A composite antibacterial agent with preservation function and its preparation method

CN118680210A8Inactive Publication Date: 2024-11-22GUANGZHOU YIPINXIAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410785604.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing antibacterial agents in food packaging have poor heat resistance, are easily oxidized, easy to decompose, are highly toxic, and have potential harm to the environment and human body, which limits their application in food packaging. In particular, transparent packaging is difficult to meet the demand for freshness.

Method used

The preparation method of composite antibacterial agents is adopted, including sodium dehydroacetate, sorbic acid, parahydroxybenzoic acid and its esters, calcium acetate, calcium propionate, titanium dioxide, chitosan and other antibacterial agents, combined with vinyltrimethoxysilane, ethylene triethoxy Silane, aluminate coupling agent, liquid paraffin, surfactant, silica gel and other materials are used to prepare nano-scale composite antibacterial agents through high-pressure nozzles, homogenizers, sand mills and nano-scale spray drying technology to enhance their stability. and compatibility.

Benefits of technology

It achieves a broad antibacterial spectrum and prolongs the duration of effect, reduces the loss rate of fruits and vegetables in the production and circulation process, prolongs the preservation time of fruits and vegetables, improves the shelf life, and regulates oxygen and carbon dioxide concentrations through microporous air-controlled materials. It delays the aging of fruits and vegetables and significantly improves the antibacterial effect and organic gas adsorption capacity of packaging products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118680210A8_ABST
    Figure CN118680210A8_ABST
Patent Text Reader

Abstract

The invention discloses a composite antibacterial agent with a preservation function, which comprises the following components by weight: 5-80 parts of antibacterial agent; 0.3-2 parts of coupling agent; 0.3-2 parts of liquid paraffin; 0.3-1 parts of surfactant; 3-5 parts of polyethylene oxide; 1-20 parts of organic gas adsorption material; 1-20 parts of microporous gas conditioning material; 10-60 parts of ultrapure water; 0.1-0.5 parts of anhydrous ethanol. The antibacterial agent is at least one or more of sodium dehydroacetate, sorbic acid, methyl paraben, propyl paraben, calcium acetate, calcium propionate, titanium dioxide, and chitosan. The composite antibacterial agent with a preservation function of the invention has a wide antibacterial spectrum and a long lasting effect. Adding it to packaging materials can reduce the loss rate of fruits and vegetables in the production and circulation links, and extend the preservation time and shelf life of fruits and vegetables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of food preservation, in particular to a composite antibacterial agent with a preservation function and a preparation method thereof. Background Art

[0002] Antibacterial materials are mainly divided into three categories: natural antibacterial materials, organic antibacterial materials and inorganic antibacterial materials. Natural antibacterial materials are generally extracted directly from animals and plants and refined. They generally have good antibacterial effects and less harm to the environment and human body. However, when they are used in food packaging, especially for transparent food packaging, their heat resistance is very poor. Generally, they begin to carbonize and decompose below 150°C, causing transparent food packaging to turn yellow or even produce large crystal points. The application range is narrow and they are not very suitable for food packaging at the current stage. Organic antibacterial materials generally have strong bactericidal ability, such as imidazoles, quaterniums, and phenols. Due to their poor safety, they are rarely used in food packaging, and are generally used in pesticide products. Due to their poor chemical stability, poor heat resistance, easy oxidation, and easy decomposition, they are generally not used in food packaging, especially for transparent food packaging, which generally produces dense crystal points. Although some literature or patents have confirmed their excellent antibacterial effects through antibacterial circle tests, or added them into polyethylene to blow out films, they often ignore that their aesthetic effect is also very important for packaging. Dense and tiny crystal points will directly reduce consumers' desire to buy. Inorganic antibacterial agents are generally used in food packaging. Silver ion antibacterial agents are currently used more, but they are difficult to preserve, have poor sustained release and are not durable, are easily oxidized and blackened, and are easy to agglomerate. They are highly toxic. At present, European and American countries have basically introduced restrictions and prohibitions on the use of silver ion antibacterial agents in food packaging. Therefore, it is necessary to provide a composite antibacterial agent with a fresh-keeping function and a preparation method thereof. Summary of the invention

[0003] In order to overcome the defects in the prior art, a composite antibacterial agent with a fresh-keeping function and a preparation method thereof are provided.

[0004] The present invention is achieved through the following scheme:

[0005] A composite antibacterial agent with a preservation function, the composite antibacterial agent comprises the following components in parts by mass:

[0006]

[0007] The antibacterial agent is at least one or more of sodium dehydroacetate, sorbic acid, methyl parahydroxybenzoate, propyl parahydroxybenzoate, calcium acetate, calcium propionate, titanium dioxide and chitosan.

[0008] The coupling agent is one or more of vinyl trimethoxy silane, vinyl triethoxy silane, vinyl triacetoxy silane and aluminate coupling agent.

[0009] The liquid paraffin is food grade liquid paraffin.

[0010] The surfactant is at least one or more of poloxamer, glyceryl monostearate, stearyl erucamide, glyceryl laurate, and polyethylene glycol stearate.

[0011] The organic gas adsorption material is at least one or more of silica gel, molecular sieve, alumina, calcium aluminum silicate, potassium aluminum silicate, and sodium aluminum silicate.

[0012] The microporous gas-conditioning material is at least one or more of microporous glass beads, silicon dioxide, bentonite, feldspar, cristobalite, and hydrotalcite.

[0013] The concentration of the anhydrous ethanol is above 99.5%.

[0014] A method for preparing a composite antibacterial agent with a fresh-keeping function, the method comprising the following steps:

[0015] S1. In a reaction vessel, dilute the coupling agent in liquid paraffin and stir evenly to obtain a diluted coupling agent;

[0016] S2. In a high-speed mixer, an antibacterial agent, an organic gas adsorption material, a microporous gas conditioning material, and anhydrous ethanol were added, and the mixture was dispersed by high-speed stirring at a speed of 50-3800r / min, and the diluted coupling agent was sprayed into the mixture in 5 batches during the stirring process through a high-pressure nozzle to obtain a composite antibacterial agent;

[0017] S3. In a homogenizer, add the composite antibacterial agent obtained in step S2, a surfactant, and ultrapure water, and homogenize at 30-120MPa for 30-180min to obtain a micron-sized composite antibacterial agent solution;

[0018] S4. The micron-grade composite antibacterial agent solution obtained in step S3 above is added to a submicron sand mill and dispersed by sand milling at a speed of 300-4200 r / min for 0.5-12 h to obtain a submicron-grade composite antibacterial agent solution of 0.5-0.8 um;

[0019] S5. The submicron composite antibacterial agent solution obtained in step S4 is added to a nano-scale sand mill, polyethylene oxide is added, and a surfactant is added in three batches, and the dispersion is sand-milled at a speed of 600-3800 r / min for 0.5-12 h to obtain a 0.1-100 nm composite antibacterial agent solution having a preservation function;

[0020] S6. The 0.1-100 nm composite antibacterial agent solution having a preservative function obtained in S5 was stirred in a reactor at a speed of 50-300 r / min, and the diluted coupling agent was added in 3 batches, and the reaction was carried out at a temperature of 50°C-80°C for 6h-24h to obtain a composite antibacterial agent solution having a preservative function;

[0021] S7. The composite antimicrobial agent having a preservative function obtained in step S6 is filtered and separated through an ultrafiltration membrane, and the filtrate obtained is a composite antimicrobial agent filtrate having a preservative function that meets the process standards;

[0022] S8. The filtrate of the composite antibacterial agent with a preservation function obtained in the above step S7 is dried by a nano-scale spray dryer at a pressure of 0.1-50MPa and a temperature of 80°C-130°C to obtain a finished composite antibacterial agent with a preservation function.

[0023] The antibacterial agent is at least one or more of sodium dehydroacetate, sorbic acid, methyl parahydroxybenzoate, propyl parahydroxybenzoate, calcium acetate, calcium propionate, titanium dioxide, and chitosan;

[0024] The coupling agent is one or more of vinyl trimethoxy silane, vinyl triethoxy silane, vinyl triacetoxy silane, and aluminate coupling agent;

[0025] The liquid paraffin is food grade liquid paraffin;

[0026] The surfactant is at least one or more of poloxamer, glyceryl monostearate, stearyl erucamide, glyceryl laurate, and polyethylene glycol stearate;

[0027] The organic gas adsorption material is at least one or more of silica gel, molecular sieve, alumina, calcium aluminum silicate, potassium aluminum silicate, and sodium aluminum silicate;

[0028] The microporous gas conditioning material is at least one or more of microporous glass beads, silica, bentonite, feldspar, cristobalite, and hydrotalcite;

[0029] The concentration of the anhydrous ethanol is above 99.5%.

[0030] The beneficial effects of the present invention are:

[0031] 1. The composite antibacterial agent with a preservation function of the present invention has a broad antibacterial spectrum and a long lasting effect. When added into packaging materials, it can reduce the loss rate of fruits and vegetables in the production and circulation links, and extend the preservation time and shelf life of fruits and vegetables.

[0032] 2. The present invention grinds the composite antibacterial agent together with a low-viscosity elastomer and a surfactant in sections, so that the composite antibacterial agent is ground into nanometer scale and obtains nanometer-scale stable dispersion in the monomer. After the surface of the antibacterial agent is modified by a surfactant, it is embedded in the monomer to enhance the compatibility with the resin in subsequent processes. When added into the packaging products, there is no crystal point phenomenon on the surface of the packaging products, and the antibacterial time is longer.

[0033] 3. The composite antibacterial agent with a fresh-keeping function prepared by the present invention can be mixed with different resins according to different packaging plastic systems to produce fruit and vegetable packaging products. It has a broad-spectrum antibacterial effect, and has a strong inhibitory effect on bacterial activity and mildew prevention; it has the ability to adsorb organic gases produced by the respiration of fruits and vegetables, prolong the fresh-keeping time of fruits and vegetables, increase their shelf life, and delay the occurrence of aging of fruits and vegetables; after being made into a sealed packaging material, in the link of fruit and vegetable transportation, especially in the decooling of fruits and vegetables from the cold chain, the microporous gas conditioning material in the present invention can effectively adjust the content of oxygen and carbon dioxide concentrations, so that fruits and vegetables are still in a state of low aerobic respiration, thereby prolonging the shelf life. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a schematic diagram of the preservation effect of the actual application of the composite antibacterial agent with preservation function. DETAILED DESCRIPTION

[0035] The preferred embodiments of the present invention are further described below in conjunction with specific embodiments:

[0036] Example 1

[0037] S1. In a reaction vessel, 0.8 parts of vinyl trimethoxysilane was diluted in 2.2 parts of liquid paraffin and stirred to obtain a diluted coupling agent;

[0038] S2. In a high-speed mixer, 5 parts of sodium dehydroacetate, 5 parts of sorbic acid, 15 parts of calcium propionate, 5 parts of titanium dioxide, 20 parts of silica gel, 15 parts of molecular sieves, 15 parts of sodium aluminum silicate, 5 parts of silicon dioxide, 10 parts of bentonite, 5 parts of cristobalite, 0.5 parts of anhydrous ethanol were added, and dispersed under high-speed stirring at 50-3800r / min, and 1.5 parts of the diluted coupling agent were sprayed into 5 batches during stirring by a high-pressure nozzle to obtain a composite antibacterial agent;

[0039] S3. In a homogenizer, 100 parts of the composite antibacterial agent obtained in step S2, 0.3 parts of poloxamer, 0.2 parts of lauric acid glyceryl, and 60 parts of ultrapure water were added, and homogenized at 30-120MPa for 30-180min to obtain a micron-sized composite antibacterial agent solution;

[0040] S4. The micron-grade composite antibacterial agent solution obtained in step S3 above is added to a submicron sand mill and dispersed by sand milling at a speed of 300-4200 r / min for 0.5-12 h to obtain a submicron-grade composite antibacterial agent solution of 0.5-0.8 um;

[0041] S5. The submicron composite antibacterial agent solution obtained in step S4 above is added to a nano-scale sand mill, 5 parts of polyethylene oxide, 0.1 parts of lauric acid glyceryl, 0.4 parts of polyethylene glycol stearate are added, and the dispersion is sand-milled at a speed of 600-3800r / min for 0.5-12h to obtain a composite antibacterial agent solution of 0.1-100nm having a preservation function;

[0042] S6. The 0.1-100 nm composite antibacterial agent solution having a preservative function obtained in S5 was stirred in a reactor at a speed of 50-300 r / min, 1.5 parts of the diluted coupling agent were added in 3 batches, and the reaction was carried out at a temperature of 50°C-80°C for 6h-24h to obtain a composite antibacterial agent solution having a preservative function;

[0043] S7. The composite antimicrobial agent having a preservative function obtained in step S6 is filtered and separated through an ultrafiltration membrane, and the filtrate obtained is a composite antimicrobial agent filtrate having a preservative function that meets the process standards;

[0044] S8. The filtrate of the composite antibacterial agent having a preservation function obtained in step S7 is dried by a nano-scale spray dryer at a pressure of 0.1-50MPa and a temperature of 80°C-130°C to obtain a composite antibacterial agent having a preservation function, and its antibacterial rate is tested;

[0045] S9. The composite antimicrobial agent with a fresh-keeping function obtained in S8 is granulated and blown to obtain a packaging film, and then bagged to obtain a fresh-keeping packaging bag, and its performance is tested.

[0046] Example 2

[0047] S1. In a reaction vessel, 0.8 parts of vinyl triethoxysilane was diluted in 2.2 parts of liquid paraffin and stirred to obtain a diluted coupling agent;

[0048] S2. In a high-speed mixer, 5 parts of Kathon, 5 parts of propyl paraben, 15 parts of calcium acetate, 5 parts of chitosan, 20 parts of silica gel, 15 parts of molecular sieves, 15 parts of sodium aluminum silicate, 5 parts of silicon dioxide, 10 parts of bentonite, 5 parts of cristobalite, 0.5 parts of anhydrous ethanol were added, and the mixture was dispersed under high-speed stirring at 50-3800r / min, and 1.5 parts of the diluted coupling agent were sprayed into 5 batches during stirring by a high-pressure nozzle to obtain a composite antibacterial agent;

[0049] S3. In a homogenizer, 100 parts of the composite antibacterial agent obtained in step S2, 0.3 parts of poloxamer, 0.2 parts of lauric acid glyceryl, and 60 parts of ultrapure water were added, and homogenized at 30-120MPa for 30-180min to obtain a micron-sized composite antibacterial agent solution;

[0050] S4. The micron-grade composite antibacterial agent solution obtained in step S3 above is added to a submicron sand mill and dispersed by sand milling at a speed of 300-4200 r / min for 0.5-12 h to obtain a submicron-grade composite antibacterial agent solution of 0.5-0.8 um;

[0051] S5. The submicron composite antibacterial agent solution obtained in step S4 above is added to a nano-scale sand mill, 5 parts of polyethylene oxide, 0.1 parts of lauric acid glyceryl, 0.4 parts of polyethylene glycol stearate are added, and the dispersion is sand-milled at a speed of 600-3800r / min for 0.5-12h to obtain a composite antibacterial agent solution of 0.1-100nm having a preservation function;

[0052] S6. The 0.1-100 nm composite antibacterial agent solution having a preservative function obtained in S5 was stirred in a reactor at a speed of 50-300 r / min, 1.5 parts of the diluted coupling agent were added in 3 batches, and the reaction was carried out at a temperature of 50°C-80°C for 6h-24h to obtain a composite antibacterial agent solution having a preservative function;

[0053] S7. The composite antimicrobial agent having a preservative function obtained in step S6 is filtered and separated through an ultrafiltration membrane, and the filtrate obtained is a composite antimicrobial agent filtrate having a preservative function that meets the process standards;

[0054] S8. The filtrate of the composite antibacterial agent having a preservation function obtained in step S7 is dried by a nano-scale spray dryer at a pressure of 0.1-50MPa and a temperature of 80°C-130°C to obtain a composite antibacterial agent having a preservation function and test its antibacterial rate;

[0055] S9. The composite antimicrobial agent with a fresh-keeping function obtained in S8 is granulated and blown to obtain a packaging film, and then bagged to obtain a fresh-keeping packaging bag, and its performance is tested.

[0056] Comparative Example 1

[0057] S1. In a reaction vessel, 0.8 parts of vinyl trimethoxysilane was diluted in 2.2 parts of liquid paraffin and stirred to obtain a diluted coupling agent;

[0058] S2. In a high-speed mixer, 5 parts of sodium dehydroacetate, 5 parts of sorbic acid, 15 parts of calcium propionate, 5 parts of titanium dioxide, and 0.5 parts of anhydrous ethanol were added, and dispersed by high-speed stirring at a speed of 50-3800r / min, and 1.5 parts of the diluted coupling agent were sprayed into 5 batches during the stirring process through a high-pressure nozzle to obtain a composite antibacterial agent, and its antibacterial rate was measured;

[0059] S3. The composite antibacterial agent with a preservation function obtained in S2 is granulated and blown to obtain a packaging film, and then bagged to obtain a packaging bag, and its performance is tested.

[0060] Comparative Example 2

[0061] S1. In a reaction vessel, 0.8 parts of vinyl triethoxysilane was diluted in 2.2 parts of liquid paraffin and stirred to obtain a diluted coupling agent;

[0062] S2. In a high-speed mixer, 5 parts of Kathon, 5 parts of propyl paraben, 15 parts of calcium acetate, 5 parts of chitosan, 20 parts of silica gel, 15 parts of molecular sieves, 15 parts of sodium aluminum silicate, 5 parts of silicon dioxide, 10 parts of bentonite, 5 parts of cristobalite, and 0.5 parts of anhydrous ethanol were added, and dispersed at a high speed of 50-3800r / min, and 1.5 parts of the diluted coupling agent were sprayed into 5 batches during the stirring process through a high-pressure nozzle to obtain a composite antibacterial agent, and its antibacterial rate was tested;

[0063] S3. The composite antibacterial agent with a preservation function obtained in S2 is granulated and blown to obtain a packaging film, and then bagged to obtain a packaging bag, and its performance is tested.

[0064] The particle size of the composite antimicrobial agent with a preservation function in Example 1 was measured using Malvern Mastersizer 3000 laser particle size analyzer LPSA. The average value of the measurement is shown in Table 1.

[0065] Table 1 Average results of particle size detection of composite antimicrobial agents with preservation function

[0066]

[0067]

[0068] According to the particle size test results, the particle size of the composite antibacterial agent with a preservation function is within 1-200nm, among which Dv(50) is 32.3nm and Dv(90) is 76.8nm, that is, the main particle size distribution of the composite antibacterial agent with a preservation function is within 0.1-100nm.

[0069] The antibacterial properties of the composite antibacterial agents obtained in Example 1, Example 2, Comparative Example 1 and Comparative Example 2 were tested according to GB / T31402-2015. Each case was tested 10 times to obtain the average value. The test results are shown in Table 2.

[0070] Table 2 Antibacterial effect of composite antibacterial agent

[0071] Test items Example 1 Example 2 Comparative Example 1 Comparative Example 2 Antibacterial rate of Staphylococcus aureus / % 99.99 99.99 99.99 99.99 Escherichia coli antibacterial rate / % 99.99 99.99 99.99 99.99

[0072] The antibacterial properties of the packaging bags obtained in Example 1, Example 2, Comparative Example 1 and Comparative Example 2 were tested according to GB / T31402-2015. Each case was tested 10 times to obtain the average value. The test results are shown in Table 3.

[0073] Table 3 Antibacterial effect of packaging bags

[0074] Test items Example 1 Example 2 Comparative Example 1 Comparative Example 2 Antibacterial rate of Staphylococcus aureus / % 99.99 99.99 23.56 24.23 Escherichia coli antibacterial rate / % 99.99 99.99 25.79 24.98

[0075] According to the comparison of Table 2 and Table 3 above, it can be seen that the antibacterial test results of a simple antibacterial agent have no guiding role for the actual packaging products produced, and on the contrary may form wrong guidance. It is easy to meet the standard for antibacterial testing of a simple antibacterial agent, but in real life, the final packaging material is the material that actually contacts the food, and only the antibacterial effect of the packaging obtained by testing the antibacterial agent has a practical guiding role. By comparing the antibacterial effects of the packaging bags of Example 1, Example 2 and Comparative Example 1, Comparative Example 2, it can be seen that when the composite antibacterial agent is ground and dispersed with the elastomer, and then its surface is modified by a surfactant to enhance the antibacterial activity, the prepared composite antibacterial agent with a fresh-keeping function has a significantly improved antibacterial effect when it is made into a packaging product.

[0076] The organic gas adsorption rates of the packaging bags obtained in Example 1, Example 2, Comparative Example 1 and Comparative Example 2 were tested with reference to GB21551.4-2010. Each case was tested 10 times to obtain an average value. The test results are shown in Table 4.

[0077] Table 4 Organic gas adsorption rate of packaging bags

[0078] Test items Example 1 Example 2 Comparative Example 1 Comparative Example 2 Organic gas adsorption rate / % 78.54 76.12 3.26 21.88

[0079] According to the comparison of Example 1, Example 2, Comparative Example 1 and Comparative Example 2, when the organic gas adsorption material is added, the prepared composite antibacterial agent has a significantly improved organic gas adsorption effect when made into packaging materials compared with the one without adding the organic gas adsorption material. And after the special nanomaterial production and dispersion process, the organic gas adsorption rate is stronger than that without sufficient dispersion.

[0080] Figure 1The figure is a schematic diagram of the fresh-keeping effect of the composite antimicrobial agent with a fresh-keeping function in actual application. According to the comparison of the fresh-keeping effect of fresh-keeping bags with composite antimicrobial agents added and packaging bags without composite antimicrobial agents added on Chinese cabbage, it is known that adding the composite antimicrobial agent prepared by the present invention to the fresh-keeping packaging of fruits and vegetables can spontaneously regulate the atmosphere in the packaging of fruits and vegetables, and adsorb the organic gas generated by the respiration of fruits and vegetables, thereby delaying the arrival of the aging period of fruits and vegetables and extending the fresh-keeping time of fruits and vegetables.

[0081] The present invention adopts a special nano antibacterial agent preparation method and a special nano dispersion method, so that the surface of the composite antibacterial agent with a preservation function is modified and wrapped, thereby solving the problem of difficult dispersion and easy agglomeration of nano materials. The composite antibacterial agent with a preservation function of the present invention has a broad-spectrum antibacterial effect and has a strong effect of inhibiting bacteria and preventing mildew. The composite antibacterial agent with a preservation function of the present invention is added to packaging material products, such as film packaging and pallet packaging, at a ratio of 1%-40%, so that the antibacterial effect and organic gas adsorption of the product can achieve good effects, and at the same time has the effect of spontaneous gas conditioning.

[0082] Although the technical solutions of the present invention have been described and listed in detail, it should be understood that it is obvious to those skilled in the art to make modifications to the above embodiments or adopt equivalent alternatives. These modifications or improvements made without departing from the spirit of the present invention are within the scope of protection required by the present invention.

Claims

1. A composite antibacterial agent with a preservation function, characterized in that: The composite antibacterial agent comprises the following components in parts by mass:

2. The composite antibacterial agent with a fresh-keeping function according to claim 1, characterized in that: The antibacterial agent is at least one or more of sodium dehydroacetate, sorbic acid, methyl parahydroxybenzoate, propyl parahydroxybenzoate, calcium acetate, calcium propionate, titanium dioxide and chitosan.

3. The composite antibacterial agent with a fresh-keeping function according to claim 1, characterized in that: The coupling agent is one or more of vinyl trimethoxy silane, vinyl triethoxy silane, vinyl triacetoxy silane and aluminate coupling agent.

4. The composite antibacterial agent with a fresh-keeping function according to claim 1, characterized in that: The liquid paraffin is food grade liquid paraffin.

5. The composite antibacterial agent with a freshness-preserving function according to claim 1, characterized in that: The surfactant is at least one or more of poloxamer, glyceryl monostearate, stearyl erucamide, glyceryl laurate, and polyethylene glycol stearate.

6. The composite antibacterial agent with a fresh-keeping function according to claim 1, characterized in that: The organic gas adsorption material is at least one or more of silica gel, molecular sieve, alumina, calcium aluminum silicate, potassium aluminum silicate, and sodium aluminum silicate.

7. The composite antibacterial agent with a freshness-preserving function according to claim 1, characterized in that: The microporous gas-conditioning material is at least one or more of microporous glass beads, silicon dioxide, bentonite, feldspar, cristobalite, and hydrotalcite.

8. The composite antibacterial agent with a freshness-preserving function according to claim 1, characterized in that: The concentration of the anhydrous ethanol is above 99.5%.

9. A method for preparing a composite antibacterial agent with a fresh-keeping function as claimed in any one of claims 1 to 8, characterized in that: The method comprises the following steps: S1. In a reaction vessel, dilute the coupling agent in liquid paraffin and stir evenly to obtain a diluted coupling agent; S2. In a high-speed mixer, an antibacterial agent, an organic gas adsorption material, a microporous gas conditioning material, and anhydrous ethanol were added, and the mixture was dispersed by high-speed stirring at a speed of 50-3800r / min, and the diluted coupling agent was sprayed into the mixture in 5 batches during the stirring process through a high-pressure nozzle to obtain a composite antibacterial agent; S3. In a homogenizer, add the composite antibacterial agent obtained in step S2, a surfactant, and ultrapure water, and homogenize at 30-120MPa for 30-180min to obtain a micron-sized composite antibacterial agent solution; S4. The micron-grade composite antibacterial agent solution obtained in step S3 above is added to a submicron sand mill and dispersed by sand milling at a speed of 300-4200 r / min for 0.5-12 h to obtain a submicron-grade composite antibacterial agent solution of 0.5-0.8 um; S5. The submicron composite antibacterial agent solution obtained in step S4 is added to a nano-scale sand mill, polyethylene oxide is added, and a surfactant is added in three batches, and the dispersion is sand-milled at a speed of 600-3800 r / min for 0.5-12 h to obtain a 0.1-100 nm composite antibacterial agent solution having a preservation function; S6. The 0.1-100 nm composite antibacterial agent solution having a preservative function obtained in S5 was stirred in a reactor at a speed of 50-300 r / min, and the diluted coupling agent was added in 3 batches, and the reaction was carried out at a temperature of 50°C-80°C for 6h-24h to obtain a composite antibacterial agent solution having a preservative function; S7. The composite antimicrobial agent having a preservative function obtained in step S6 is filtered and separated through an ultrafiltration membrane, and the filtrate obtained is a composite antimicrobial agent filtrate having a preservative function that meets the process standards; S8. The filtrate of the composite antibacterial agent with a preservation function obtained in the above step S7 is dried by a nano-scale spray dryer at a pressure of 0.1-50MPa and a temperature of 80°C-130°C to obtain a finished composite antibacterial agent with a preservation function.

10. The method for preparing a composite antibacterial agent with a fresh-keeping function according to claim 9, characterized in that: The antibacterial agent is at least one or more of sodium dehydroacetate, sorbic acid, methyl parahydroxybenzoate, propyl parahydroxybenzoate, calcium acetate, calcium propionate, titanium dioxide, and chitosan; The coupling agent is one or more of vinyl trimethoxy silane, vinyl triethoxy silane, vinyl triacetoxy silane, and aluminate coupling agent; The liquid paraffin is food grade liquid paraffin; The surfactant is at least one or more of poloxamer, glyceryl monostearate, stearyl erucamide, glyceryl laurate, and polyethylene glycol stearate; The organic gas adsorption material is at least one or more of silica gel, molecular sieve, alumina, calcium aluminum silicate, potassium aluminum silicate, and sodium aluminum silicate; The microporous gas conditioning material is at least one or more of microporous glass beads, silica, bentonite, feldspar, cristobalite, and hydrotalcite; The concentration of the anhydrous ethanol is above 99.5%.