and small-particle magnesium oxide was omitted, the water was supplemented to 100%, and the rest was the same as Example 1, and a high-temperature fiber filter tube was obtained, but the problems of stratification and cracking occurred.

[0083] The high temperature fiber filter tubes prepared in Examples 1-3, Comparative Example 1 and Comparative Example 2 were tested for flexural strength, compressive strength, porosity and air permeability resistance. The results are shown in Table 1.

[0084] Table 1 Performance test results of high temperature fiber filter tube

[0085]

[0086] It can be seen that compared with Comparative Example 1, the porosity of the high-temperature fiber filter tube in Example 1 of the present invention is significantly improved, and the air permeability resistance is significantly reduced. When the porosity of the high-temperature fiber filter tube in the field reaches 75%, it is very difficult to increase it by 1 percentage point. The porosity of Example 1 is increased by 6 percentage points compared with Comparative Example 1, achieving significant technical progress.

[0087] The high-temperature fiber filter tube prepared in Comparative Example 2 showed delamination and cracking problems after molding and drying. Compared with Example 1, the flexural strength and compressive strength of the high-temperature fiber filter tube in Comparative Example 2 were significantly reduced, and the air permeability resistance was increased by 66.7%, indicating that the metal oxides (α-alumina, zirconium oxide, small-particle magnesium oxide) in the composite binder have a significant effect on the strength and air permeability of the finally prepared high-temperature fiber filter tube.

[0088] The high-temperature fiber filter tubes prepared in Example 1, Comparative Example 1, and Comparative Example 2 were tested for toughness performance. The specific test method was as follows: the high-temperature fiber filter tube was placed vertically on a 3-meter platform, the upper end was fixed, and the initial position of the high-temperature fiber filter tube was recorded. Subsequently, a horizontal pulling force was applied to the lower end, and the displacement under the same pulling force and the force and displacement applied to break the high-temperature fiber filter tube were recorded respectively. The test data are shown in Tables 2 and 3.

[0089] Table 2 Displacement of high temperature fiber filter tube under the same tension

[0090]

[0091] Table 3 Tensile force and displacement when high temperature fiber filter tube breaks

[0092]

[0093] It can be seen from Table 2 and Table 3 that the high-temperature fiber filter tube prepared in Example 1 has significantly greater displacement at 60N, and greater tensile force and displacement at break than those in Comparative Example 1, indicating that the high-temperature fiber filter tube prepared in Example 1 has stronger toughness than that in Comparative Example 1; the high-temperature fiber filter tube prepared in Example 1 has also greater displacement at 60N, and greater tensile force and displacement at break than those in Comparative Example 2, indicating that omitting the addition of metal oxides in the composite binder also has a certain effect on the toughness of the high-temperature fiber filter tube.

Claims

1. A method for preparing a high-temperature fiber filter tube, characterized in that: The preparation method comprises preparing a fiber web, winding and forming, and drying; the winding method comprises winding and forming the fiber web on a vacuum mold, and during the forming process, spraying a water dispersion of a composite binder on the fiber web to apply glue, and at the same time, the vacuum mold is sucked to form a high-temperature filter tube blank; The aqueous dispersion of the composite binder includes the following components by weight percentage: 24-26wt% silica sol, 9-11wt% boric acid; 2.6-3.2wt% cellulose, 0.8-1.2wt% corn starch; 2.7-3.3wt% alpha alumina, 0.8-1.2wt% zirconium oxide, 0.7-1.3wt% small-particle magnesium oxide, and water makes up 100%; The mass ratio of the fiber web to the composite binder is 3:1.5-1.7; The angle and speed of winding the fiber web on the vacuum mold are set as follows: the winding angle is 67-73°; when starting to form, the winding speed is controlled to 72-77 r / min; when the wall thickness is 2 / 3, the winding speed is adjusted to 48-52 r / min; The method for preparing the fiber web comprises selecting high-aluminum aluminum silicate fiber cotton with a diameter of 3-5 μm, and obtaining a fiber web with a thickness of 4±0.5 mm through opening and combing.

2. The method for preparing a high temperature fiber filter tube according to claim 1, characterized in that: The particle size of the α-alumina is 0.7 μm; the particle size of the zirconium oxide is 1 μm; and the particle size of the small-particle magnesium oxide is 1 μm.

3. The method for preparing a high temperature fiber filter tube according to claim 1, characterized in that: The vacuum mold is sucked at a pressure of 0.18-0.22 MPa.

4. The method for preparing a high temperature fiber filter tube according to claim 1, characterized in that: The high-aluminum aluminum silicate fiber cotton has an aluminum content of 52-55wt% and an aluminum-silicon content of ≥99wt%.

5. The method for preparing a high temperature fiber filter tube according to claim 1, characterized in that: The drying method comprises heating the high-temperature filter tube blank from room temperature to 77-81°C within 0.7-1.2 hours, then heating to 98-103°C within 1.8-2.2 hours, keeping the temperature for 1.8-2.2 hours, then heating to 118-123°C within 0.7-1.2 hours, keeping the temperature for 1-2 hours, and obtaining the high-temperature fiber filter tube.

6. A high temperature fiber filter tube, characterized in that: The high-temperature fiber filter tube is prepared by the preparation method described in any one of claims 1-5.

Citation Information

Patent Citations

  • Winding preparation method of high-porosity porous ceramic pipe

    CN106565258A

  • High-temperature dust removal filter tube and preparation method thereof

    CN108892532A

  • Dust removal and denitration integrated ceramic filtering material as well as preparation method and application thereof

    CN116036729A

  • Ceramic filter element and its manufacture

    JP2001046818A