A garnet-type composite solid electrolyte and its preparation method and application
By depositing a rare earth nickel coating with perovskite structure on the surface of garnet solid electrolytes, the problem of lithium dendrites and interface reactions in lithium-ion batteries is solved, the stability and performance of the battery are improved, and lithium metal is realized safe contact.
Patent Information
- Application Number
- CN202411103260.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Garnet-type solid electrolytes are prone to lithium carbonate impurities in lithium-ion batteries, resulting in poor contact between positive and negative electrodes, hindering ions and electron conduction, and lithium metal contacts with solid electrolytes and easily forms lithium dendrites, causing short circuits in the battery.
Pulse laser deposition technology is used to deposit a rare earth nickelate coating with perovskite structure on the surface of garnet solid electrolytes, inhibiting the negative electrode interface reduction reaction and avoiding the formation of lithium dendrites.
It effectively improves the stability of the negative electrode interface, avoids the formation of lithium dendrites, improves the electronic conductivity of the electrolyte and the negative electrode interface, allows the direct use of lithium metal, and enhances the performance and safety of all-solid-state lithium batteries.
Smart Images

Figure CN118676424B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solid electrolytes, and in particular relates to a garnet-type composite solid electrolyte and a preparation method and application thereof. Background Art
[0002] The use of solid electrolytes to replace liquid electrolytes has great prospects such as high safety and high energy density, and is an inevitable development direction in the field of energy storage. Garnet-type solid electrolytes have great development prospects due to their high room temperature ionic conductivity, wide electrochemical window and high mechanical strength. However, garnet-type solid electrolytes still face many practical problems that need to be solved, such as the easy generation of impurities such as lithium carbonate, rigid contact with the positive and negative electrodes resulting in poor physical contact, which will hinder the conduction of ions and electrons, and side reactions at the interface, etc., which are easy to generate lithium dendrites and cause battery short circuits.
[0003] Lithium metal has a high theoretical specific capacity and is the holy grail of lithium-ion batteries. However, directly using lithium metal as the negative electrode in contact with a solid electrolyte can easily form lithium dendrites, leading to battery short circuits. Summary of the invention
[0004] The purpose of the present invention is to provide a garnet-type composite solid electrolyte and a preparation method and application thereof in view of the problems existing in the prior art.
[0005] The present invention adopts pulsed laser deposition technology to deposit rare earth nickelates with a perovskite structure on the garnet solid electrolyte / Li interface, effectively inhibiting the occurrence of reduction reaction at the negative electrode interface, avoiding the formation and growth of lithium dendrites, and providing a material basis for the commercial development of all-solid-state lithium batteries.
[0006] The purpose of the present invention can be achieved by the following scheme:
[0007] The invention provides a garnet type composite solid electrolyte, comprising a garnet type solid electrolyte film and a negative electrode interface layer; the negative electrode interface layer is a rare earth nickelate coating deposited on the surface of the garnet type solid electrolyte film.
[0008] The rare earth nickelate coating is deposited on one side of the surface of the garnet-type solid electrolyte film. When preparing a solid-state battery, the rare earth nickelate coating is in contact with the negative electrode. The solid-state battery is an all-solid-state lithium-ion battery, and the negative electrode is a lithium negative electrode.
[0009] As one embodiment of the present invention, the chemical formula of the garnet-type solid electrolyte is Li x A 2 (LaO 4 ) 3; Wherein, A includes one or more metals such as Al, Fe, Ga, Zr, Ta, Sc, etc., x>0, preferably 7>x>6.
[0010] As one embodiment of the present invention, the chemical formula of rare earth nickelate is RNiO 3 ; R is one of the rare earth metals other than La, including one of Nd, Sm, and Sr. The rare earth nickelate of the present invention is a rare earth nickelate with a perovskite structure. The rare earth nickelate is preferably SmNiO 3 .
[0011] LaNiO 3 Under the action of an electric field, no phase change occurs, and the reduction reaction of the interface during lithium ion transmission cannot be suppressed, so La is not applicable to the present invention. Other rare earth acid salts (rare earth silicates, rare earth niobates, rare earth tantalates, rare earth zirconates, etc.) also cannot undergo phase change under the action of an electric field, and cannot be used in the present invention.
[0012] As one embodiment of the present invention, the thickness of the garnet-type solid electrolyte film is 50-500 μm.
[0013] As one embodiment of the present invention, the thickness of the rare earth nickelate coating is 5-150 nm.
[0014] The present invention provides a method for preparing a garnet-type composite solid electrolyte, the preparation method comprising the following steps:
[0015] S1, pressing a garnet-type solid electrolyte into a sheet, and sintering to obtain a garnet-type solid electrolyte film;
[0016] S2. Using pulsed laser deposition technology, a rare earth nickelate coating is deposited on the surface of the obtained garnet-type solid electrolyte film to obtain the garnet-type solid electrolyte.
[0017] As an implementation method of the present invention, in step S1, the sintering temperature ranges from 350 to 500° C. and the sintering time ranges from 4 hours to 24 hours.
[0018] As an implementation method of the present invention, in step S2, the target material used in the pulsed laser deposition technology is RNiO 3 ; R is one of the rare earth metals other than La, including one of Nd, Sm, and Sr.
[0019] As an implementation method of the present invention, in step S1, in the pulse laser deposition technology, the oxygen partial pressure ranges from 1 to 40 Pa; the deposition temperature ranges from 300 to 600° C. Sol-gel and other technologies can also synthesize rare earth nickelates, but such methods use solvents, which reduce the ionic conductivity of the electrolyte (the solvent reacts with the electrolyte, and the generated impurities reduce its ionic conductivity), inhibiting lithium ion transmission.
[0020] The present invention provides a method for modifying the interface of a negative electrode based on a garnet-type solid electrolyte, comprising the following steps:
[0021] A1, pressing a garnet-type solid electrolyte into a sheet, and sintering to obtain a garnet-type solid electrolyte film;
[0022] A2. A rare earth nickelate coating is deposited on the surface of the obtained garnet-type solid electrolyte film using pulsed laser deposition technology. When preparing an all-solid-state battery, one side of the rare earth nickelate coating is assembled with the negative electrode.
[0023] The present invention also provides an all-solid-state battery, comprising the garnet-type composite solid electrolyte negative electrode. When preparing the all-solid-state battery, one side of the rare earth nickelate coating is assembled with the negative electrode.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) Garnet-type solid electrolytes are prone to generate impurities such as lithium carbonate, and the rigid contact with the positive and negative electrodes leads to poor physical contact, which hinders the conduction of ions and electrons. There are also side reactions at the interface between the positive and negative electrodes, and lithium metal cannot be used as the negative electrode to directly contact the solid electrolyte. The present invention coats the garnet-type solid electrolyte film with a rare earth nickelate with a perovskite structure, effectively inhibiting the occurrence of reduction reactions at the negative electrode interface and avoiding the formation and growth of lithium dendrites.
[0026] (2) The electronic conductivity of rare earth nickelate materials with perovskite structure will decrease under low voltage conditions, but can be reversibly reduced to the original conductivity under high voltage. Therefore, during the discharge process, the electronic conductivity of the electrolyte and the negative electrode interface will decrease, the electrolyte will not undergo reduction reaction, and side reactions at the negative electrode interface will not occur. It can directly contact with lithium metal, thereby improving the stability of the negative electrode interface.
[0027] (3) Rare earth nickelate coatings can inhibit the occurrence of side reactions caused by low-pressure reduction of electrolytes; improve the stability of the negative electrode / electrolyte interface; and allow the direct use of lithium metal, avoiding the formation and growth of lithium dendrites. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0029] Figure 1 The first charge and discharge curves of the sulfide all-solid-state batteries prepared in Example 1 and Comparative Examples 1 and 2.
[0030] Figure 2 The cyclic stability curves of the sulfide all-solid-state batteries prepared in Example 2 and Comparative Example 3 at 2C rate.
[0031] Figure 3 The first cycle charge and discharge curves of the sulfide all-solid-state batteries prepared in Example 2 and Comparative Examples 4 and 5 at a rate of 0.1C. DETAILED DESCRIPTION
[0032] The present invention is described in detail below in conjunction with specific embodiments. The following examples are implemented under the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, which will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.
[0033] Example 1
[0034] 1) Weigh 20 mg Li 7 La 3 Zr 2 O 12 Solid electrolyte powder, using a 10mm tableting die to press the electrolyte into tablets at 400MPa, and calcined in a muffle furnace at 500°C for 4h to obtain a solid electrolyte film with a thickness of 100μm;
[0035] 2) Pulsed laser deposition equipment is used, and the target material is SmNiO 3 The substrate is the solid electrolyte film prepared in step 1), and the target material is deposited onto the substrate by pulse laser at an oxygen partial pressure of 30 Pa and a temperature of 400° C. to a thickness of 100 nm, cooled to room temperature, and taken out;
[0036] 3) In a glove box filled with argon, weigh 75 mg NCM811 and 22 mg Li 7 La 3 Zr 2 O 12 The electrolyte powder and 3 mg VGCF powder were placed in a mortar and ground for 30 min until the powders were evenly mixed to obtain a composite positive electrode material for use.
[0037] 4) Assembling a pressure battery: In an argon-filled glove box, weigh 40 mg of the composite positive electrode material prepared in step 3) and place it in a pressure battery mold with a diameter of 10 mm. The composite positive electrode material is rotated and flattened by rotating the stainless steel column, and pressed into sheets on a tablet press at a pressure of 120 MPa for 2 minutes. The deposited electrolyte film prepared in step 2) (the direction without deposition coating faces the positive electrode) and the electrolyte surface with deposition coating are placed with 9 mm diameter lithium metal, and the current collector is Cu foil. After assembly, a pressure of 50 MPa is applied to obtain an all-solid-state lithium-ion battery.
[0038] Example 2
[0039] 1) Weigh 20 mg Li 6.3 La 3 Zr 1.4 Ta 0.6 O 12 Solid electrolyte powder, using a 10mm tableting die to press the electrolyte into tablets at 400MPa, and calcined in a muffle furnace at 500°C for 4h to obtain a solid electrolyte film with a thickness of 100μm;
[0040] 2) Pulsed laser deposition equipment is used, and the target material is NdNiO 3 The powder is the solid electrolyte film prepared in step 1) and is deposited on the bottom by using a pulsed laser at an oxygen partial pressure of 25 Pa and a temperature of 550°C to deposit the target material to a thickness of 100 nm, cooled to room temperature, and taken out;
[0041] 3) In a glove box filled with argon, weigh 70 mg NCM811 and 28 mg Li 6.3 La 3 Zr 1.4 Ta 0.6 O 12 The electrolyte powder and 2 mg VGCF powder were placed in a mortar and ground for 30 min until the powders were evenly mixed to obtain a composite positive electrode material for use.
[0042] 4) Assembling a pressure battery: In an argon-filled glove box, weigh 30 mg of the composite positive electrode material prepared in step 3) and place it in a pressure battery mold with a diameter of 10 mm. The composite positive electrode material is rotated and flattened by rotating the stainless steel column, and pressed into sheets on a tablet press at a pressure of 120 MPa for 2 minutes. The deposited electrolyte film prepared in step 2) (the direction without deposition coating faces the positive electrode) and the electrolyte surface with deposition coating are placed with 9 mm diameter lithium metal, and the current collector is Cu foil. After assembly, a pressure of 50 MPa is applied to obtain an all-solid-state lithium-ion battery.
[0043] Comparative Example 1
[0044] The difference from Example 1 is that the electrolyte is not subjected to pulsed laser deposition coating treatment, and the pressure battery solid electrolyte directly uses the electrolyte film of step 1) in Example 1.
[0045] Comparative Example 2
[0046] The difference from Example 1 is that the negative electrode interface layer obtained by pulsed laser deposition is a lithium nickelate coating.
[0047] Comparative Example 3
[0048] The difference from Example 2 is that the negative electrode interface layer obtained by pulsed laser deposition is a lanthanum nickelate coating.
[0049] Comparative Example 4
[0050] The difference from Example 2 is that the negative electrode interface layer obtained by pulsed laser deposition is a lithium silicate coating.
[0051] Comparative Example 5
[0052] The difference from Example 2 is that the negative electrode interface layer obtained by pulsed laser deposition is Nd(NO 3 ) 3 coating.
[0053] Performance Testing
[0054] The Xinwei battery testing system, equipment model: CT-4000, was used to test the all-solid-state battery. The 0.1C / 0.1C charge and discharge process was used to test the first charge and discharge capacity of the solid-state lithium battery. The first efficiency % = first discharge capacity / first charge capacity × 100%. Figure 1 The first charge and discharge curves of the sulfide all-solid-state batteries prepared in Example 1 and Comparative Examples 1 and 2. The first charge and discharge efficiency of Example 1 is 84.22%, and the charge and discharge specific capacities are 218.87mAh / g and 195.08mAh / g, respectively; the first charge and discharge efficiency of Comparative Example 1 is 80.80%, and the charge and discharge specific capacities are 218.87mAh / g and 176.85mAh / g, respectively. The first charge and discharge efficiency of Comparative Example 2 is 59.03%, and the charge and discharge specific capacities are 88.12mAh / g and 52.01mAh / g, respectively.
[0055] The Xinwei battery testing system, equipment model: CT-4000, is also used to test the all-solid-state battery, using a 2C / 2C charge and discharge process to test the capacity retention rate at the 50th cycle. Figure 2 The cyclic stability curves at 2C rate of the sulfide all-solid-state batteries prepared in Example 2 and Comparative Example 3. After 50 cycles of charge and discharge, the capacity retention rate of Example 1 is 93.7%, and the capacity retention rate of Comparative Example 1 is 82.66%.
[0056] Figure 3 The first charge and discharge curves of the sulfide all-solid-state batteries prepared in Example 2, Comparative Examples 4 and 5 at a rate of 0.1C. The first charge and discharge efficiency of Example 2 is 80.28%, and the charge and discharge specific capacities are 256.70mAh / g and 206.08mAh / g, respectively. The first charge and discharge efficiency of Comparative Example 3 is 63.76%, and the charge and discharge specific capacities are 252.68mAh / g and 161.10mAh / g, respectively. The first charge and discharge efficiency of Comparative Example 4 is 57.31%, and the charge and discharge specific capacities are 251.32mAh / g and 144.02mAh / g, respectively.
[0057] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A garnet-type composite solid electrolyte, characterized in that: The garnet-type composite solid electrolyte comprises a garnet-type solid electrolyte film and a negative electrode interface layer; The negative electrode interface layer is a rare earth nickelate coating deposited on the surface of the garnet-type solid electrolyte film; In the garnet-type solid electrolyte film, the chemical formula of the garnet-type solid electrolyte is Li x A2(LaO4)3; wherein A includes one or more metals selected from the group consisting of Al, Fe, Ga, Zr, Ta, and Sc, and x>0; The general chemical formula of rare earth nickelates is RNiO3; R is one of the rare earth metals except La.
2. The garnet-type composite solid electrolyte according to claim 1, characterized in that: The thickness of the garnet-type solid electrolyte film is 50-500 μm; And / or, the rare earth nickelate coating has a thickness of 5-150 nm.
3. A method for preparing the garnet-type composite solid electrolyte according to claim 1, characterized in that: The preparation method comprises the following steps: S1, pressing a garnet-type solid electrolyte into a sheet, and sintering to obtain a garnet-type solid electrolyte film; S2. Using pulsed laser deposition technology, a rare earth nickelate coating is deposited on the surface of the obtained garnet-type solid electrolyte film to obtain the garnet-type composite solid electrolyte.
4. The method for preparing the garnet-type composite solid electrolyte according to claim 3, characterized in that: In step S1, the sintering temperature is 350-500°C and the sintering time is 4-24 hours.
5. The method for preparing the garnet-type composite solid electrolyte according to claim 3, characterized in that: In step S2, in the pulse laser deposition technology, the target material used is RNiO3; R is one of the rare earth metals except La.
6. The method for preparing the garnet-type composite solid electrolyte according to claim 3, characterized in that: In step S2, in the pulse laser deposition technology, the oxygen partial pressure is 1-40 Pa; and the deposition temperature is 300-600°C.
7. An all-solid-state battery, characterized in that: It comprises the garnet-type composite solid electrolyte as claimed in claim 1.