A high-precision and high-strength micro-modulus gear metal powder forming process

Through the mixed feeding preparation and sintering forming process of high-strength stainless steel metal powder and POM-based binder, combined with high-strength stainless steel sintering plate, the problem of insufficient precision of small module gears and powder injection molding is solved by traditional mechanical processing that is difficult to form, and the traditional mechanical processing is not enough. , realizes high-precision and high-strength micro-module digital gear forming, meeting the needs of high-end precision equipment.

CN118682134BActive Publication Date: 2024-11-15GANNAN UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411180223.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Traditional machining methods are difficult to accurately mold extremely small module gears. In powder injection molding technology, material shrinkage behavior is complex and difficult to predict, resulting in difficult to ensure dimensional consistency and accuracy, which limits the application of micro gears in the field of high-end precision equipment.

Method used

Prepare the mixture of high-strength stainless steel metal powder and POM-based binder. The sintering process is combined with high-strength stainless steel sintering plate to control the sintering process. Thermal stress and shrinkage rate improve dimensional accuracy.

Benefits of technology

It realizes high-precision and high-strength micro-module digital gear forming, reduces the frequency of sintering and cracking, improves dimensional accuracy and mechanical properties, meets the needs of high-end precision equipment, reduces preparation costs, and improves output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118682134B_ABST
    Figure CN118682134B_ABST
Patent Text Reader

Abstract

The present invention relates to a powder forming process, and in particular to a high-precision and high-strength micro-modulus gear metal powder forming process. A high-precision and high-strength micro-modulus gear metal powder forming process includes feed preparation, injection molding, catalytic degreasing, sintering molding, and solution aging and shaping. The present invention adopts a high-strength stainless steel support plate that is the same as the micro-modulus gear matrix material for support, which can reduce the difference in thermal expansion coefficients of the contact interface between the support plate and the micro-modulus gear, thereby reducing the internal thermal stress of the micro-modulus gear and reducing the frequency of sintering cracking in the micro-modulus gear. Since the support plate and the micro-modulus gear shrink together, the force distribution of the micro-modulus gear during the sintering process can be optimized, the shrinkage rate can be controlled at a predetermined level of about 13.5%, and the size of the micro-modulus gear can be improved to improve the dimensional accuracy of the micro-modulus gear.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a powder forming process, in particular to a high-precision and high-strength micro-modulus gear metal powder forming process. Background Art

[0002] In the development of gear manufacturing technology, traditional machining methods, such as milling, turning and grinding, have always been the main means of manufacturing gears. With the growing demand in the field of precision machinery and micro-machinery, traditional machining technology has encountered challenges, especially when dealing with gears with extremely small modulus (such as less than 0.08 modulus). Due to the small size, the physical limitations of mechanical tools make it difficult to accurately shape, and the stability and precision control during the cutting process have also become a problem, making it difficult for traditional machining technology to meet the manufacturing requirements of such tiny gears, limiting its application in the fields of precision instruments and micro-motors. In this context, powder injection molding technology has opened up a new path for the manufacture of tiny gears. This technology mixes metal powder with a binder and injects it into a mold. After a series of processes such as cooling and solidification, degreasing, and sintering, the gear parts are finally formed. The advantage of this process is that the material strength of the powder injection gear produced can be close to or even reach the same level as that of conventional metal gears of the same material. This means that in micro devices, even if the gear is small in size, it can carry the necessary load and ensure the reliable operation of the system.

[0003] However, powder injection molding technology also faces some challenges: due to the complex and unpredictable shrinkage behavior of materials during powder sintering, it is difficult to ensure the dimensional consistency and accuracy of the final product. The highest accuracy level that can be achieved in the industry is generally GB / T236310. Although this level of accuracy can meet some application requirements, there is still a certain gap for high-end precision equipment, which limits the in-depth application of powder injection gears in a wider range of fields. Therefore, how to further improve its dimensional accuracy and break through the existing accuracy bottleneck has become the focus of current research and practice in this field, and is also the key to achieving the widespread application of powder injection gears in the field of precision manufacturing. Summary of the invention

[0004] In order to overcome the shortcomings in the prior art that it is difficult to machine extremely small modulus gears using mechanical machining methods, and that the shrinkage behavior of materials during powder sintering in powder injection molding technology is complex and difficult to predict, resulting in difficulty in ensuring the dimensional consistency and accuracy of the final product, the present invention provides a high-precision and high-strength micro-modulus gear metal powder forming process.

[0005] The technical implementation scheme of the present invention is: a high-precision and high-strength micro-modulus gear metal powder forming process, comprising the following steps: feeding preparation, mixing high-strength stainless steel metal powder and POM-based binder in a mass percentage ratio of 60-70%:30-40%, mixing in a V-type mixer at a temperature of 160-200°C, a stirring time of 2-4h, and a rotation speed of 20-40r / min; then, taking out the mixed raw materials and cooling them, and then granulating them in a granulator to obtain granular raw materials required for injection molding;

[0006] Injection molding, using an injection molding machine and a universal MIM plastic base system for feeding injection, the temperature of each temperature zone is set as follows: injection machine nozzle 180-200℃, temperature zone 1 175-195℃, temperature zone 2 165-185℃, temperature zone 3 155-175℃, temperature zone 4 145-165℃; injection time is 1-5s, injection pressure is 85-100MPa, holding time is 1-5s, holding pressure is 80-100MPa, cooling time is 5-15s;

[0007] Catalytic degreasing, the acidic atmosphere used is ≥95% concentrated nitric acid, and the protective atmosphere is nitrogen; the fan speed is set to 1200-1500rad / min, degreasing is performed with ≥95% concentrated nitric acid, the degreasing temperature is 80-120°C, nitrogen is introduced into the degreasing furnace as a protective gas, the nitrogen flow rate is 1.5-3.0m3 / h, the oxygen content in the degreasing furnace is <6%, the supply amount of ≥95% concentrated nitric acid is 300-400mL / h, the degreasing time is 3.5-4.5h, the degreasing rate is 1-3mm / h from the outside to the inside, and the degreasing is completed when the degreasing rate is ≥7%;

[0008] Sintering forming, using a high-strength stainless steel setter plate that is the same as the micro-modulus gear base material for sintering. The setter plate is the same as the micro-modulus gear base material. Argon is filled into the sintering furnace as a protective gas. The sintering temperature is 1300-1500°C and the sintering time is 180-360min.

[0009] Solution aging and shaping: After sintering, the micro-modulus gear sintered product is placed in a vacuum sintering furnace, and the solution temperature is 950-1150℃, and the solution time is 1-2h to form a supersaturated solid solution; the aging temperature is 450-650℃, and the aging time is 2-4h to precipitate the alloy from the supersaturated solid solution to form a small and evenly distributed strengthening phase. At the same time, the stress caused by cold and hot processing is eliminated, and the alloy is recrystallized, and then a shaping machine is used for shaping.

[0010] More preferably, the temperature setting during the sintering forming is as follows: stage one: heating from room temperature to 250-300°C at a heating rate of 5-15°C / min, and keeping warm for 40-80min; stage two: heating to 550-750°C at a heating rate of 1-10°C / min, and keeping warm for 40-80min; stage three: heating to 950-1150°C at a heating rate of 1-10°C / min, keeping warm for 40-80min, and maintaining the argon pressure at 20-40KPa; stage four: heating to 1280-1480°C at a heating rate of 1-5°C / min, keeping warm for 120-240min, and maintaining the argon pressure at 20-40Kpa; stage five: cooling to room temperature at a cooling rate of 10-20°C / min, and maintaining the argon pressure at 66-106Kpa; taking out the micro-modulus gear product.

[0011] More preferably, the parameters of the micro-module gear are a module of 0.05-0.1 mm, a number of teeth of 10-20, a tooth width of 0.5-1.5 mm, and an accuracy level of less than 8 under the GB2363-90 standard.

[0012] More preferably, the high-strength stainless steel metal powder is prepared by water vapor combined atomization.

[0013] More preferably, the average particle size D50 of the high-strength stainless steel metal powder is 4.5um; the mass percentages of the components of the POM-based binder are polyoxymethylene (POM) 80-90%, polypropylene (PP) 4.5-6.5%, high-density polyethylene (HDPE) 5.5-7.5%, and stearic acid 1-3%.

[0014] More preferably, the injection molding uses a Haitian MA-900 injection molding machine, the catalytic degreasing uses a Huiteng HT-220L catalytic degreasing furnace, and the sintering molding and solution aging are both performed using a Hengpu PVLG20 / 20 vacuum sintering furnace.

[0015] More preferably, the shaping process uses a self-made shaping machine, which includes an upper die and a lower die. During shaping, the micro-modulus gear is placed in the female die hole, and the micro-modulus gear after solution aging is pressed again by applying pressure through the upper and lower dies.

[0016] Compared with the prior art, the present invention has the following advantages: during the sintering process, the present invention uses a high-strength stainless steel support plate that is the same as the micro-modulus gear matrix material for support sintering. The support plate and the micro-modulus gear matrix material are the same, which can reduce the difference in thermal expansion coefficients of the contact interface between the support plate and the micro-modulus gear, thereby reducing the internal thermal stress of the micro-modulus gear and reducing the frequency of sintering cracking in the micro-modulus gear. Since the support plate and the micro-modulus gear shrink together, the force distribution of the micro-modulus gear during the sintering process is optimized, and the shrinkage rate is controlled at a predetermined level of about 13.5%, thereby improving the size of the micro-modulus gear and improving the dimensional accuracy of the micro-modulus gear. Both sintering forming and solution aging are carried out in a Hengpu PVLG20 / 20 vacuum sintering furnace, which can reduce the preparation cost and increase the output of high-performance micro-modulus gears. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a process flow chart of high-precision and high-strength micro-modulus gear metal powder forming process of the present invention;

[0018] Figure 2 It is a schematic diagram of the arrangement of the degreased blank and the support plate of the micro-modulus gear during the sintering process of the present invention. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0020] A high-precision and high-strength micro-modulus gear metal powder forming process, such as Figure 1 As shown, the steps include: feed material preparation, injection molding, catalytic debinding, sintering, solution aging and shaping.

[0021] Specifically, a micro-module gear having a module of 0.075 mm, a number of teeth of 15, a tooth width of 1 mm, and an accuracy level of less than 8 under the GB2363-90 standard is prepared as an example. In one embodiment, the feed preparation specifically includes the following steps:

[0022] High-strength stainless steel metal powder and POM-based binder are used to prepare feed; high-strength stainless steel metal powder and POM-based binder are mixed in a ratio of 64%:36% by mass, and mixed in a V-type mixer at a temperature of 180°C, a stirring time of 3h, and a rotation speed of 30r / min. Subsequently, the mixed raw materials are taken out and cooled, and then granulated in a granulator to obtain the granular raw materials required for injection molding. The high-strength stainless steel metal powder is prepared by water vapor combined atomization, which not only reduces the preparation cost, but also improves the roundness of the powder and improves the flowability of the powder. The average particle size D50 of the powder is 4.5m, the sphericity is good, and there is no obvious agglomeration phenomenon. The mass percentages of the components of the POM-based binder are polyoxymethylene (POM) 86%, polypropylene (PP) 5.5%, high-density polyethylene (HDPE) 6.5%, and stearic acid 2%. As the main binder, POM is sensitive to acidic atmosphere, can be quickly catalytically decomposed into formaldehyde in an acidic atmosphere, and can be quickly removed during the degumming process. HDPE is selected as the high molecular weight component to provide sufficient support strength for the injection blank during the degreasing process. PP can maintain the shape of the blank and has a certain compatibility with POM, ensuring the uniformity of the feed.

[0023] In one embodiment, the specific operation of injection molding is: adopting the general MIM plastic-based system feeding injection process, using Haitian MA-900 injection molding machine, and the temperature of each temperature zone is set as: injection machine nozzle 190°C, temperature zone one 185°C, temperature zone two 175°C, temperature zone three 165°C, temperature zone four 155°C; injection time is 2s, injection pressure is 93MPa, holding time is 1.5s, holding pressure is 90MPa, and cooling time is 9s.

[0024] In one embodiment, the catalytic degreasing process is as follows: in a Huiteng HT-220L catalytic degreasing furnace, the fan speed is set to 1200 rad / min, degreasing is performed with ≥95% concentrated nitric acid, the degreasing temperature is 80°C, and nitrogen is introduced into the degreasing furnace as a protective gas, and the nitrogen flow rate is 1.5m 3 / h, the oxygen content in the degreasing furnace is <6%, the supply amount of concentrated nitric acid ≥95% is 350mL / h, the degreasing time is 3.5h, the degreasing rate is 1mm / h from outside to inside, and the degreasing is completed when the degreasing rate is ≥7%.

[0025] In another embodiment, the catalytic degreasing process is as follows: in a Huiteng HT-220L catalytic degreasing furnace, the fan speed is set to 1500 rad / min, degreasing is performed with ≥95% concentrated nitric acid, the degreasing temperature is 80-120°C, and nitrogen is introduced into the degreasing furnace as a protective gas, and the nitrogen flow rate is 3.0m 3 / h, the oxygen content in the degreasing furnace is <6%, the supply amount of concentrated nitric acid ≥95% is 350mL / h, the degreasing time is 4.5h, the degreasing rate is 1mm / h from outside to inside, and the degreasing is completed when the degreasing rate is ≥7%.

[0026] In one embodiment, the specific steps of sintering are: using Hengpu PVLG20 / 20 vacuum sintering furnace, filling argon into the sintering furnace as a protective gas, the sintering temperature is 1380°C, the sintering time is 180min, and the specific sintering temperature is as follows: stage one: heating from room temperature to 300°C at a heating rate of 10°C / min, and keeping warm for 60min; stage two: heating from 300°C to 650°C at a heating rate of 5°C / min, and keeping warm for 60min; The third stage: heating from 650°C to 1050°C at a heating rate of 4.5°C / min, keeping warm for 60 minutes, and maintaining the argon pressure at 30KPa; the fourth stage: heating from 1050°C to 1380°C at a heating rate of 2°C / min, keeping warm for 180 minutes, and maintaining the argon pressure at 30KPa; the fifth stage: cooling from 1380°C to room temperature at a cooling rate of 15°C / min, and maintaining the argon pressure at 86KPa; take out the micro-modulus gear products.

[0027] In a preferred embodiment, reference Figure 2 The schematic diagram of the arrangement of the degreased blank and the firing plate of the micro-modulus gear of the present invention during the sintering process is shown; during the sintering process, a high-strength stainless steel firing plate which is the same as the micro-modulus gear matrix material is used for firing, and the firing plate and the micro-modulus gear matrix material are the same; using a high-strength stainless steel firing plate which is the same as the micro-modulus gear matrix material for firing can reduce the difference in thermal expansion coefficients of the contact interface between the firing plate and the micro-modulus gear, thereby reducing the internal thermal stress of the micro-modulus gear and reducing the frequency of sintering cracking in the micro-modulus gear. Since the firing plate and the micro-modulus gear shrink together, the force distribution of the micro-modulus gear during the sintering process can be optimized, the shrinkage rate is controlled at a predetermined level of about 13.5%, and the size of the micro-modulus gear is improved to improve the dimensional accuracy of the micro-modulus gear.

[0028] In one embodiment, the solution aging adopts Hengpu PVLG20 / 20 vacuum sintering furnace to reduce the preparation cost and increase the output of high-performance micro-modulus gears; the solution aging process includes a solution process and an aging process. After the sintering is completed, the micro-modulus gear sintered product is placed in a vacuum sintering furnace, and the solution is carried out with a solution temperature of 1050°C and a solution time of 1.5h as parameters to ensure that the alloy is dissolved into the matrix to form a supersaturated solid solution; the aging is carried out with an aging temperature of 550°C and an aging time of 3h as parameters to precipitate the alloy from the supersaturated solid solution to form a fine and evenly distributed strengthening phase, while eliminating the stress caused by cold and hot processing, causing the alloy to recrystallize, thereby improving the uniform distribution of the micro-modulus gear structure and the mechanical properties. Taking the tensile specimen as an example for verification, after the solution aging process with a solution temperature of 1050℃, a solution time of 1.5h, an aging temperature of 550℃, and an aging time of 3h, the average tensile strength of the tensile specimen increased from 900MPa to 1650MPa, the average hardness increased from 300Hv to 530Hv, and the average density increased from 7.74g / cm 3 Increased to 7.78g / cm 3 , the mechanical properties are greatly improved.

[0029] Finally, the shaping process uses a self-made shaping machine, which includes an upper die and a lower die. The micro-modulus gears after solution aging are pressed again to change their shape and improve their precision. During shaping, the micro-modulus gears are placed in the female die hole and are pressurized once by the upper and lower dies to make the molded gears meet the high-density requirements, and their density is increased by 5%-12%.

[0030] The technical principles of the embodiments of the present invention are described above in conjunction with specific embodiments. These descriptions are only for explaining the principles of the embodiments of the present invention and cannot be interpreted in any way as limiting the protection scope of the embodiments of the present invention. Based on the explanations herein, those skilled in the art can think of other specific implementation methods of the embodiments of the present invention without creative work, and these methods will fall within the protection scope of the embodiments of the present invention.

Claims

1. A high-precision and high-strength micro-modulus gear metal powder forming process, characterized in that: The following steps are involved: Feeding preparation: high-strength stainless steel metal powder and POM-based binder are mixed in a mass percentage ratio of 60-70%:30-40%, and mixed in a V-type mixer at a temperature of 160-200°C, a stirring time of 2-4h, and a rotation speed of 20-40r / min; then, the mixed raw materials are taken out and cooled, and then granulated in a granulator to obtain the granular raw materials required for injection molding; injection molding: an injection molding machine is used and a universal MIM plastic-based system is used for feeding injection, and the temperature of each temperature zone is set as follows: injection machine nozzle 180-200°C, temperature zone one 175-195°C, temperature zone The temperature of the second zone is 165-185℃, the third zone is 155-175℃, and the fourth zone is 145-165℃; the injection time is 1-5s, the injection pressure is 85-100MPa, the holding time is 1-5s, the holding pressure is 80-100MPa, and the cooling time is 5-15s; catalytic degreasing, the acidic atmosphere used is ≥95% concentrated nitric acid, and the protective atmosphere is nitrogen; the fan speed is set to 1200-1500rad / min, degreasing is performed with ≥95% concentrated nitric acid, the degreasing temperature is 80-120℃, and nitrogen is introduced into the degreasing furnace as a protective gas, and the nitrogen flow rate is 1.5-3.0m 3 / h, the oxygen content in the degreasing furnace is less than 6%, the supply amount of concentrated nitric acid ≥95% is 300-400mL / h, the degreasing time is 3.5-4.5h, the degreasing rate is 1-3mm / h from the outside to the inside, and the degreasing is completed when the degreasing rate is ≥7%; sintering forming, using a high-strength stainless steel support plate that is the same as the micro-modulus gear matrix material for support sintering, the support plate and the micro-modulus gear matrix material are the same, argon is filled into the sintering furnace as a protective gas, the sintering temperature is 1300-1500℃, and the sintering time is 180-3 60min; solution aging and shaping. After sintering, the micro-modulus gear sintered product is placed in a vacuum sintering furnace, and the solution temperature is 950-1150℃, and the solution time is 1-2h. The solid solution is formed by the parameters of the solid solution; the aging temperature is 450-650℃, and the aging time is 2-4h. The alloy is precipitated from the supersaturated solid solution to form a small and evenly distributed strengthening phase. At the same time, the stress caused by cold and hot processing is eliminated, and the alloy is recrystallized. Then the shaping machine is used for shaping. The temperature setting during sintering is as follows: the first stage: heating from room temperature to 250-300°C at a heating rate of 5-15°C / min, and keeping warm for 40-80min; the second stage: heating to 550-750°C at a heating rate of 1-10°C / min, and keeping warm for 40-80min; the third stage: heating to 950-1150°C at a heating rate of 1-10°C / min, and keeping warm for 40-80min, and the argon pressure is maintained at 20-40KPa; the fourth stage: heating at 1-5°C / min, and keeping warm at 550-750°C ... C / min heating rate, heating to 1280-1480℃, keeping warm for 120-240min, and maintaining the argon pressure at 20-40Kpa; five stages: cooling to room temperature at a cooling rate of 10-20℃ / min, and maintaining the argon pressure at 66-106Kpa; taking out the micro-modulus gear product; the shaping process adopts a self-made shaping machine, which includes an upper die and a lower die. During shaping, the micro-modulus gear is placed in the female die hole, and the micro-modulus gear after solution aging is pressed again by applying pressure through the upper and lower dies.

2. A high-precision and high-strength micro-modulus gear metal powder forming process according to claim 1, characterized in that: The parameters of the micro-module gear are a module of 0.05-0.1 mm, a number of teeth of 10-20, a tooth width of 0.5-1.5 mm, and an accuracy level of less than 8 under the GB2363-90 standard.

3. A high-precision and high-strength micro-modulus gear metal powder forming process according to claim 2, characterized in that: The high-strength stainless steel metal powder is prepared by water vapor combined atomization.

4. A high-precision and high-strength micro-modulus gear metal powder forming process according to claim 3, characterized in that: The average particle size D50 of the high-strength stainless steel metal powder is 4.5um; the mass percentages of the components of the POM-based adhesive are polyoxymethylene (POM) 80-90%, polypropylene (PP) 4.5-6.5%, high-density polyethylene (HDPE) 5.5-7.5%, and stearic acid 1-3%.

5. A high-precision and high-strength micro-modulus gear metal powder forming process according to claim 4, characterized in that: The injection molding uses a Haitian MA-900 injection molding machine, the catalytic degreasing uses a Huiteng HT-220L catalytic degreasing furnace, and the sintering molding and solution aging are both performed using a Hengpu PVLG20 / 20 vacuum sintering furnace.